Polyethylene-based insulated cables and their preparation methods
By synergistically designing a compound base resin and surface-modified nanofillers, combined with stepwise mixing and high-temperature, high-pressure vulcanization processes, the problem of electrical treeing aging in cross-linked polyethylene insulated cables was solved, achieving a comprehensive performance improvement in the insulation layer, making it suitable for medium and high voltage power transmission.
Patent Information
- Application Number
- CN202611437984.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cross-linked polyethylene insulated cables are prone to electrical treeing aging during long-term operation, leading to insulation failure. The dispersion of nanofillers is difficult, and the contradiction between elastomer toughening and heat resistance is hard to resolve.
A polyethylene-based insulated cable is prepared by using a base resin system composed of low-density polyethylene, high-density polyethylene, and linear low-density polyethylene, combined with ethylene-octene copolymer and maleic anhydride-grafted polyethylene, and using surface-modified composite nanofillers and voltage stabilizer 1,2-diphenylethylene glycol. The process involves stepwise mixing and high-temperature and high-pressure vulcanization.
It significantly improves the resistance to electrical treeing, thermal aging stability and dielectric properties of polyethylene-based insulated cables, making them suitable for medium and high voltage power transmission.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application relates to the field of cable material technology, and in particular to a polyethylene-based insulated cable and its preparation method. Background Technology
[0002] Cross-linked polyethylene (XLPE) insulated cables are widely used in medium- and high-voltage power transmission due to their excellent insulation, mechanical, and heat resistance properties. However, long-term operational experience shows that electrical treeing is the main cause of insulation failure in XLPE cables. Electrical treeing is a dendritic discharge channel that forms at micropores or defects inside the insulation under the influence of a strong electric field, leading to insulation breakdown and shortening the cable's service life.
[0003] To improve the electrical dendrite resistance of cross-linked polyethylene insulation materials, existing technologies typically incorporate nanofillers and elastomers. However, in practical applications, these methods still suffer from the following prominent problems: Nanofillers are difficult to disperse. Unmodified nanoparticles have high specific surface energy and are prone to agglomeration in polymer matrices, forming interface defects and local electric field concentrations. This reduces the breakdown field strength and increases dielectric loss, making it difficult to exert the expected electrical tree blocking effect. There is a trade-off between toughening and heat resistance with elastomers. While adding elastomers can improve flexibility, it can lead to a decrease in the heat resistance, mechanical strength, and dimensional stability of the insulation layer, making it difficult to resist long-term thermal aging.
[0004] Therefore, how to simultaneously improve the electrical treeing resistance of polyethylene-based insulated cables through the synergistic design of components and processes has become a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] This application is made in view of the above-mentioned problems, and its purpose is to provide a polyethylene-based insulated cable and a method for preparing the same.
[0006] Specifically, the first aspect of this application provides a polyethylene-based insulated cable, comprising a conductor and an insulation layer covering the conductor. The insulation layer is formed by cross-linking a polyethylene-based insulating material. The polyethylene-based insulating material comprises, by weight, 100 parts of base resin, 5-12 parts of ethylene-octene copolymer, 2-6 parts of maleic anhydride-grafted polyethylene, 2-6 parts of surface-modified composite nanofiller, 0.1-0.5 parts of voltage stabilizer, 0.3-0.8 parts of antioxidant, 0.05-0.2 parts of metal passivator, 1.5-2.5 parts of dicumyl peroxide, and 0.3-1.0 parts of triallyl isocyanurate.
[0007] Furthermore, the base resin is composed of 60-75 parts of low-density polyethylene, 8-15 parts of high-density polyethylene, and 15-25 parts of linear low-density polyethylene.
[0008] Furthermore, the density of the low-density polyethylene is 0.918–0.925 g / cm³. 3 The density of the high-density polyethylene is 0.945–0.955 g / cm³. 3 The linear low-density polyethylene has a density of 0.920–0.930 g / cm³. 3 .
[0009] Furthermore, the surface-modified composite nanofiller is a mixture of nano-silica and nano-magnesium oxide in a mass ratio of 2:1 to 4:1, formed by surface treatment with γ-aminopropyltriethoxysilane, wherein the amount of γ-aminopropyltriethoxysilane is 0.5 to 2 wt% of the total mass of the composite nanofiller; the average particle size of the nano-silica is 20 to 50 nm; and the average particle size of the nano-magnesium oxide is 30 to 80 nm.
[0010] Furthermore, the voltage stabilizer is 1,2-diphenylethylenedione, which is pre-loaded onto the surface of nano-silica.
[0011] Furthermore, the antioxidant is a compound of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010) and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168) in a mass ratio of 1:1 to 1.5:1.
[0012] Furthermore, the metal passivating agent is N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine.
[0013] A second aspect of this application provides a method for preparing the aforementioned polyethylene-based insulated cable, comprising the following steps: S1. Surface-modified composite nanofiller and maleic anhydride-grafted polyethylene are added to a mixer at a mass ratio of 0.8:1 to 1.5:1 and mixed at 120 to 130°C and 40 to 60 rpm for 5 to 8 minutes. The mixture is then extruded and granulated to obtain nanocomposite masterbatch. The surface-modified composite nanofiller contains 1,2-diphenylethylene glycol supported on nano-silica. S2. Add the base resin, ethylene-octene copolymer, nanocomposite masterbatch, antioxidant, and metal passivator to a mixer and mix at 115-125°C and 40-60 rpm for 8-12 minutes. Then cool down to 105-115°C, add dicumyl peroxide and triallyl isocyanurate, and continue mixing for 3-5 minutes to obtain the compound. S3. Feed the compound into a twin-screw extruder and extrude and granulate it at 110-130°C to obtain polyethylene-based insulation material; S4. Extrude polyethylene-based insulation material into the conductor in a cable extruder at 110-130°C, with the die head temperature at 115-125°C. S5. After extrusion, the cable enters the vulcanizing tube. The temperature of the vulcanizing tube is 350-420℃, the nitrogen pressure is 1.1-1.4MPa, and the residence time in the high-temperature zone is 5-12min. The cross-linked cable is then treated at 70-90℃ for 24-48h.
[0014] Furthermore, the preparation method of the surface-modified composite nanofiller includes: Nano-magnesium oxide was vacuum dried at 120–150 °C for 2–4 hours. 1,2-Diphenylethylenedione was dissolved in an ethanol / acetone mixed solvent, and nano-silica was added. The mixture was stirred for 30–60 min under ultrasonic dispersion conditions at 25–40 °C. The solvent was removed by vacuum distillation to obtain nano-silica loaded with 1,2-diphenylethylenedione. Then, the nano-silica loaded with 1,2-diphenylethylenedione and pre-dried nano-magnesium oxide were added to a high-speed mixer, along with γ-aminopropyltriethoxysilane and an aqueous ethanol solution. The mixture was stirred for 30–60 min at 60–80 °C and 800–1200 rpm, and then vacuum dried to obtain a surface-modified composite nanofiller.
[0015] Further, in step S1, the mass ratio of ethanol to acetone in the ethanol / acetone mixed solvent is 1:1 to 1:3, and the mass ratio of 1,2-diphenylethylenedione to the mixed solvent is 1:5 to 1:10.
[0016] Further, in step S2, dicumyl peroxide and triallyl isocyanurate are added in the form of a premixed liquid at a temperature of 40–50°C. Specifically, dicumyl peroxide is first heated to 45–50°C to melt, and then mixed evenly with triallyl isocyanurate and kept warm for later use.
[0017] Furthermore, in step S4, the length-to-diameter ratio of the cable extruder screw is 20:1 to 25:1, and the compression ratio is 2.0:1 to 2.5:1.
[0018] The present invention has the following beneficial effects: This invention significantly improves the overall performance of polyethylene-based insulated cables through the synergistic effect of component design and process optimization. First, a base resin system composed of low-density polyethylene, high-density polyethylene, and linear low-density polyethylene is used, ensuring good processing fluidity while also considering mechanical strength, heat resistance, and crystallinity control. Second, ethylene-octene copolymer is introduced as an elastomer toughening component, and maleic anhydride-grafted polyethylene is used as a compatibilizer, effectively improving the interfacial bonding between the elastomer and the polyethylene matrix. This avoids the heat resistance degradation problem caused by traditional toughening methods, achieving a balance between flexibility and thermal stability.
[0019] Furthermore, this invention innovatively constructs a surface-modified composite nanofiller system: on the one hand, γ-aminopropyltriethoxysilane is used to treat the surface of nano-silica / magnesium oxide, which significantly improves the dispersion stability of nanoparticles in the polyethylene matrix and reduces local electric field distortion caused by agglomeration; on the other hand, the voltage stabilizer 1,2-diphenylethylenedione is preloaded on the surface of nano-silica, so that it can be released in situ in the insulating layer, effectively suppressing the avalanche effect of free electrons under high electric field and delaying the initiation and development of electrical trees.
[0020] In terms of the preparation process, a step-by-step mixing strategy is adopted. First, the nanofiller and compatibilizer are pre-formed into masterbatch, which is then mixed with the main resin and other additives in stages. The temperature of the crosslinking agent is strictly controlled to avoid premature crosslinking reaction, ensuring uniform dispersion and stable processing of materials. The vulcanization stage uses a high-temperature, high-pressure nitrogen atmosphere to promote full crosslinking while inhibiting oxidative degradation. The final cable insulation layer has excellent resistance to electrical dendrites, thermal aging stability, and dielectric properties, making it suitable for medium and high voltage power transmission scenarios. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of this application clearer, the following description and illustration are provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application. All other embodiments obtained by those skilled in the art based on the embodiments provided in this application without inventive effort are within the scope of protection of this application.
[0022] Obviously, the following description is merely some examples or embodiments of this application. Those skilled in the art can apply this application to other similar scenarios without any inventive effort. Furthermore, it is understood that although the effort involved in such development may be complex and lengthy, for those skilled in the art related to the content disclosed in this application, any changes to design, manufacturing, or production based on the technical content disclosed in this application are merely conventional technical means and should not be construed as insufficient disclosure of the content of this application.
[0023] An embodiment of the first aspect of this application provides a polyethylene-based insulated cable, comprising a conductor and an insulating layer covering the conductor. The insulating layer is formed by cross-linking a polyethylene-based insulating material, wherein the polyethylene-based insulating material comprises, by weight, 100 parts of base resin, 5-12 parts of ethylene-octene copolymer, 2-6 parts of maleic anhydride-grafted polyethylene, 2-6 parts of surface-modified composite nanofiller, 0.1-0.5 parts of voltage stabilizer, 0.3-0.8 parts of antioxidant, 0.05-0.2 parts of metal passivator, 1.5-2.5 parts of dicumyl peroxide, and 0.3-1.0 parts of triallyl isocyanurate.
[0024] The polyethylene-based insulated cable composition of this invention achieves a synergistic effect of compounded base resin, elastomer toughening components, and surface-modified composite nanofillers, simultaneously ensuring the mechanical strength, flexibility, and heat resistance stability of the insulation layer. This solves the problem of decreased heat resistance caused by traditional elastomer toughening. Furthermore, by pre-loading the voltage stabilizer 1,2-diphenylethylenedione (benzoyl) onto the surface of nano-silica, uniform dispersion of the voltage stabilizer in the matrix is achieved. Combined with the inhibitory effect of the modified nanofillers on electric field distortion, the initiation and growth of electrical trees are effectively delayed, ultimately resulting in a cross-linked polyethylene insulation material with excellent comprehensive performance, meeting the performance requirements for long-term operation of medium and high voltage cables.
[0025] In this embodiment, the base resin is composed of 60-75 parts of low-density polyethylene, 8-15 parts of high-density polyethylene, and 15-25 parts of linear low-density polyethylene. The density of the low-density polyethylene is 0.918-0.925 g / cm³. 3 The density of the high-density polyethylene is 0.945–0.955 g / cm³. 3 The linear low-density polyethylene has a density of 0.920–0.930 g / cm³. 3 .
[0026] The low-density polyethylene is Sinopec 2426H; the high-density polyethylene is Sinopec 5000S; and the linear low-density polyethylene is Sinopec DFDA-7042. The ethylene-octene copolymer used was Dow ENGAGE™ 8150; the maleic anhydride-grafted polyethylene used was Coase-W1B.
[0027] In this embodiment, the surface-modified composite nanofiller is a mixture of nano-silica and nano-magnesium oxide in a mass ratio of 2:1 to 4:1, formed by surface treatment with γ-aminopropyltriethoxysilane. The amount of γ-aminopropyltriethoxysilane is 0.5 to 2 wt% of the total mass of the composite nanofiller. The average particle size of the nano-silica is 20 to 50 nm, and the average particle size of the nano-magnesium oxide is 30 to 80 nm. The surface-modified composite nanofiller functions to block the growth of electrical trees, improve the electric field distribution inside the insulation layer, enhance the heat resistance and breakdown strength of the insulation layer, avoid interface defects caused by nanofiller agglomeration, and synergize with voltage stabilizers to resist electrical tree aging.
[0028] Furthermore, the voltage stabilizer is 1,2-diphenylethylenedione, which is pre-loaded onto the surface of nano-silica. The 1,2-diphenylethylenedione is sourced from Shanghai Aladdin. This method of pre-loading 1,2-diphenylethylenedione onto the surface of nano-silica solves the problem of easy migration and aggregation of 1,2-diphenylethylenedione in the matrix when directly added, and also allows it to be uniformly dispersed in the insulating layer along with the nano-silica.
[0029] In this embodiment, the antioxidant is a compound of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010) and tris(2,4-di-tert-butylphenyl) phosphite (antioxidant 168) in a mass ratio of 1:1 to 1.5:1; the metal passivator is N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine (antioxidant 1024). The compounded antioxidant can simultaneously exert chain termination and hydroperoxide decomposition effects, and together with the metal passivator, inhibit the migration of metal ions from the conductor to the insulating layer, thereby improving the long-term thermal aging stability of the insulating layer.
[0030] An embodiment of the second aspect of this application provides a method for preparing the aforementioned polyethylene-based insulated cable, comprising the following steps: S1. Surface-modified composite nanofiller and maleic anhydride-grafted polyethylene are added to a mixer at a mass ratio of 0.8:1 to 1.5:1 and mixed at 120 to 130°C and 40 to 60 rpm for 5 to 8 minutes. The mixture is then extruded and granulated to obtain nanocomposite masterbatch. The surface-modified composite nanofiller contains 1,2-diphenylethylene glycol supported on nano-silica. S2. Add the base resin, ethylene-octene copolymer, nanocomposite masterbatch, antioxidant, and metal passivator to a mixer and mix at 115-125℃ and 40-60rpm for 8-12 minutes to fully melt the base resin and uniformly disperse the nanocomposite masterbatch and additives. Then cool to 105-115℃ and add a premix of dicumyl peroxide and triallyl isocyanurate (first heat the dicumyl peroxide to 45-50℃ to melt it, then mix it evenly with the triallyl isocyanurate and keep it warm for later use). Continue mixing for 3-5 minutes to prevent the decomposition of dicumyl peroxide and the formation of pre-crosslinking, and obtain the compound. S3. Feed the compound into a twin-screw extruder. The temperatures of each section are set as follows: feeding section 112℃, compression section 118℃, homogenization section 124℃, and die head 122℃; screw speed 200 rpm, feeding rate 15 kg / h. After extrusion, the material is water-cooled and pelletized to obtain polyethylene-based insulation material; the overall extrusion temperature is controlled within the range of 110–130℃, with a maximum of 130℃. S4. The insulating material obtained in S3 is extruded in a cable extruder to coat the 10kV compacted copper conductor. The temperature settings for each section of the extruder are as follows: feeding section 112℃, compression section 120℃, homogenization section 126℃, and die head 118℃; the screw length-to-diameter ratio is 25:1, the compression ratio is 2.2:1, and the screw speed is 40 rpm. The nominal thickness of the insulation layer is 3.4 mm. S5. Immediately after extrusion, the cable is fed into a continuous vulcanizing tube (CCV line). The temperature and process parameters of each section of the vulcanizing tube are as follows: preheating section temperature 355℃, cross-linking section temperature 370℃, and insulation section temperature 390℃; nitrogen pressure is 1.1~1.4MPa, and the residence time in the high-temperature zone is 5~12min; the cross-linked cable is treated at 70~90℃ for 24~48h to remove cross-linking byproducts and obtain the finished polyethylene-based insulated cable.
[0031] In a preferred embodiment, the method for preparing the surface-modified composite nanofiller includes: Nano-magnesium oxide is dried at 120–150°C under a vacuum of -0.09 MPa for 2–4 hours. After drying, it is immediately placed in a desiccator to cool to room temperature for later use. This step removes adsorbed moisture from the surface of nano-MgO to avoid the formation of Mg(OH)2 in subsequent processing, which would lead to increased dielectric loss. 1,2-Diphenylethylene glycol was dissolved in an ethanol / acetone mixed solvent (ethanol to acetone mass ratio of 1:1 to 1:3), and the mass ratio of 1,2-diphenylethylene glycol to the mixed solvent was 1:5 to 1:10; the solution was stirred at room temperature until completely dissolved. Nano-silica was added, and the mixture was stirred for 30 to 60 min under ultrasonic dispersion conditions at 25–40 °C and 40 kHz to allow 1,2-diphenylethylene glycol to be fully adsorbed and loaded onto the surface and pores of nano-SiO2. The solvent was removed by vacuum distillation at 40 °C and a vacuum degree of -0.09 MPa to obtain nano-silica loaded with 1,2-diphenylethylene glycol. Then, nano-silica loaded with 1,2-diphenylethylenedione and pre-dried nano-magnesium oxide were added to a high-speed mixer, along with γ-aminopropyltriethoxysilane (KH550) and an aqueous ethanol solution (ethanol:water = 9:1, mass ratio). The mixture was stirred for 30–60 min at 60–80 °C and 800–1200 rpm, and then vacuum dried at 60 °C for 2 h to obtain the surface-modified composite nanofiller.
[0032] The mass concentration of the ethanol aqueous solution is 90 wt%, and the amount added is 13 wt% of the total mass of the composite nanofiller (containing 1,2-diphenylethylenedione).
[0033] Example The following examples describe the disclosure of this invention in more detail. These examples are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on weight. Unless otherwise stated, all reagents used in the examples are available commercially or synthesized using conventional methods and are ready for use without further processing. Unless otherwise stated, all instruments used in the examples are available commercially.
[0034] Example 1 A polyethylene-based insulated cable includes a conductor and an insulation layer covering the conductor. The insulation layer is formed by cross-linking a polyethylene-based insulating material. The polyethylene-based insulating material comprises, by weight, 70 parts low-density polyethylene, 10 parts high-density polyethylene, 20 parts linear low-density polyethylene, 8 parts ethylene-octene copolymer, 3 parts maleic anhydride-grafted polyethylene, 2.5 parts nano-silica, 1.0 part nano-magnesium oxide, 0.15 parts γ-aminopropyltriethoxysilane, 0.3 parts 1,2-diphenylethylene glycol, 0.3 parts antioxidant 1010, 0.2 parts antioxidant 168, 0.1 parts antioxidant 1024, 2 parts dicumyl peroxide, and 0.6 parts triallyl isocyanurate. The method for preparing the polyethylene-based insulated cable includes the following steps: S1. Preparation of surface-modified composite nanofiller: Dry 1 part of nano magnesium oxide at 130℃ under vacuum of -0.09MPa for 3h, take it out and immediately place it in a desiccator to cool to room temperature for later use; 0.3 parts of 1,2-diphenylethylene glycol were dissolved in 3 parts of a mixed solvent of ethanol and acetone (ethanol to acetone mass ratio of 1:1); the solution was stirred at room temperature until completely dissolved. 2.5 parts of nano-silica were added, and the mixture was stirred for 45 min under ultrasonic dispersion at 30℃ and 40 kHz to allow 1,2-diphenylethylene glycol to be fully adsorbed and loaded onto the surface and pores of nano-SiO2. The solvent was removed by vacuum distillation at 40℃ and a vacuum degree of -0.09 MPa to obtain nano-silica loaded with 1,2-diphenylethylene glycol. Then, nano-silica loaded with 1,2-diphenylethylenedione and 1 part of pre-dried nano-magnesium oxide were added to a high-speed mixer, along with 0.15 parts of γ-aminopropyltriethoxysilane and 1 part of an aqueous ethanol solution (ethanol:water = 9:1, mass ratio). The mixture was stirred at 70℃ and 1000rpm for 60 min, and then vacuum dried at 60℃ for 2 h to obtain the surface-modified composite nanofiller. S2. Add the surface-modified composite nanofiller and 3 parts of maleic anhydride-grafted polyethylene into a mixer and mix them at 125°C and 50 rpm for 6 minutes. Then, extrude and granulate to obtain nanocomposite masterbatch. S3. Add 70 parts of low-density polyethylene, 10 parts of high-density polyethylene, 20 parts of linear low-density polyethylene, 8 parts of ethylene-octene copolymer, nanocomposite masterbatch (approximately 6.8 parts), 0.3 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 0.1 parts of antioxidant 1024 to a mixer and mix at 120°C and 50 rpm for 10 minutes. Then cool to 105°C and add a premix of dicumyl peroxide and triallyl isocyanurate (first heat 2 parts of dicumyl peroxide to 45°C to melt, then mix evenly with 0.6 parts of triallyl isocyanurate and keep warm at 45°C for later use). Continue mixing for 3 minutes to obtain the compound. S4. The compound is fed into a twin-screw extruder, with the following temperatures set: feeding section 110℃, compression section 115℃, homogenization section 120℃, and die head 118℃; screw speed 150 rpm, and feeding rate 15 kg / h. After extrusion, the material is water-cooled and pelletized to obtain polyethylene-based insulation material. S5. The insulation material obtained in S4 is extruded in a cable extruder to coat the 10kV compacted copper conductor. The temperature settings for each section of the extruder are as follows: feeding section 110℃, compression section 118℃, homogenization section 122℃, and die head 116℃; the screw length-to-diameter ratio is 25:1, the compression ratio is 2.2:1, and the screw speed is 40 rpm. The nominal thickness of the insulation layer is 3.4 mm. S6. The extruded cable is immediately fed into the continuous vulcanizing tube. The temperature and process parameters of each section of the vulcanizing tube are as follows: preheating section temperature 355℃, cross-linking section temperature 370℃, heat preservation section temperature 390℃; nitrogen pressure is 1.2MPa, and the residence time in the high-temperature zone is 6min; the cross-linked cable is treated at 80℃ for 36h to remove cross-linking byproducts and obtain the finished polyethylene-based insulated cable.
[0035] Example 2 This embodiment is basically the same as Embodiment 1, except that the polyethylene-based insulation material comprises, by weight, the following: 65 parts of low-density polyethylene, 12 parts of high-density polyethylene, 23 parts of linear low-density polyethylene, 10 parts of ethylene-octene copolymer, 4 parts of maleic anhydride-grafted polyethylene, 2.5 parts of nano-silica, 1.0 part of nano-magnesium oxide, 0.15 parts of γ-aminopropyltriethoxysilane, 0.4 parts of 1,2-diphenylethylenedione, 0.4 parts of antioxidant 1010, 0.3 parts of antioxidant 168, 0.15 parts of antioxidant 1024, 2.2 parts of dicumyl peroxide, and 0.8 parts of triallyl isocyanurate.
[0036] Example 3 This embodiment is basically the same as Embodiment 1, except that the polyethylene-based insulation material comprises, by weight, the following: 75 parts low-density polyethylene, 8 parts high-density polyethylene, 17 parts linear low-density polyethylene, 6 parts ethylene-octene copolymer, 2.5 parts maleic anhydride-grafted polyethylene, 2.0 parts nano silica, 0.8 parts nano magnesium oxide, 0.15 parts γ-aminopropyltriethoxysilane, 0.5 parts 1,2-diphenylethylenedione, 0.25 parts antioxidant 1010, 0.2 parts antioxidant 168, 0.08 parts antioxidant 1024, 1.8 parts dicumyl peroxide, and 0.5 parts triallyl isocyanurate.
[0037] Example 4 This embodiment is basically the same as Embodiment 1, except that the polyethylene-based insulation material comprises, by weight, the following: 68 parts of low-density polyethylene, 11 parts of high-density polyethylene, 21 parts of linear low-density polyethylene, 9 parts of ethylene-octene copolymer, 3.5 parts of maleic anhydride-grafted polyethylene, 3.0 parts of nano-silica, 1.1 parts of nano-magnesium oxide, 0.15 parts of γ-aminopropyltriethoxysilane, 0.35 parts of 1,2-diphenylethylenedione, 0.35 parts of antioxidant 1010, 0.25 parts of antioxidant 168, 0.12 parts of antioxidant 1024, 2.1 parts of dicumyl peroxide, and 0.7 parts of triallyl isocyanurate.
[0038] Example 5 This embodiment is basically the same as Embodiment 1, except that the polyethylene-based insulation material comprises, by weight, the following: 72 parts of low-density polyethylene, 9 parts of high-density polyethylene, 19 parts of linear low-density polyethylene, 7 parts of ethylene-octene copolymer, 3 parts of maleic anhydride-grafted polyethylene, 2.8 parts of nano-silica, 1.0 part of nano-magnesium oxide, 0.15 parts of γ-aminopropyltriethoxysilane, 0.3 parts of 1,2-diphenylethylenedione, 0.3 parts of antioxidant 1010, 0.2 parts of antioxidant 168, 0.1 parts of antioxidant 1024, 2.0 parts of dicumyl peroxide, and 0.6 parts of triallyl isocyanurate.
[0039] Comparative Example 1 This comparative example is basically the same as Example 1, except that it does not contain nano-silica, nano-magnesium oxide, γ-aminopropyltriethoxysilane, maleic anhydride-grafted polyethylene, that is, it does not contain the surface-modified composite nanofiller preparation step S1; 1,2-diphenylethylenedione is added in a free state in step S3.
[0040] Comparative Example 2 This comparative example is basically the same as Example 1, except that γ-aminopropyltriethoxysilane is not included in step S1; maleic anhydride-grafted polyethylene is not included in step S2; and 1,2-diphenylethylenedione is added in a free state in step S3.
[0041] Comparative Example 3 This comparative example is basically the same as Example 1, except that step S3 does not contain ethylene-octene copolymer.
[0042] Comparative Example 4 This comparative example is basically the same as Example 1, except that step S1 does not contain 1,2-diphenylethylenedione and nano magnesium oxide.
[0043] Comparative Example 5 This comparative example is basically the same as Example 1, except that in step S3, the mixing is carried out at 135°C and 50rpm for 10min in the internal mixer; then the temperature is raised to 140°C, and the premixed solution of dicumyl peroxide and triallyl isocyanurate is added and the mixing is continued for 4min. Step S4: The temperature settings for each section of the twin-screw extruder are as follows: feeding section 135℃, compression section 138℃, homogenization section 145℃, and die head 140℃.
[0044] Comparative Example 6 This comparative example is basically the same as Example 1, except that the ratio of nano-SiO2:MgO is 1:1 (1.75 parts each).
[0045] Comparative Example 7 This comparative example is basically the same as Example 1, except that the ratio of nano-SiO2:MgO is 5:1 (2.92 parts SiO2 + 0.58 parts MgO).
[0046] Experimental Case The following tests were conducted on the samples from Examples 1-5 and Comparative Examples 1-7: (1) Volume resistivity: According to GB / T 1410, the sample thickness is 1 mm, the diameter is 100 mm, a DC voltage of 500 V is applied, the reading time is 60 s, and the temperature is 20℃. (2) Dielectric loss tangent: According to GB / T 1409, the sample thickness is 1 mm, the frequency is 50 Hz, the voltage is 1 kV, and the temperature is 20℃; (3) Starting voltage of electrical tree: needle plate electrode method, needle tip curvature radius 5μm, sample thickness 5mm, needle plate spacing 5mm, voltage rise rate of 0.5kV / s at 50Hz, record the voltage when the length of electrical tree reaches 100μm, and take the average value of 5 samples.
[0047] (4) Initiation voltage of electrical tree after thermal aging: After the sample is thermally aged at 80℃ for 30 days, the initiation voltage of electrical tree is tested according to the above method; the test results are shown in Table 1.
[0048] Table 1. Test results of Examples 1-5 and Comparative Examples 1-7
[0049] As shown in Table 1, the polyethylene-based insulated cables prepared in Examples 1-5 are significantly superior to those in Comparative Examples 1-7 in terms of key electrical properties such as volume resistivity, dielectric loss tangent, and electrical tree initiation voltage. Among them, Example 2 exhibits the best overall performance, indicating that it has excellent insulation stability and resistance to electrical treeing.
[0050] In contrast, Comparative Example 1, lacking surface-modified composite nanofillers and with 1,2-diphenylethylene glycol added in a free state, exhibited significantly deteriorated performance across various aspects. This demonstrates that the synergistic loading structure of the nano-SiO2 / MgO composite filler and 1,2-diphenylethylene glycol is crucial for improving the material's insulation properties. Comparative Example 2, lacking silane coupling agent KH550 and maleic anhydride-grafted polyethylene, resulted in decreased filler dispersibility and interfacial compatibility, leading to a significant reduction in performance. In Comparative Example 3, the removal of the ethylene-octene copolymer resulted in compromised material flexibility and dielectric properties. Comparative Example 4, by omitting 1,2-diphenylethylene glycol and nano-magnesium oxide, weakened its free radical capture and thermal stabilization effects. Comparative Example 5, employing excessively high mixing and extrusion temperatures, may have triggered early crosslinking or degradation of polyethylene, affecting the final structural uniformity. Comparative Examples 6 and 7, by adjusting the ratio of nano-SiO2 to MgO away from the preferred range (e.g., 1:1 or 5:1), also resulted in performance inferior to the ratio of 2.0-3.0 parts SiO2 to 0.8-1.1 parts MgO used in Examples 1-5. In summary, this invention effectively improves the electrical properties and long-term operational reliability of polyethylene insulation materials by optimizing the composition of the composite nanofiller, the surface modification process, and the matrix formulation.
[0051] (5) Thermal elongation permanent deformation: According to GB / T 2951.21, the cross-sectional area of the sample is 1.5 mm², a load of 0.2 MPa is applied, and the sample is kept at 200℃ for 15 min. After cooling, the permanent elongation is measured. (6) Space charge density: The maximum space charge density was measured by the pulse electroacoustic method (PEA) with a sample thickness of 0.5 mm and polarized for 30 min under a DC electric field of 30 kV / mm. (7) Tensile strength retention rate after heat aging: The sample was prepared according to GB / T 1040, and the tensile strength was tested after aging at 135℃ for 30 days. The retention rate was calculated by comparing the tensile strength before aging with the tensile strength before aging.
[0052] The test results are shown in Table 2.
[0053] Table 2 Test results of Examples 1-5 and Comparative Examples 1-7
[0054] As shown in Table 2, Examples 1-5 also exhibit significant advantages in terms of thermal elongation permanent deformation, space charge suppression capability, and mechanical retention after thermal aging. Among them, Example 2 shows the lowest thermal elongation permanent deformation and a space charge density of only 1.6 C / m. 3 This indicates that its cross-linked network structure is dense and the interface trap distribution is optimized, effectively suppressing the accumulation of space charge; although its tensile strength retention rate is slightly lower than that of Examples 1 and 3 (89% vs. 93%, 92%), it is still significantly higher than all comparative examples.
[0055] Comparative Example 1, lacking the synergistic reinforcing effect of the composite nanofiller and maleic anhydride-grafted polyethylene, exhibited a thermal elongation deformation as high as 5.0% and a space charge density of 6.5 C / m. 3 This indicates the presence of numerous deep traps and interface defects within the material, which easily induce electric field distortion. In Comparative Example 2, due to the lack of surface modification using γ-aminopropyltriethoxysilane, the interface bonding between the nanofiller and the matrix was poor, leading to a further increase in thermal elongation permanent deformation to 5.9%, and the space charge density also remained at a high level (5.8 C / m²). 3 This reflects the crucial role of interfacial compatibility in suppressing space charge accumulation. Comparative Example 3, lacking the ethylene-octene copolymer, exhibited decreased material flexibility, impaired crosslinking network uniformity, a thermal elongation deformation of 4.1%, and a space charge density reaching 5.2 C / m². 3 In Comparative Example 4, omitting 1,2-diphenylethylenedione and nano-magnesium oxide not only weakened the free radical scavenging ability but also resulted in the loss of the synergistic barrier effect of the composite filler, leading to a mechanical property retention rate of only 79% after thermal aging. Comparative Example 5, due to excessively high processing temperature, experienced partial degradation of the polymer chains, resulting in a permanent thermal elongation deformation as high as 6.9%, the worst among all groups, while the tensile strength retention rate dropped to 72%. Although Comparative Examples 6 and 7 introduced composite nanofillers, the imbalance in the SiO2 to MgO ratio prevented the formation of an effective interface control network, with space charge densities of 4.8 C / m², respectively. 3 and 5.4 C / m 3 The thermal elongation deformation was also significantly higher than that of the example group.
[0056] In summary, this invention, through multi-component synergistic design and precise process control, not only significantly improves the electrical properties of polyethylene insulation materials, but also takes into account their thermomechanical stability and anti-aging ability, providing a reliable technical solution for insulation materials for high-voltage DC cables.
[0057] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A polyethylene-based insulated cable, characterized in that, The device includes a conductor and an insulating layer covering the conductor. The insulating layer is formed by cross-linking a polyethylene-based insulating material. The polyethylene-based insulating material comprises, by weight, 100 parts of base resin, 5-12 parts of ethylene-octene copolymer, 2-6 parts of maleic anhydride-grafted polyethylene, 2-6 parts of surface-modified composite nanofiller, 0.1-0.5 parts of voltage stabilizer, 0.3-0.8 parts of antioxidant, 0.05-0.2 parts of metal passivator, 1.5-2.5 parts of dicumyl peroxide, and 0.3-1.0 parts of triallyl isocyanurate.
2. The polyethylene-based insulated cable according to claim 1, characterized in that, The base resin is composed of 60-75 parts of low-density polyethylene, 8-15 parts of high-density polyethylene, and 15-25 parts of linear low-density polyethylene.
3. The polyethylene-based insulated cable according to claim 1, characterized in that, The surface-modified composite nanofiller is a mixture of nano-silica and nano-magnesium oxide in a mass ratio of 2:1 to 4:1, formed by surface treatment with γ-aminopropyltriethoxysilane. The amount of γ-aminopropyltriethoxysilane used is 0.5 to 2 wt% of the total mass of the composite nanofiller. And / or, the average particle size of the nano-silica is 20–50 nm; And / or, the average particle size of the nano-magnesium oxide is 30-80 nm.
4. The polyethylene-based insulated cable according to claim 2, characterized in that, The voltage stabilizer is 1,2-diphenylethylenedione, which is preloaded onto the surface of nano-silica.
5. The polyethylene-based insulated cable according to claim 1, characterized in that, The antioxidant is a compound of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl)phosphite in a mass ratio of 1:1 to 1.5:
1.
6. The polyethylene-based insulated cable according to claim 1, characterized in that, The metal passivating agent is N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine.
7. A method for preparing a polyethylene-based insulated cable according to any one of claims 1-6, characterized in that, Includes the following steps: S1. The surface-modified composite nanofiller and maleic anhydride-grafted polyethylene are added to a mixer and mixed at 120-130°C, then extruded and granulated to obtain nanocomposite masterbatch; wherein the surface-modified composite nanofiller contains 1,2-diphenylethylene glycol loaded on nano silica. S2. Add the base resin, ethylene-octene copolymer, nanocomposite masterbatch, antioxidant, and metal passivator to a mixer and mix at 115-125°C; then cool down to 105-115°C, add dicumyl peroxide and triallyl isocyanurate and continue mixing to obtain the compound. S3. Feed the compound into a twin-screw extruder and extrude and granulate it at 110-130°C to obtain polyethylene-based insulation material; S4. Extrude polyethylene-based insulation material into the conductor in a cable extruder at 110-130°C, with the die head temperature at 115-125°C. S5. After extrusion, the cable enters the vulcanizing tube. The temperature of the vulcanizing tube is 350-420℃, the nitrogen pressure is 1.1-1.4MPa, and the residence time in the high-temperature zone is 5-12min. The cross-linked cable is then treated at 70-90℃ for 24-48h.
8. The method for preparing a polyethylene-based insulated cable according to claim 7, characterized in that, The preparation method of the surface-modified composite nanofiller includes: Nano-magnesium oxide was vacuum dried at 120–150 °C for 2–4 hours. 1,2-Diphenylethylenedione was dissolved in an ethanol / acetone mixed solvent, and nano-silica was added. The mixture was stirred for 30–60 min under ultrasonic dispersion conditions at 25–40 °C. The solvent was removed by vacuum distillation to obtain nano-silica loaded with 1,2-diphenylethylenedione. Then, the nano-silica loaded with 1,2-diphenylethylenedione and pre-dried nano-magnesium oxide were added to a high-speed mixer, along with γ-aminopropyltriethoxysilane and an aqueous ethanol solution. The mixture was stirred for 30–60 min at 60–80 °C and 800–1200 rpm, and then vacuum dried to obtain a surface-modified composite nanofiller.
9. The method for preparing a polyethylene-based insulated cable according to claim 8, characterized in that, In step S1, the mass ratio of ethanol to acetone in the ethanol / acetone mixed solvent is 1:1 to 1:3, and the mass ratio of 1,2-diphenylethylenedione to the mixed solvent is 1:5 to 1:
10.