A method for preparing a weakly acidic and precipitation-resistant polymeric phosphorus-nitrogen flame retardant and a compound flame retardant thereof.
By employing low-temperature stepwise reaction and high-temperature dehydration and end-sealing treatment, a polymeric phosphorus-nitrogen flame retardant with weak acidity and precipitation resistance was prepared. This solved the problems of uneven blending and corrosion in compound intumescent flame retardants, and improved the flame retardant performance and stability.
Patent Information
- Application Number
- CN202611243931.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing compound intumescent flame retardants suffer from uneven blending, increased mixing steps, and reduced flame retardant stability and consistency of materials. Piperazine pyrophosphate is prone to corroding equipment and precipitates easily. Traditional preparation processes are cumbersome and energy-intensive.
Using pyrophosphate, piperazine, and melamine as raw materials at low temperature, a mixture of piperazine pyrophosphate and melamine pyrophosphate is formed through a stepwise reaction. Subsequently, the mixture is dehydrated at high temperature and subjected to an end-capping reaction to prepare a polymeric phosphorus-nitrogen flame retardant with weak acidity and resistance to precipitation.
It achieves lower water solubility and higher resistance to precipitation, reduces corrosion to metal equipment, simplifies the preparation process, and improves compatibility with matrix materials.
Smart Images

Figure CN123107093A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flame retardants, and particularly to a method for preparing a weakly acidic and precipitation-resistant polymeric phosphorus-nitrogen flame retardant and a compound flame retardant. Background Technology
[0002] Flame retardants are the most direct and effective processing aids for improving the flame retardant properties of materials. Although traditional halogenated flame retardants have excellent flame retardant efficiency, they pose potential hazards to the environment and human health during use and disposal. Inorganic flame retardants, while environmentally friendly, have low flame retardant efficiency, and high addition amounts can significantly degrade the processing flowability and mechanical properties of the matrix material. Therefore, developing non-toxic, efficient, and green flame retardant systems and their synergistic technologies has become an important development direction in the field of flame retardant materials.
[0003] Intumescent flame retardants (IFRs) are a type of environmentally friendly halogen-free flame retardant system, typically composed of three components: an acid source, a carbon source, and a gas source. They offer advantages such as low smoke, low toxicity, and resistance to dripping. However, traditional IFRs still suffer from problems in practical applications, including easy migration, poor compatibility with polymer matrices, high required addition amounts, and significant damage to the mechanical properties of composite materials, which restricts their large-scale application.
[0004] Piperazine pyrophosphate (PAPP) is a phosphorus-nitrogen-containing polymeric flame retardant with a high phosphorus content. It functions as an acid source, carbon source, and gas source, making it suitable for various polymer materials such as polypropylene, polyethylene, nylon, epoxy resin, polyurethane, and elastomers, showing promising application prospects. However, PAPP itself has a low nitrogen content, resulting in insufficient foaming and charring ability. Therefore, it usually needs to be used in combination with other flame retardants, such as ammonium polyphosphate (APP), aluminum diethylphosphinate, melamine cyanurate (MCA), melamine pyrophosphate (DMPY), and melamine polyphosphate (MPP), to synergistically improve flame retardant efficiency and reduce overall costs. Studies have shown that the halogen-free intumescent flame retardant obtained by combining piperazine pyrophosphate and melamine pyrophosphate exhibits superior flame retardant properties and mechanical retention in a polypropylene matrix. Compared to the traditional ammonium polyphosphate system, it has significant advantages in terms of lower addition amount and higher flame retardant efficiency, thus gaining widespread attention and application in polyolefin materials.
[0005] Currently, compounded flame retardants are the most common application of piperazine pyrophosphate. However, most existing compounded intumescent flame retardants are physical blending systems, such as ammonium polyphosphate blended with char-forming agents (e.g., triazine, pentaerythritol), and piperazine pyrophosphate blended with melamine pyrophosphate. These systems suffer from uneven mixing, increased mixing steps, and the physical mixing method affecting the final material's flame retardant stability and consistency. Furthermore, piperazine pyrophosphate itself has a low pH, high water solubility, and is hygroscopic, which can corrode equipment during processing, cause precipitation during material use, and pose a risk of clumping during storage. While compounding with melamine-based flame retardants can alleviate these defects to some extent, the inherent performance defects of the product are not fundamentally resolved because the compounding method is still primarily physical mixing.
[0006] To address the aforementioned issues, CN116410473A describes the preparation of piperazine diphosphate and melamine phosphate salts using phosphoric acid and piperazine, and phosphoric acid and melamine, respectively. These salts are then mixed with an antioxidant under vacuum conditions and subjected to a heated reaction. The mixture is then cooled and an alkaline end-capping agent is added for end-capping treatment, ultimately yielding a novel polymeric flame retardant. Compared to the physical compound system of piperazine pyrophosphate and melamine polyphosphate / melamine pyrophosphate, this novel polymeric flame retardant exhibits lower water solubility, higher resistance to precipitation, and a weakly alkaline nature, significantly reducing its corrosiveness to metal equipment. However, this process involves reacting phosphoric acid and piperazine, and phosphoric acid and melamine, at 70-90 degrees Celsius for 2-4 hours, followed by cooling for 1-2 hours for crystallization, filtration, drying, and pulverization to prepare piperazine diphosphate and melamine phosphate salts, which are then weighed, mixed in proportion, and subjected to a further heated reaction. This process is cumbersome and energy-intensive. This invention uses pyrophosphate, piperazine, and triamine as raw materials, reacting them at 0-20 degrees Celsius for 2-6 hours. After the reaction, the mixture is directly filtered and synthesized in one step into a mixture of melamine pyrophosphate and piperazine pyrophosphate. The mixture is then dried, pulverized, and subjected to a further heated reaction. The process involves fewer steps, is simpler, and utilizes low-temperature reaction with low energy consumption and is safe.
[0007] In summary, the key technical problems that urgently need to be solved in the current research on piperazine pyrophosphate intumescent flame retardants are how to simplify the preparation process, improve the uniformity of compounding, reduce the water solubility and hygroscopicity of the product, and enhance its compatibility with the matrix material while maintaining high flame retardant performance. Summary of the Invention
[0008] To address the aforementioned deficiencies, this invention provides a method for preparing a polymeric phosphorus-nitrogen flame retardant with weak acidity and resistance to precipitation, as well as a compounded flame retardant. This method offers lower water solubility, higher resistance to precipitation, and a weakly acidic pH value that reduces corrosiveness to metal equipment.
[0009] A method for preparing a weakly acidic and resistant-to-expansion polymeric phosphorus-nitrogen flame retardant involves using pyrophosphate, piperazine, and melamine as raw materials, and reacting piperazine, pyrophosphate powder, and melamine in steps to obtain a weakly acidic and resistant-to-expansion polymeric phosphorus-nitrogen flame retardant.
[0010] In one or more optional embodiments of the present invention, the following steps are included: S1, Add solvent and piperazine to the reaction vessel, cool to below room temperature, and slowly add pyrophosphate while stirring to obtain a mixture of pyrophosphate and piperazine pyrophosphate. The reaction temperature is 0℃~20℃, the reaction time is 0.5h~1.5h, and the mass ratio of piperazine to pyrophosphate is 1:2.5~3.5. S2, Melamine is prepared into a slurry with a solvent, and the melamine slurry is slowly added to the reaction vessel under stirring to carry out the reaction. The reaction temperature is 0℃~20℃, the reaction time is 2h~5h, and the mass ratio of melamine to pyrophosphate is 1:1.8~4.2. S3, after filtration, separation, and drying, yields a weakly acidic and resistant polymeric phosphorus-nitrogen flame retardant.
[0011] In one or more alternative embodiments of the present invention, the pyrophosphate is a solid pyrophosphate powder.
[0012] In one or more alternative embodiments of the present invention, in S1 and S2, the solvent is selected from water, methanol or ethanol.
[0013] In one or more optional embodiments of the present invention, in S1, the mass ratio of piperazine to solvent is 1:7 to 8.5, and in S2, the mass ratio of melamine to solvent is 1:1.5 to 3.
[0014] In one or more alternative embodiments of the present invention, the piperazine is 68-piperazine.
[0015] In one or more optional embodiments of the present invention, after S3, S4 is further included, in which a weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant is mixed with an antioxidant under a nitrogen atmosphere, heated to 200°C~250°C and reacted for 1~3 hours, cooled to 130°C~190°C, and a sealing agent is added for a sealing reaction for 0.5 hours~2 hours. The mixture is then discharged and pulverized to obtain a weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant.
[0016] In one or more optional embodiments of the present invention, in S4, the antioxidant is selected from phenolic antioxidants or phosphorus antioxidants, and the mass of the antioxidant is 0.1wt% to 1wt% of the mass of the weakly acidic and resistant to precipitation polymeric phosphorus-nitrogen flame retardant. The end-capping agent is selected from melamine, ammonia, urea, melamine, metal oxides or metal hydroxides, and the mass of the end-capping agent is 0.1wt% to 3wt% of the mass of the weakly acidic and resistant to precipitation polymeric phosphorus-nitrogen flame retardant.
[0017] The present invention also provides a compound flame retardant.
[0018] A compound flame retardant includes a thermoplastic resin and is further compounded with a weakly acidic and resistant-to-expansion polymeric phosphorus-nitrogen flame retardant prepared by the above method.
[0019] In one or more alternative embodiments of the present invention, the thermoplastic resin is selected from PP, PE, ABS or PA.
[0020] Compared with existing technologies, the invention principles and beneficial effects are as follows: This invention achieves the effect of existing flame retardants by forming a mixture of piperazine pyrophosphate and melamine pyrophosphate at low temperature, without the need for high-temperature polymerization to "assemble" the two salt materials into macromolecules or for "end-capping" treatment. It can be used alone as a flame retardant. Furthermore, based on the formation of the mixture of piperazine pyrophosphate and melamine pyrophosphate, this invention obtains a polymeric phosphorus-nitrogen flame retardant with even better performance through high-temperature dehydration and end-capping reaction.
[0021] Compared with flame retardants formed by combining piperazine pyrophosphate and melamine pyrophosphate, the polymeric phosphorus-nitrogen flame retardant of this invention has lower water solubility, higher resistance to precipitation, and a weakly acidic pH value, which reduces its corrosiveness to metal equipment.
[0022] Figure 1 This is a TG diagram of the product in Embodiment 1 of the present invention; Figure 2 This is a TG diagram of the product in Embodiment 4 of the present invention; Figure 3 This is the TG diagram of the product in Comparative Example 1 of this invention; Figure 4 This is the TG diagram of the product in Comparative Example 2 of this invention; Figure 5 This is the TG diagram of Comparative Example 3 of the present invention; Figure 6 This is the TG diagram of Comparative Example 4 of the present invention. Detailed Implementation
[0023] The present invention will be further described below.
[0024] As used in this article: "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.
[0025] The conjunction "composed of..." excludes any unspecified elements, steps, or components. If used in a claim, this phrase makes the claim closed, excluding materials other than those described, except for associated conventional impurities. When the phrase "composed of..." appears in a clause of the body of a claim rather than immediately following it, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0026] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1–5” is disclosed, the described range should be interpreted as including ranges “1–4”, “1–3”, “1–2”, “1–2 and 4–5”, “1–3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.
[0027] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0028] Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified, specific conditions in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Reagents (materials) or instruments (equipment) used without a specified manufacturer are all commercially available conventional products.
[0029] In these embodiments, unless otherwise specified, the portions and percentages are all by weight.
[0030] "Parts by mass" refers to the basic unit of measurement that expresses the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2.689g. If we say that component A has "a" parts by mass and component B has "b" parts by mass, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it can mean that the mass of component A is aK and the mass of component B is bK (K is any number representing a multiplier). It is important to understand that, unlike the number of parts by mass, the sum of the mass parts of all components is not limited to 100 parts.
[0031] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0032] In the following examples and comparative examples, the pyrophosphate powder contained ≥98% pyrophosphate. Example 1 S1. Water and 68-piperazine were added to the reactor. The amount of water added was 43.6 kg and the amount of 68-piperazine added was 6.18 kg. After the 68-piperazine dissolved, the temperature was lowered to 10°C. Pyrophosphate powder of 10.47 kg was slowly added while stirring. The reaction was carried out for 1 hour at a reaction temperature of 15°C to obtain a mixture of pyrophosphate and piperazine pyrophosphate.
[0033] S2, 2.52 kg of melamine was mixed with 6 kg of water to form a slurry. The melamine slurry was slowly added to the reactor with stirring and reacted for 4 hours at a temperature of 15°C.
[0034] S3, after the reaction is completed, the material is filtered, separated, and dried to obtain 16.89 kg of a solid product consisting of a mixture of piperazine pyrophosphate and melamine pyrophosphate. The TG graph of this solid product is shown in the figure below. Figure 1 .
[0035] In the solid product of S3, which is a mixture of piperazine pyrophosphate and melamine pyrophosphate, the amount of piperazine pyrophosphate is 4.22 kg and the amount of melamine pyrophosphate is 12.67 kg.
[0036] In S1, the stirring rate is 25 Hz, and in S2, the stirring rate is 50 Hz.
[0037] Example 2 The difference compared to Example 1 is as follows: In S1, the reaction temperature is 10℃, the amount of water added is 31.4 kg, the amount of 68 piperazine added is 4.12 kg, and the amount of pyrophosphate powder added is 7.58 kg.
[0038] In S2, the reaction temperature is 10℃, the reaction time is 5h, and the amount of melamine added is 2.52kg.
[0039] In S3, the amount of the solid product of the mixture of piperazine pyrophosphate and melamine pyrophosphate is 12.65 kg.
[0040] Example 3 The difference compared to Example 1 is as follows: In S1, the reaction temperature is 20℃, the amount of water added is 25.26 kg, the amount of 68 piperazine added is 3.09 kg, and the amount of pyrophosphate powder added is 6.13 kg.
[0041] In S2, the reaction temperature is 20℃, the reaction time is 4h, and the amount of melamine added is 2.52kg.
[0042] In S3, the amount of the solid product of the mixture of piperazine pyrophosphate and melamine pyrophosphate is 12.65 kg.
[0043] Example 4 Compared to Example 1, after S3, S4 is also included: S4. A mixture of 16.89 kg of piperazine pyrophosphate and melamine pyrophosphate, along with 0.16 kg of antioxidant trinonylphenyl phosphite, was thoroughly mixed and then added to another reactor. Nitrogen gas was introduced, and the mixture was heated to 240°C for high-temperature dehydration for 2 hours. The temperature was then lowered to 170°C, and 0.5 kg of melamine was added. The reaction was maintained at 170°C for 0.5 hours, and the mixture was discharged at room temperature. After pulverization, 16.82 kg of a polymeric phosphorus-nitrogen flame retardant was obtained. This polymeric phosphorus-nitrogen flame retardant exhibits weak acidity and resistance to precipitation. The TG diagram of this polymeric phosphorus-nitrogen flame retardant is shown below. Figure 2 .
[0044] Comparative Example 1 Compared with Example 1, the difference lies in S1. In this comparative example, S1 is: 6.18 kg of piperazine was added to a reaction vessel containing 43.6 kg of water. Stirring was started, and then 13.55 kg of 85% phosphoric acid was slowly added dropwise over 0.5 hours. After the addition was complete, the temperature was raised to 80°C and the reaction was carried out for 4 hours. After cooling, the mixture was centrifuged and dried to obtain 14.71 kg of a mixture of piperazine diphosphate and melamine phosphate.
[0045] The TG graph of the solid product in Comparative Example S3 is shown below. Figure 3 .
[0046] Comparative Example 2 The difference compared to Example 1 is as follows: In S1 and S2, the reaction temperature is 80℃.
[0047] The TG graph of the solid product in Comparative Example S3 is shown below. Figure 4 .
[0048] Comparative Example 3 Compared with Comparative Example 2, the reaction time was 2 hours.
[0049] The TG graph of the solid product in Comparative Example S3 is shown below. Figure 5 .
[0050] Comparative Example 4 The difference compared to Example 1 is as follows: In this comparative example, piperazine pyrophosphate and melamine pyrophosphate, in the same amount as S3 in Example 1, were mixed thoroughly. The TG curve is shown below. Figure 6 .
[0051] In this comparative example: The preparation process of piperazine pyrophosphate with the same amount as S3 in Example 1 is as follows: water and 68-piperazine are added to the reaction vessel. The amount of water added is 43.6 kg and the amount of 68-piperazine added is 6.18 kg. After the 68-piperazine is dissolved, the temperature is lowered to 10°C, and 8.69 kg of pyrophosphate powder is slowly added under stirring. The reaction is carried out for 4 hours at a reaction temperature of 15°C to obtain 12.4 kg of piperazine pyrophosphate. The stirring rate is 25 Hz.
[0052] The preparation process of melamine pyrophosphate with the same amount as S3 in Example 1 is as follows: 2.52 kg of melamine is mixed with 6 kg of water to form a slurry. The melamine slurry is slowly added to a reaction vessel containing 1.78 kg of pyrophosphate powder under stirring and reacted for 4 hours. The reaction temperature is 15°C and the stirring rate is 50 Hz.
[0053] Compare Figures 1-6 The temperature at which TG weight loss is 1% is taken as the thermal decomposition temperature.
[0054] Table 1 The flame retardants prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were tested for water solubility and pH value. The results are shown in Table 2.
[0055] Table 2 The flame retardants prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were applied to PP to produce flame-retardant PP materials. Using polypropylene (PP) as the base material, the flame-retardant application of polymeric phosphorus-nitrogen flame retardants in polypropylene was studied. The application test was conducted on the flame-retardant polypropylene samples by vertical burning test. The test method was carried out according to the method specified in the national standard "Determination of Burning Performance of Plastics - Horizontal and Vertical Methods" and the test was completed using a horizontal and vertical burning apparatus. The test results are shown in Table 3.
[0056] Table 3 As shown in Table 1, the mixture prepared by this invention has a thermal decomposition temperature of 278.8℃, which is higher than the 264.9℃ of simple physical mixing. After high-temperature dehydration and end-capping reaction, its thermal decomposition temperature reaches 286.6℃, resulting in a polymeric phosphorus-nitrogen flame retardant with even better performance.
[0057] As can be seen from Table 2, after high-temperature dehydration and end-capping reaction, the pH value of the mixture prepared by the present invention is significantly increased, the water solubility is significantly decreased, the product has higher resistance to precipitation, and the product is weakly acidic with a pH value that is less corrosive to metal equipment.
[0058] As can be seen from Table 3, after forming a mixture of piperazine pyrophosphate and melamine pyrophosphate at low temperature, the present invention can achieve the UL94 V0 rating without the need for high-temperature polymerization to "assemble" the two material salts into macromolecules or for "end-capping" treatment, and can be used alone as a flame retardant. Furthermore, based on the formation of the mixture of piperazine pyrophosphate and melamine pyrophosphate, the limiting oxygen index is further improved after high-temperature dehydration and end-capping reaction, resulting in better flame retardant effect.
[0059] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant, characterized in that, Using pyrophosphate, piperazine, and melamine as raw materials, piperazine and pyrophosphate powder are added stepwise to react with melamine to obtain a polymeric phosphorus-nitrogen flame retardant with weak acidity and resistance to precipitation.
2. The preparation method of the weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant according to claim 1, characterized in that, Includes the following steps: S1, Add solvent and piperazine to the reaction vessel, cool to below room temperature, and slowly add pyrophosphate while stirring to obtain a mixture of pyrophosphate and piperazine pyrophosphate. The reaction temperature is 0℃~20℃, the reaction time is 0.5h~1.5h, and the mass ratio of piperazine to pyrophosphate is 1:2.5~3.
5. S2, Melamine is prepared into a slurry with a solvent, and the melamine slurry is slowly added to the reaction vessel under stirring to carry out the reaction. The reaction temperature is 0℃~20℃, the reaction time is 2h~5h, and the mass ratio of melamine to pyrophosphate is 1:1.8~4.
2. S3, after filtration, separation, and drying, yields a weakly acidic and resistant polymeric phosphorus-nitrogen flame retardant.
3. The preparation method of the weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant according to claim 2, characterized in that, The pyrophosphate is a solid powder of pyrophosphate.
4. The preparation method of the weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant according to claim 2, characterized in that, In S1 and S2, the solvent is selected from water, methanol or ethanol.
5. The method for preparing a weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant according to claim 2, characterized in that, In S1, the mass ratio of piperazine to solvent is 1:7~8.5, and in S2, the mass ratio of melamine to solvent is 1:1.5~3.
6. The preparation method of the weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant according to claim 2, characterized in that, The piperazine is 68-piperazine.
7. The preparation method of the weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant according to claim 2, characterized in that, Following S3, S4 is also included. Under a nitrogen atmosphere, a weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant is mixed with an antioxidant, heated to 200℃~250℃ and reacted for 1~3 hours, then cooled to 130℃~190℃, and a sealing agent is added for a sealing reaction of 0.5 hours~2 hours. The mixture is then discharged and pulverized to obtain a weakly acidic and resistant-to-precipitation end-capped polymeric phosphorus-nitrogen flame retardant.
8. The method for preparing the weakly acidic and resistant-to-precipitation polymeric phosphorus-nitrogen flame retardant according to claim 2, characterized in that, In S4, the antioxidant is selected from phenolic antioxidants or phosphorus antioxidants, and the mass of the antioxidant is 0.1wt% to 1wt% of the mass of the weakly acidic and resistant to precipitation polymeric phosphorus-nitrogen flame retardant. The end-capping agent is selected from melamine, ammonia, urea, melamine, metal oxides or metal hydroxides, and the mass of the end-capping agent is 0.1wt% to 3wt% of the mass of the weakly acidic and resistant to precipitation polymeric phosphorus-nitrogen flame retardant.
9. A compound flame retardant comprising a thermoplastic resin, characterized in that, It is also compounded with a weakly acidic and resistant to precipitation polymeric phosphorus-nitrogen flame retardant prepared by the method described in any one of claims 1-8.
10. The compound flame retardant according to claim 1, characterized in that, The thermoplastic resin is selected from PP, PE, ABS or PA.