Modified ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof
By loading titanium doped iron oxide in the iron-based pyrophosphate positive electrode material, the modified sodium ferrophosphate positive electrode material is solved, and the problem of difficulty in taking into account both the magnification and circulation performance of existing materials is significantly improved. Electrochemical properties.
Patent Information
- Application Number
- CN202411366598.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-29
AI Technical Summary
The existing iron-based pyrophosphate cathode materials are difficult to improve both rate performance and cycle performance.
Sodium phosphate phosphate is used as the matrix material, and the titanium-doped iron oxide material is loaded. By adjusting the chemical formula and molar ratio, a modified sodium phosphate phosphate positive electrode material is formed, and the trivalent iron ions in the iron oxide material are doped by titanium-doped iron oxide material and Sodium ions form Na-Ti-O bonds, improving the structural stability and electron conductivity of the material.
It effectively improves the cycle stability and rate performance of sodium ion batteries, ensures the stable concentration of iron ions inside and on the surface of the crystal, and promotes the rapid transmission of sodium ions and electrons.
Smart Images

Figure CN119050329A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a modified sodium iron phosphate pyrophosphate positive electrode material, a preparation method thereof and an application thereof. Background Art
[0002] Sodium-ion batteries have attracted widespread attention due to their advantages such as low cost, high power and good stability. In recent years, with the increasing demand for portable devices and electric vehicle endurance, higher requirements have been placed on the cycle performance and rate performance of sodium-ion batteries. The positive electrode material is one of the important factors affecting the electrochemical performance of the battery. Among them, iron-based phosphoric acid pyrophosphate positive electrode materials have gradually become the focus of research due to their low cost, high theoretical specific capacity and high average operating voltage.
[0003] However, the structural stability, sodium ion diffusion rate and electronic conductivity of iron-based phosphate pyrophosphate are poor, and the rate performance and cycle performance cannot meet the requirements of practical applications. It is usually necessary to coat and dope its surface to achieve performance optimization. However, the current modification effect is limited, and it is difficult to take into account the improvement of rate performance and cycle performance.
[0004] Therefore, how to improve both the rate performance and cycle performance of iron-based phosphate pyrophosphate is a technical problem that needs to be solved urgently in this field. Summary of the invention
[0005] The main purpose of the present invention is to provide a modified sodium iron phosphate pyrophosphate positive electrode material and a preparation method and application thereof, so as to solve the problem that the existing iron-based sodium iron phosphate pyrophosphate is difficult to improve both rate performance and cycle performance.
[0006] In order to achieve the above-mentioned object, a first aspect of the present invention provides a modified sodium iron phosphate pyrophosphate positive electrode material, comprising sodium iron phosphate pyrophosphate and a titanium-doped iron oxide material supported on the sodium iron phosphate pyrophosphate.
[0007] Furthermore, the chemical formula of sodium iron phosphate pyrophosphate is Na4Fe3(PO4)2(P2O7); the chemical formula of the titanium-doped iron oxide material is Fe x Ti y O3, wherein x:y=1:(0.001-0.005), x+y=2.
[0008] Furthermore, the molar ratio of sodium ferric pyrophosphate to titanium-doped iron oxide material is 1:(0.03-0.08).
[0009] Furthermore, the D50 particle size of the modified sodium iron phosphate pyrophosphate positive electrode material is 5 to 8 μm.
[0010] The second aspect of the present invention provides a method for preparing the modified sodium iron phosphate pyrophosphate positive electrode material provided in the first aspect, comprising the following steps:
[0011] Step S1, mixing trivalent iron salt, sodium salt, titanium salt and water, adjusting the pH value to 1-2, and sequentially performing heating treatment, drying treatment and first sintering treatment to obtain a titanium-doped iron oxide material;
[0012] Step S2, solid-phase mixing the sodium source, the divalent iron source, and the phosphate, and performing a second sintering treatment to obtain a sodium iron pyrophosphate material;
[0013] Step S3, mixing the sodium iron phosphate pyrophosphate material, the titanium-doped iron oxide material and ethanol, performing ball milling treatment, and obtaining a modified sodium iron phosphate pyrophosphate positive electrode material after drying.
[0014] Furthermore, in step S1, the molar ratio of the trivalent iron salt, the sodium salt and the titanium salt is 1:(8-15):(0.001-0.005).
[0015] Furthermore, in step S2, the molar ratio of the sodium element in the sodium source, the divalent iron source and the phosphate is (4.1-4.2):3:4; and / or, in step S3, the molar ratio of the sodium ferric pyrophosphate material to the titanium-doped iron oxide material is 1:(0.03-0.08).
[0016] Furthermore, the temperature of the heating treatment is 100-130°C, and the time is 4-8h; and / or, the temperature of the first sintering treatment is 600-800°C, and the time is 10-30min; and / or, the second sintering treatment is carried out under an inert atmosphere, and the inert atmosphere includes at least one of nitrogen and argon; the temperature of the second sintering treatment is 850-1100°C, and the time is 10-30h; and / or, the rotation speed of the ball milling treatment is 250-400r / min, the diameter of the ball milling medium is 5-8mm, the ball-to-material ratio is (8-15):1, the temperature is room temperature, and the ball milling time is 0.5-5h.
[0017] Further, the trivalent iron salt includes ferric chloride; and / or, the sodium salt includes at least one of sodium nitrate and sodium acetate; and / or, the titanium salt includes at least one of titanium trichloride and titanium tetrachloride; and / or, and / or, the sodium source includes at least one of sodium oxide, sodium hydroxide, sodium carbonate, and sodium nitrate; and / or, the divalent iron source includes at least one of ferrous nitrate, ferrous acetate, and ferrous oxide; and / or, the phosphate includes at least one of diammonium hydrogen phosphate and ammonium dihydrogen phosphate.
[0018] The third aspect of the present invention provides a sodium ion battery, comprising the modified sodium ferrous sulfate positive electrode material provided by the first aspect or the modified sodium ferric phosphate pyrophosphate positive electrode material prepared by the preparation method provided by the second aspect.
[0019] The implementation of the present invention has at least the following beneficial effects:
[0020] The modified sodium iron phosphate pyrophosphate positive electrode material provided by the present invention limits the materials of the matrix and the support. Since the titanium-doped iron oxide material contains trivalent iron ions, the irreversible migration of iron ions in the lattice during the desodiumization process can be effectively suppressed, the concentration of iron ions inside and on the surface of the crystal can be ensured to be stable, and the reversibility of the material crystal structure can be effectively improved; at the same time, the titanium in the titanium-doped iron oxide material can provide a large number of reactive active sites, and can further form Na-Ti-O bonds with the sodium ions in the matrix material. The chemical bonds have the characteristics of a fast ion conductor and can effectively promote the rapid transmission of sodium ions and electrons. Therefore, the modified sodium iron phosphate pyrophosphate positive electrode material is applied to a sodium ion battery, which is helpful to improve the cycle stability and rate performance of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope (SEM) image of the modified sodium iron phosphate pyrophosphate positive electrode material in Example 1 of the present invention;
[0022] Figure 2 This is a transmission electron microscope (TEM) image of the modified sodium iron phosphate pyrophosphate positive electrode material in Example 1 of the present invention after 100 cycles under 2C conditions;
[0023] Figure 3 This is a transmission electron microscope (TEM) image of the positive electrode material in Comparative Example 1 of the present invention after 100 cycles under 2C conditions. DETAILED DESCRIPTION
[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0025] As described in the background art, it is difficult for existing iron-based phosphate pyrophosphates to improve both rate performance and cycle performance. In order to solve the above technical problems, the first aspect of the present invention provides a modified sodium iron phosphate pyrophosphate positive electrode material, including sodium iron phosphate pyrophosphate and a titanium-doped iron oxide material loaded on the sodium iron phosphate pyrophosphate.
[0026] In the modified sodium iron phosphate pyrophosphate positive electrode material of the present invention, the sodium iron phosphate pyrophosphate is used as a base material, and the titanium-doped iron oxide material is used as a modifying material.
[0027] Among them, titanium-doped iron oxide material refers to a material formed by doping titanium into the iron oxide lattice. Titanium-doped iron oxide material can improve the structural stability of the positive electrode material, reduce the structural changes during the charge and discharge process, thereby improving the cycle stability of the battery, and at the same time can improve the electron and sodium ion conductivity of the positive electrode material, thereby improving the battery's multiple efficiency performance.
[0028] Specifically, the titanium-doped iron oxide material contains trivalent iron ions, which can effectively inhibit the irreversible migration of iron ions in the lattice during the sodium removal process, ensure the stability of the concentration of iron ions inside and on the surface of the crystal, and improve the reversibility of the material's crystal structure, thereby helping to improve the battery's rate performance and cycle stability. At the same time, the doped titanium element can provide a large number of reactive sites, improve electronic conductivity, and further form Na-Ti-O bonds with sodium ions in the matrix material. This chemical bond has the characteristics of a fast ion conductor and can effectively promote the rapid transmission of ions and electrons, thereby helping to further improve the material's rate performance.
[0029] The present invention does not limit the specific types of the base material and the modified material. For example, in some embodiments, the chemical formula of sodium iron pyrophosphate is Na4Fe3(PO4)2(P2O7); the chemical formula of titanium-doped iron oxide material is Fe x Ti y O3, wherein x:y = 1: (0.001-0.005), x + y = 2. By limiting the chemical formula of sodium iron phosphate pyrophosphate and titanium-doped iron oxide materials, it is beneficial to exert the synergistic effect between the components and further improve the electrochemical performance of the positive electrode material.
[0030] The present invention does not limit the ratio of the base material and the modified material, and can be adjusted according to actual needs. In some embodiments, the molar ratio of sodium ferric pyrophosphate to titanium-doped iron oxide material is 1: (0.03-0.08), for example, 1: 0.03, 1: 0.05, 1: 0.07, 1: 0.08 or any two of them. By limiting the molar ratio of sodium ferric pyrophosphate to titanium-doped iron oxide material within the above range, the specific capacity of the positive electrode material can be further improved, thereby taking into account the improvement of specific capacity and rate performance.
[0031] In some embodiments, the D50 particle size of the modified sodium iron phosphate pyrophosphate positive electrode material is 5 to 8 μm. By limiting the particle size of the modified sodium iron phosphate pyrophosphate positive electrode material to the above range, it is ensured that the positive electrode material has sufficient exposed active sites to improve the electrochemical performance of the positive electrode material.
[0032] The second aspect of the present invention provides a method for preparing the modified sodium iron phosphate pyrophosphate positive electrode material provided in the first aspect, comprising the following steps:
[0033] Step S1, mixing trivalent iron salt, sodium salt, titanium salt and water, adjusting the pH value to 1-2, and sequentially performing heating treatment, drying treatment and first sintering treatment to obtain a titanium-doped iron oxide material;
[0034] Step S2, solid-phase mixing the sodium source, the divalent iron source, and the phosphate, and performing a second sintering treatment to obtain a sodium iron pyrophosphate material;
[0035] Step S3, mixing the sodium iron phosphate pyrophosphate material, the titanium-doped iron oxide material and ethanol, performing ball milling treatment, and obtaining a modified sodium iron phosphate pyrophosphate positive electrode material after drying.
[0036] Among them, the titanium-doped iron oxide material is first synthesized by a liquid phase annealing method. Specifically, in step S1, first, a precursor solution is prepared: trivalent iron salt, sodium salt, and titanium salt are dissolved in water according to a required molar ratio to form a precursor solution, wherein the ratio of titanium doping can be adjusted according to experimental requirements; then the pH value of the precursor solution is adjusted to 1-2 by a pH regulator. Under acidic conditions, the trivalent iron salt and the titanium salt undergo a hydrolysis reaction to form a hydroxyl oxide (Fe x Ti y OOH), wherein, since trivalent iron is very easy to be passivated in an acidic solution, which slows down or stops the reaction, the introduction of sodium salt can prevent the passivation of trivalent iron, provide an ion conduction medium for the subsequent generation of oxide precursors, and promote the generation of oxide precursors. After heat treatment, while constantly stirring, at this time, the hydroxyl oxide will undergo a decomposition reaction to generate the corresponding oxide, wherein the heat treatment can be achieved through an oil bath; the precipitate is dried in a vacuum drying oven to remove the moisture therein; the dried precipitate is placed in a high-temperature furnace (for example, a muffle furnace) for a first sintering treatment, wherein the temperature and time of the first sintering treatment need to be adjusted according to actual needs, and during the first sintering treatment, the precipitate will be converted into titanium-doped iron oxide nanoparticles. After the first sintering treatment is completed, the sample is taken out of the high-temperature furnace, naturally cooled to room temperature, and the titanium-doped iron oxide nanoparticles are collected to obtain a titanium-doped iron oxide material.
[0037] The titanium-doped iron oxide material can be obtained through the above steps. In the specific implementation process, the raw material ratio, the temperature and time of the first sintering treatment and other parameters can be adjusted according to actual needs to obtain the titanium-doped iron oxide material with specific properties.
[0038] In step S2, the sodium iron pyrophosphate material is first prepared by solid phase sintering. Specifically, the sodium source, the divalent iron source, and the phosphate are placed in a ball mill or a stirrer and mixed thoroughly. The mixing time can be adjusted according to the actual situation to ensure that the raw materials are fully mixed; the mixed raw materials are placed in a high-temperature furnace (for example, a tubular furnace) for a second sintering treatment. The specific temperature of the second sintering treatment can be adjusted according to the experimental conditions and the characteristics of the raw materials to ensure that the reaction is fully carried out; after the second sintering treatment is completed, the sample is taken out of the high-temperature furnace, naturally cooled to room temperature, and the cooled sample is crushed to obtain finer particles. The crushed sample is sieved to remove larger particles and retain the required particle size range to finally obtain the sodium iron pyrophosphate material. The sodium iron pyrophosphate material is prepared by a solid phase method, which has the advantages of simple operation and low cost.
[0039] In step S3, the titanium-doped iron oxide material and the sodium ferrous phosphate pyrophosphate material are compounded by a liquid phase coating method to form a modified sodium ferrous phosphate pyrophosphate positive electrode material. Specifically, the sodium ferrous phosphate pyrophosphate material and the titanium-doped iron oxide material are dispersed in ethanol, and ball milling is performed to ensure sufficient contact, and the concentration, temperature, stirring speed and other conditions of the solution are controlled to form a uniform coating layer on the surface of the sodium ferrous phosphate pyrophosphate material on the titanium-doped iron oxide material; then the coated material is dried to volatilize the ethanol and enhance the bonding force between the titanium-doped iron oxide material and the sodium ferrous phosphate pyrophosphate material.
[0040] The present invention does not limit the ratio of each raw material and can be adjusted according to actual needs. For example, in some embodiments, in step S1, the molar ratio of the trivalent iron salt to the titanium salt is 1: (0.001-0.005), such as 1: 0.001, 1: 0.002, 1: 0.003, 1: 0.004, 1: 0.005 or any two of them, and the molar ratio of the trivalent iron salt to the sodium salt is 1: (8-15), such as 1: 8, 1: 9, 1: 10, 1: 11, 1: 12, 1: 13, 1: 14, 1: 15 or any two of them. By limiting the molar ratio of the trivalent iron salt, the titanium salt and the sodium salt, it is helpful to dope the titanium element into the lattice of the iron oxide, thereby obtaining a titanium-doped iron oxide material.
[0041] In the solid phase synthesis process of sodium ferric phosphate pyrophosphate, the amount of raw materials added can usually be adjusted to meet the stoichiometric ratio. In order to achieve complete reaction, in some embodiments, in step S2, the molar ratio of sodium element, divalent iron source and phosphate in the sodium source is (4.1-4.2):3:4. In this way, by making the sodium source excessive, the reaction can be ensured to be complete and side reactions can be avoided.
[0042] By adjusting the molar ratio of the sodium iron phosphate pyrophosphate material to the titanium-doped iron oxide material, it is helpful to prepare positive electrode materials with different loading amounts. For example, in some embodiments, the molar ratio of the sodium iron phosphate pyrophosphate material to the titanium-doped iron oxide material is 1:(0.03-0.08), such as 1:0.03, 1:0.05, 1:0.07, 1:0.08 or a range composed of any two of them. By limiting the molar ratio of the sodium iron phosphate pyrophosphate to the titanium-doped iron oxide material within the above range, the specific capacity of the positive electrode material can be further improved, thereby taking into account the improvement of the specific capacity and rate performance.
[0043] In some embodiments, the heating treatment temperature is 100-130°C, for example, 100°C, 110°C, 120°C, 130°C or a range consisting of any two thereof, and the time is 4-8h, for example, 4h, 5h, 6h, 7h, 8h or a range consisting of any two thereof.
[0044] The first sintering treatment is used to promote the formation of titanium-doped iron oxide material. In some embodiments, the temperature of the first sintering treatment is 600-800°C, such as 600°C, 700°C, 800°C or any two thereof, and the time is 10-30 minutes, such as 10 minutes, 20 minutes, 30 minutes or any two thereof. By limiting the temperature and time of the first sintering treatment to the above range, the reaction can be promoted to be complete and impurities can be avoided.
[0045] The second sintering treatment is used to promote the formation of the sodium iron phosphate pyrophosphate material. In some embodiments, the second sintering treatment is performed under an inert atmosphere, the inert atmosphere includes at least one of nitrogen and argon; the temperature of the second sintering treatment is 850 to 1100°C, for example, 850°C, 900°C, 950°C, 1000°C, 1100°C or a range consisting of any two thereof, and the time is 10 to 30 hours, for example, 10 hours, 15 hours, 20 hours, 25 hours, 30 hours or a range consisting of any two thereof.
[0046] In some embodiments, the ball milling speed is 250-400 r / min, the diameter of the ball milling medium is 5-8 mm, the ball-to-material ratio is (8-15):1, the temperature is room temperature, and the ball milling time is 0.5-5 h.
[0047] The present invention does not limit the specific types of each raw material. For example, in some embodiments, the trivalent iron salt includes ferric chloride; and / or the sodium salt includes at least one of sodium nitrate and sodium acetate; and / or the titanium salt includes at least one of titanium trichloride and titanium tetrachloride; and / or, and / or, the sodium source includes at least one of sodium oxide, sodium hydroxide, sodium carbonate, and sodium nitrate; and / or, the divalent iron source includes at least one of ferrous nitrate, ferrous acetate, and ferrous oxide; and / or, the phosphate includes at least one of diammonium hydrogen phosphate and ammonium dihydrogen phosphate.
[0048] The third aspect of the present invention provides a sodium ion battery, comprising the modified sodium ferrous sulfate positive electrode material provided by the first aspect or the modified sodium ferric phosphate pyrophosphate positive electrode material prepared by the preparation method provided by the second aspect.
[0049] Due to the inclusion of the modified sodium iron phosphate pyrophosphate positive electrode material, the sodium ion battery of the present invention has excellent electrochemical properties, such as rate performance and cycle stability.
[0050] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0051] Example 1
[0052] The preparation of the modified sodium iron phosphate pyrophosphate positive electrode material of this embodiment includes the following steps:
[0053] Step S1, dissolving 0.5mmol FeCl3 and 5mmol NaNO3 in 10mL deionized water to form solution A; adding 1μmol TiCl4 to solution A, and adjusting the pH value of the solution to 1.5 with 5mol / L hydrochloric acid to obtain solution B; subjecting solution B to a 100°C oil bath reaction for 4h, washing and drying, and then transferring it to a muffle furnace for high-temperature sintering at 680°C for 20min to obtain Ti-doped Fe2O3 nanomaterials.
[0054] Step S2, after solid phase mixing 0.0207 mol Na2O, 0.03 mol FeO and 0.04 mol (NH4)2HPO4, placing the mixture in a tube furnace and sintering at 950°C for 24 hours to prepare Na4Fe3(PO4)2(P2O7) positive electrode material;
[0055] Step S3, disperse the Na4Fe3(PO4)2(P2O7) positive electrode material in ethanol, add the Ti-doped Fe2O3 nanomaterial prepared in step S1, and perform ball milling mixing at 300r / min at room temperature for 2h, the ball-to-material ratio is 10:1, the diameter distribution of the ball milling beads is 40% with a diameter of 8mm, and the diameter is 60% with a diameter of 5mm. After drying at 75°C, the Ti-doped Fe2O3@Na4Fe3(PO4)2(P2O7) positive electrode material is finally obtained.
[0056] Example 2
[0057] The preparation of the modified sodium iron phosphate pyrophosphate positive electrode material of this embodiment includes the following steps:
[0058] Step S1, dissolving 0.3mmol FeCl3 and 3mmol NaNO3 in 10mL deionized water to form solution A; adding 0.6μmol TiCl3 to solution A, adjusting the pH value of the solution to 1.5 with 5mol / L hydrochloric acid to obtain solution B; subjecting solution B to a 100°C oil bath reaction for 4h, washing and drying, and then transferring it to a muffle furnace for high-temperature sintering at 680°C for 20min to obtain Ti-doped Fe2O3 nanomaterials.
[0059] Step S2, after solid phase mixing 0.0207 mol Na2O, 0.03 mol FeO, and 0.04 mol (NH4)2HPO4, placing the mixture in a tube furnace and sintering at 950°C for 24 hours to prepare a Na4Fe3(PO4)2(P2O7) positive electrode material;
[0060] Step S3, dispersing the Na4Fe3(PO4)2(P2O7) cathode material in ethanol, adding the Ti-doped Fe2O3 nanomaterial prepared in step S1, and ball milling at 250r / min for 2h at room temperature, with a ball-to-material ratio of 8:1, and a ball milling bead diameter distribution of 40% diameter 8mm and 60% diameter 5mm. After drying at 80°C, the Ti-doped Fe2O3@Na4Fe3(PO4)2(P2O7) cathode material was finally obtained.
[0061] Example 3
[0062] The preparation of the modified sodium iron phosphate pyrophosphate positive electrode material of this embodiment includes the following steps:
[0063] Step S1, dissolving 0.8mmol FeCl3 and 8mmol NaNO3 in 10ml deionized water to form solution A; adding 1.6μmol TiCl4 to solution A; adjusting the pH value of the solution to 1.5 with 5mol / L hydrochloric acid to obtain solution B; subjecting solution B to a 100°C oil bath reaction for 4h, washing and drying, and then transferring it to a muffle furnace for high-temperature sintering at 680°C for 20min to obtain Ti-doped Fe2O3 nanomaterials.
[0064] Step S2, after solid phase mixing 0.0207 mol Na2O, 0.03 mol FeO and 0.04 mol (NH4)2HPO4, placing the mixture in a tube furnace and sintering at 950°C for 24 hours to prepare Na4Fe3(PO4)2(P2O7) positive electrode material;
[0065] Step S3, dispersing Na4Fe3(PO4)2(P2O7) cathode material in ethanol, adding the Ti-doped Fe2O3 nanomaterial prepared in step S1, and ball milling at 400r / min for 2h at room temperature, with a ball-to-material ratio of 15:1, and a ball milling bead diameter distribution of 40% diameter 8mm and 60% diameter 5mm. After drying at 85°C, Ti-doped Fe2O3@Na4Fe3(PO4)2(P2O7) cathode material was finally obtained.
[0066] Comparative Example 1
[0067] After 0.0207 mol Na2O, 0.03 mol FeO and 0.04 mol (NH4)2HPO4 were solid-phase mixed, they were placed in a tube furnace and sintered at 950°C for 24 hours to prepare Na4Fe3(PO4)2(P2O7) positive electrode material.
[0068] Comparative Example 2
[0069] The difference from Example 1 is that in step S1, TiCl4 is not added.
[0070] Example 4
[0071] The difference from Example 1 is that in step S1, "1 μmol of TiCl 4" is replaced by "10 μmol of TiCl 4".
[0072] Test example
[0073] 1. Battery Assembly
[0074] The prepared products of the embodiment and the comparative example were used as positive electrode materials. The positive electrode material, acetylene black (AB), and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 7:2:1, and N-methylpyrrolidone (NMP) was used as a solvent. The mixture was placed in a beaker and stirred at a speed of 800 r / min for 2 hours to obtain a slurry. The slurry was coated on a current collector aluminum foil using an automatic coating machine, placed flat on a tempered glass and dried in a vacuum drying oven at 85°C for 4 hours, and punched into sheets with a diameter of 12 The electrode piece of mm was then dried at 105°C in a vacuum drying oven for 4 h, placed in a glove box with an argon atmosphere and a water and oxygen content of less than 0.1 ppm for 4 h to reduce the moisture adsorbed by the electrode piece during the transfer process, and then assembled into a CR2032 button battery in the glove box; the metallic sodium was rolled into thin sheets and punched into 14 mm round sodium sheets as the negative electrode, 1 mol / L NaClO4 solution was used as the electrolyte, and a glass fiber membrane with a diameter of 16 mm was used as the diaphragm.
[0075] 1. Sodium ion diffusion coefficient (sodium ion conductivity) test
[0076] The sodium ion diffusion coefficient (sodium ion conductivity) test is as follows: the above positive electrode materials are assembled into button cells and an AC impedance test is performed under the test conditions of a disturbance voltage of 5 mV and a test frequency of 0.01 Hz to 100 kHz.
[0077] 2. Electrochemical performance test
[0078] After aging the assembled battery for 12 hours, the first charge and discharge capacity test was performed. The test conditions were: charge to 4V at 0.1C, stand for 1 minute, and then discharge to 2.2V at 0.1C. The charge and discharge curves were obtained, and the first discharge specific capacity D0 from 2.2 to 4V was recorded respectively.
[0079] The battery was charged and discharged at 25°C using a battery charge and discharge tester. The battery was charged to 4V at 0.1C constant current, and then discharged to 2.2V at 0.1C constant current after standing for 1 minute. This cycle was repeated for 5 cycles. After standing for 1 minute, the battery was charged to 4V at 2C constant current. After standing for 1 minute, the battery was discharged to 2.2V at 2C constant current. This cycle was repeated for 100 cycles. The discharge capacity Q1 at the first cycle under 2C conditions and the discharge capacity Q at the 100th cycle under 2C conditions were determined. 100 , calculate the capacity retention rate after 100 cycles according to the following formula:
[0080] Capacity retention rate Q = Q 100 / Q1×100%.
[0081] 3. Rate performance test:
[0082] The battery was charged and discharged at 25°C using a battery charge and discharge tester. The battery was charged to 4V at 2C constant current, then charged to 4V constant voltage until the current decreased by 0.02C. After standing for 5 minutes, the battery was discharged to 2.2V at 2C constant current. The discharge capacity Q was recorded. 2C After standing for 5 minutes, charge at 2C constant current to 4V, switch to 4V constant voltage charging until the current decreases by 0.02C, stand for 5 minutes, discharge at 5C constant current to 2.2V, and record the discharge capacity Q 5C After standing for 5 minutes, charge at 5C constant current to 4V, switch to 4V constant voltage charging until the current decreases by 0.02C, and after standing for 5 minutes, discharge at 10C constant current to 2.2V, and record the discharge capacity Q 10C .
[0083] 4. Structural stability test
[0084] The criterion is whether the primary particles of the positive electrode material are broken after 100 cycles under 2C conditions, and TEM is used to test whether the material particles have cracks.
[0085] The test results are shown in Table 1.
[0086] Table 1
[0087]
[0088] Figure 1 This is a SEM image of the modified sodium iron phosphate pyrophosphate positive electrode material in Example 1. Figure 2 and Figure 3 It can be seen that after 100 cycles under 2C conditions, the positive electrode material particles of Example 1 were not broken, while the positive electrode material particles of Comparative Example 1 were broken, indicating that the positive electrode material of the present invention has excellent structural stability.
[0089] It can be seen from Table 1 that applying the modified sodium iron phosphate pyrophosphate provided by the present invention to a sodium ion battery can effectively improve the rate performance and cycle stability of the battery.
[0090] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A modified sodium iron phosphate pyrophosphate positive electrode material, characterized in that: The invention comprises sodium ferric phosphate pyrophosphate and a titanium-doped iron oxide material supported on the sodium ferric phosphate pyrophosphate.
2. The modified sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The chemical formula of the sodium iron phosphate pyrophosphate is Na4Fe3(PO4)2(P2O7); the chemical formula of the titanium-doped iron oxide material is Fe x Ti y O3, where x:y = 1:(0.001 - 0.005) and x + y = 2.
3. The modified sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The molar ratio of the sodium ferric phosphate pyrophosphate to the titanium-doped iron oxide material is 1:(0.03-0.08).
4. The modified sodium iron phosphate pyrophosphate positive electrode material according to claim 1, characterized in that: The D50 particle size of the modified sodium iron phosphate pyrophosphate positive electrode material is 5 to 8 μm.
5. A method for preparing the modified sodium iron phosphate pyrophosphate positive electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step S1, mixing trivalent iron salt, sodium salt, titanium salt and water, adjusting the pH value to 1-2, and sequentially performing heating treatment, drying treatment and first sintering treatment to obtain a titanium-doped iron oxide material; Step S2, solid-phase mixing the sodium source, the divalent iron source, and the phosphate, and performing a second sintering treatment to obtain a sodium iron pyrophosphate material; Step S3, mixing the sodium iron phosphate pyrophosphate material, the titanium-doped iron oxide material and ethanol, performing ball milling treatment, and obtaining the modified sodium iron phosphate pyrophosphate positive electrode material after drying.
6. The preparation method according to claim 5, characterized in that: In step S1, the molar ratio of the trivalent iron salt, the sodium salt and the titanium salt is 1:(8-15): (0.001~0.005)。 7. The preparation method according to claim 5, characterized in that: In step S2, the molar ratio of the sodium element in the sodium source, the divalent iron source and the phosphate is (4.1-4.2):3:4; and / or the molar ratio of the sodium ferric pyrophosphate material to the titanium-doped iron oxide material is 1:(0.03-0.08).
8. The preparation method according to claim 5, characterized in that: The temperature of the heating treatment is 100-130°C, and the time is 4-8h; and / or, the temperature of the first sintering treatment is 600-800°C, and the time is 10-30min; and / or, the second sintering treatment is carried out under an inert atmosphere, and the inert atmosphere includes at least one of nitrogen and argon; the temperature of the second sintering treatment is 850-1100°C, and the time is 10-30h; and / or, the rotation speed of the ball milling treatment is 250-400r / min, the diameter of the ball milling medium is 5-8mm, the ball-to-material ratio is (8-15):1, the temperature is room temperature, and the time is 0.5-5h.
9. The preparation method according to claim 5, characterized in that: The ferric iron salt includes ferric chloride; and / or, the sodium salt includes at least one of sodium nitrate and sodium acetate; and / or, the titanium salt includes at least one of titanium trichloride and titanium tetrachloride; and / or, and / or, the sodium source includes at least one of sodium oxide, sodium hydroxide, sodium carbonate, and sodium nitrate; and / or, the ferrous iron source includes at least one of ferrous nitrate, ferrous acetate, and ferrous oxide; and / or, the phosphate includes at least one of diammonium hydrogen phosphate and ammonium dihydrogen phosphate.
10. A sodium ion battery, characterized in that: The invention comprises the modified sodium iron phosphate pyrophosphate positive electrode material according to any one of claims 1 to 4 or the modified sodium iron phosphate pyrophosphate positive electrode material prepared by the preparation method according to any one of claims 5 to 9.
Citation Information
Cited By
High-magnification ferric sodium pyrophosphate-barium titanate positive electrode material and preparation method thereof
CN120376637A
Preparation method of ferric sodium pyrophosphate positive electrode material
CN121269666A
Sodium vanadium pyrophosphate composite material, preparation method, sodium ion battery and application
CN121292395A