A seawater-resistant and corrosion-resistant deep-sea watertight cable material, its preparation method, and the cable.

By using seawater-responsive fillers in deep-sea cable materials, the problem of the spread of corrosive seawater media under local defects in the cable was solved, achieving a balance between the cable's high-efficiency barrier performance and tensile strength.

CN123107220APending Publication Date: 2026-11-17HUNAN XIANGJIANG CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611614491.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing deep-sea cables are unable to effectively limit the spread of corrosive seawater media under localized defects, leading to a decrease in cable durability. Furthermore, the use of inorganic fillers may increase agglomeration and interfacial detachment, affecting the coordination between barrier performance and tensile properties.

Method used

The seawater-responsive filler consists of a calcined magnesium-aluminum layered bimetallic oxide core coated with a first ethylene-acrylic acid ionomer layer and a locking outer layer. It is prepared by atomization spraying to form a seawater-responsive filler with structural memory effect, which reduces the migration of corrosive ions and maintains structural stability during melt processing.

Benefits of technology

It improves the watertight barrier properties of the cable material, reduces the corrosive effect of seawater ions on the internal metal structure, and maintains the tensile strength and processing stability of the cable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of deep-sea cable technology, and more particularly to a seawater-resistant and corrosion-resistant deep-sea watertight cable material, its preparation method, and the cable itself. The cable material comprises high-density polyethylene, metallocene polyethylene, ethylene-octene copolymer, and seawater-responsive filler. The filler has a calcined magnesium-aluminum layered bimetallic oxide core, a first ethylene-acrylic acid ionomer layer, and a locking outer layer. The locking outer layer contains a second ethylene-acrylic acid ionomer and an ethylene-methacrylate glycidyl ester copolymer. The seawater-responsive filler is constructed by drying the pre-formed ionomer, atomizing it, and partially opening the rings of the outer layer. This filler is then blended with polyolefins and used in the inner and outer sheaths of the cable, aiming to balance the material's tensile properties, dimensional stability after seawater immersion, and corrosion protection against internal metal structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of deep-sea cable technology, and in particular to a seawater-resistant and corrosion-resistant deep-sea watertight cable material, its preparation method, and the cable itself. Background Technology

[0002] Deep-sea cables are used for power and signal transmission between seabed observation equipment, underwater operating equipment, and marine engineering facilities. They typically need to maintain sheath integrity under long-term immersion, high hydrostatic pressure, and bending loads during deployment and service. Polyolefin materials possess good water resistance, electrical insulation properties, and processing adaptability, making them suitable for both inner and outer sheaths of cables. By adjusting the composition and proportions of the polyolefin matrix, the strength, flexibility, and extrusion processing performance of the sheath material can be balanced to a certain extent.

[0003] In a complete polyolefin sheath, there is a phenomenon of moisture migration and liquid seawater migration within through-defects. When defects occur in the cable during production or long-term service, moisture can gradually enter the amorphous region of the polymer. Salty seawater is more likely to come into contact with the inside of the sheath along the interface gaps formed during processing, microcracks induced by bending, armor indentations, and local scratches. When there is a pressure difference on both sides of the defect, seawater can continue to migrate along the defect. When water and corrosive ions reach the metal water-blocking layer or armor layer, it may cause local corrosion and affect the cable's durability.

[0004] Existing cable protection technologies typically improve barrier performance by increasing the density of the polyolefin matrix, adding inorganic fillers, installing metal-plastic composite tapes or metal sheaths, and increasing sheath thickness. These measures all rely on the initial barrier structure and are insufficient to continuously limit the spread of corrosive media after localized damage. Furthermore, excessive use of inorganic fillers and incompatible interfacial states can increase agglomeration, interfacial delamination, and stress concentration, thus limiting the balance between barrier performance and tensile properties. Summary of the Invention

[0005] The purpose of this invention is to provide a seawater-resistant and corrosion-resistant deep-sea watertight cable material, its preparation method, and the cable itself, which, while maintaining the processing and tensile properties of polyolefin materials, reduces the risk of seawater continuing to migrate through local defects in the sheath and corroding the internal metal structure.

[0006] A seawater-resistant and corrosion-resistant deep-sea cable material, comprising the following components by weight: 55-70 parts by weight of high-density polyethylene, 30-35 parts by weight of metallocene polyethylene, 10-15 parts by weight of ethylene-octene copolymer, 8-10 parts by weight of seawater responsive filler, 1.5-4 parts by weight of maleic anhydride grafted polyethylene, 1.5-3 parts by weight of carbon black, 0.2-0.8 parts by weight of antioxidant and 0.2-0.8 parts by weight of lubricant; Among them, the melt index of metallocene polyethylene at 190℃ and 2.16kg is 0.5-2g / 10min, and the melt index of ethylene-octene copolymer at 190℃ and 2.16kg is 2-5g / 10min; The seawater responsive packing consists of a calcined magnesium-aluminum layered bimetallic oxide core, a first ethylene-acrylic acid ionomer layer covering the outside of the calcined magnesium-aluminum layered bimetallic oxide core, and a locking outer layer covering the outside of the first ethylene-acrylic acid ionomer layer. The sodium ion neutralization degree of the carboxylic acid groups in the first ethylene-acrylic acid ionomer layer is 55-75 mol%. The locked outer layer is composed of a second ethylene-acrylic acid ionomer with a sodium ion neutralization degree of 15-25 mol% and an ethylene-glycidyl methacrylate copolymer. Some of the unneutralized carboxylic acid groups in the second ethylene-acrylic acid ionomer undergo a ring-opening esterification reaction with the epoxy groups in the ethylene-glycidyl methacrylate copolymer to form covalent bonds.

[0007] Furthermore, in the seawater responsive filler, the locking outer layer is composed of a second ethylene-acrylic acid ionomer and an ethylene-glycidyl methacrylate copolymer in a mass ratio of 1:(0.1-0.15), and some unneutralized carboxylic acid groups undergo a ring-opening reaction with epoxy groups. Based on the mass of each solid component fed during preparation, the mass ratio of the calcined magnesium-aluminum layered bimetallic oxide core, the first ethylene-acrylic acid ionomer used to form the first ethylene-acrylic acid ionomer layer, and the second ethylene-acrylic acid ionomer and ethylene-glycidyl methacrylate copolymer used to form the locking outer layer is 1:(0.15-0.3):(0.1-0.15), and the D50 of the calcined magnesium-aluminum layered bimetallic oxide core is 10-20 μm.

[0008] Furthermore, the calcined magnesium-aluminum layered bimetallic oxide core is obtained by calcining carbonate-type magnesium-aluminum layered bimetallic hydroxide at 480-500℃ for 2-3 hours, and the molar ratio of Mg to Al in the carbonate-type magnesium-aluminum layered bimetallic hydroxide is (3.6-4.2):1.

[0009] Furthermore, the mass fraction of acrylic structural units in the first ethylene-acrylic acid copolymer forming the first ethylene-acrylic acid ionomer layer is 15-22%, the mass fraction of acrylic structural units in the second ethylene-acrylic acid copolymer used to prepare the second ethylene-acrylic acid ionomer in the locking outer layer is 8-15%, and the mass fraction of glycidyl methacrylate structural units in the ethylene-glycidyl methacrylate copolymer is 5-12%.

[0010] A method for preparing a seawater-resistant and corrosion-resistant deep-sea cable material includes the following steps: S1: Magnesium nitrate hexahydrate and aluminum nitrate nonahydrate were prepared into a mixed salt solution, and then co-precipitated with an alkaline solution to prepare carbonate-type magnesium-aluminum layered bimetallic hydroxide, which was then calcined to obtain calcined magnesium-aluminum layered bimetallic oxide core. S2: Dissolve the pre-prepared and dried first ethylene-acrylic acid ionomer powder with a sodium carboxylate ion neutralization degree of 55-75 mol% in a mixed organic solvent to obtain a first ionomer coating liquid. Spray the first ionomer coating liquid onto the surface of the calcined magnesium-aluminum layered bimetallic oxide core in multiple atomizations. Simultaneously evaporate the mixed organic solvent under reduced pressure during the spraying process to deposit the first ethylene-acrylic acid ionomer onto the surface of the calcined magnesium-aluminum layered bimetallic oxide core to obtain a single-coated particle. S3: Dissolve the pre-prepared and dried second ethylene-acrylic acid ionomer powder with a sodium carboxylate ion neutralization degree of 15-25 mol% in a mixed organic solvent to obtain a second ionomer coating liquid. Spray the second ionomer coating liquid onto the surface of the first-coated particles in stages while simultaneously evaporating the mixed organic solvent under reduced pressure to form a second ethylene-acrylic acid ionomer pre-coating layer. Add N,N-dimethylbenzylamine to a xylene solution of ethylene-glycidyl methacrylate copolymer and mix evenly. Then, spray the resulting solution onto the surface of the second ethylene-acrylic acid ionomer pre-coating layer in stages. After removing the xylene, heat and cool to obtain seawater responsive filler. S4: By weight, 8-10 parts of seawater-responsive filler are melt-blended with 55-70 parts of high-density polyethylene, 30-35 parts of metallocene polyethylene, 10-15 parts of ethylene-octene copolymer, 1.5-4 parts of maleic anhydride-grafted polyethylene, 1.5-3 parts of carbon black, 0.2-0.8 parts of antioxidant and 0.2-0.8 parts of lubricant, extruded and granulated to obtain seawater-resistant and corrosion-resistant deep-sea cable material.

[0011] Further, in step S1, magnesium nitrate hexahydrate and aluminum nitrate nonahydrate are prepared into a mixed salt solution with a Mg to Al molar ratio of (3.6-4.2):1. The solution is then co-precipitated with a mixed alkaline solution containing NaOH and Na2CO3 under conditions of 55-70℃ and pH 9.5-10.5. The molar concentration ratio of aluminum nitrate nonahydrate in the mixed salt solution to NaOH and Na2CO3 in the mixed alkaline solution is 1:10:1. The solution is then aged at 80-110℃ for 8-12 hours, washed, dried, and calcined at 480-500℃ for 2-3 hours.

[0012] Furthermore, in steps S2 and S3, the mixed organic solvent used to dissolve the first ethylene-acrylic acid ionomer and the second ethylene-acrylic acid ionomer is composed of tetrachloroethylene, isopropanol, and toluene, with a mass ratio of tetrachloroethylene, isopropanol, and toluene of 80:10:10. The solid content of the first ionomer coating solution and the second ionomer coating solution is 3-5 wt%, and the dissolution temperature is 60-75°C. The coating process in steps S2 and S3 is carried out under particle temperature and reduced pressure conditions of 40-60°C, using a method of multi-stage atomized spraying and simultaneous evaporation of the mixed organic solvent.

[0013] Further, in step S3, the ethylene-glycidyl methacrylate copolymer solution is prepared by dissolving the ethylene-glycidyl methacrylate copolymer in xylene, with a solid content of 3-8 wt%. The amount of N,N-dimethylbenzylamine is 0.05-0.1% of the total mass of the second ethylene-acrylic acid ionomer and the ethylene-glycidyl methacrylate copolymer. After removing xylene, the reaction is carried out at 120-140℃ for 20-40 min.

[0014] Furthermore, in step S4, the temperature of each zone of the twin-screw extruder is 160-185℃, the screw speed is 180-320rpm, and a vacuum exhaust is set after the melting section.

[0015] A seawater-resistant and corrosion-resistant deep-sea watertight cable includes, from the inside out, a conductive functional cable core, an insulation layer, a radial water-blocking layer, an inner sheath layer, an armor layer, and an outer sheath layer, wherein the inner sheath layer and the outer sheath layer are both formed by extrusion of the aforementioned seawater-resistant and corrosion-resistant deep-sea watertight cable material.

[0016] Furthermore, the thickness of the inner sheath layer is 1-3 mm, and the thickness of the outer sheath layer is 4-6 mm.

[0017] Furthermore, the radial water-blocking layer is a metal-plastic composite strip, a longitudinally wrapped welded metal sleeve, or a combination thereof, and the armor layer is one of galvanized steel wire, aluminum alloy wire, or fiber-reinforced armor layer.

[0018] The beneficial effects are: 1. The seawater-responsive filler of this invention uses a calcined magnesium-aluminum layered bimetallic oxide core with structural memory effect as its core. When defects occur during cable production or long-term service, and seawater enters the defect area, the calcined magnesium-aluminum layered bimetallic oxide can react with water and Cl-. - SO4 2- Under the action of anions, restricted hydration reconstruction occurs, which restores the layered structure while fixing corrosive anions. The local volume compensation generated by solid-phase reconstruction reduces the effective cross-section of the permeation channel, thereby reducing the flux of corrosive ions to continue migrating to the armor layer or metal water-blocking layer. This achieves the purpose of improving the watertight barrier performance of the obtained cable material and reducing the corrosive effect of seawater corrosive ions on the internal metal structure.

[0019] 2. This invention prepares a responsive filler by coating a calcined magnesium-aluminum layered bimetallic oxide core with a first ethylene-acrylic acid ionomer layer and a locking outer layer using an atomized spraying method. The locking outer layer is prepared by ring-opening esterification of the epoxy groups of a second ethylene-acrylic acid ionomer and an ethylene-methacrylic acid glycidyl ester copolymer under the action of a ring-opening reaction promoter, thereby forming a β-hydroxy ester covalent bond structure in the locking outer layer. This improves the structural retention of the locking outer layer during subsequent melt processing and long-term seawater exposure, prevents premature rehydration of the calcined magnesium-aluminum layered bimetallic oxide core during coating, and limits large-scale interdiffusion between the first ethylene-acrylic acid ionomer layer and the locking outer layer during subsequent melt extrusion. Simultaneously, the interfacial interaction between the locking outer layer, maleic anhydride-grafted polyethylene, and the polyolefin matrix reduces interfacial defects and stress concentration caused by the introduction of inorganic fillers. The first ethylene-acrylic acid ionomer layer further reacts with Ca2+ after seawater exposure. 2+ Mg 2+ This process forms multivalent ion aggregates, thereby achieving the goals of balancing low water absorption under normal conditions and processing stability, maintaining radial functional zones, reducing the migration of seawater and corrosive ions, and maintaining the tensile strength of the cable material. Detailed Implementation

[0020] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] Example 1: A method for preparing a seawater-resistant and corrosion-resistant deep-sea cable material, comprising the following steps: S1: Preparation of calcined magnesium-aluminum layered bimetallic oxide cores; S1.1: Add 0.36 mol magnesium nitrate hexahydrate and 0.1 mol aluminum nitrate nonahydrate to an appropriate amount of deionized water, stir until completely dissolved, and then use deionized water to make up to 500 mL, so that the molar ratio of Mg to Al is 3.6:1, to obtain a mixed salt solution. Dissolve NaOH and Na2CO3 separately in an appropriate amount of deionized water and mix them to prepare a 500 mL mixed alkaline solution with a NaOH concentration of 2 mol / L and a Na2CO3 concentration of 0.2 mol / L. S1.2: Add 500 mL of deionized water to the reaction vessel and heat to 55 °C. Stir at 500 rpm. Add 500 mL of mixed salt solution to the reaction vessel at a uniform rate over 60 min. At the same time, add mixed alkali solution and adjust the addition rate of mixed alkali solution to maintain the pH of the system at 9.5. After the mixed salt solution is added, stop adding mixed alkali solution and continue stirring at 500 rpm for 1 h to obtain coprecipitated slurry. S1.3: The co-precipitated slurry was placed in a closed hydrothermal reactor and aged at 80℃ for 8 hours. Then it was filtered and the resulting filter cake was repeatedly washed with deionized water until the pH of the final washing liquid was 7.0±0.2 and the conductivity was not higher than 100μS / cm. The resulting filter cake was dried at 90℃ for 10 hours and pulverized to obtain carbonate-type magnesium-aluminum layered bimetallic hydroxide. The carbonate-type magnesium-aluminum layered bimetallic hydroxide was placed in a muffle furnace and heated to 480℃ at a heating rate of 3℃ / min and held at that temperature for 2 hours. After calcination, it was cooled to below 100℃ with the furnace, removed and placed in a desiccator to cool to room temperature and then lightly pulverized so that the D50 of the resulting particles measured by a laser particle size analyzer was 10μm, thus obtaining the calcined magnesium-aluminum layered bimetallic oxide core.

[0022] S2: Preparation of the first ethylene-acrylic acid ionomer layer; S2.1: An ethylene-acrylic acid copolymer with an acrylic structural unit mass fraction of 15% was selected as the first ethylene-acrylic acid copolymer. The first ethylene-acrylic acid copolymer was added to a co-rotating twin-screw extruder for melting. In the melting section, a NaOH aqueous solution with a mass fraction of 20% was added for neutralization reaction. The molar ratio of NaOH in the NaOH aqueous solution to the carboxylic acid groups contained in the first ethylene-acrylic acid copolymer was 0.55:1. After the reaction section, the moisture was removed by vacuum exhaust. The extrudate was air-cooled, pelletized and pulverized at low temperature and then dried under vacuum at 70°C for 8 hours to make its moisture content not higher than 0.5 wt%, so as to obtain the first ethylene-acrylic acid ionomer powder with a sodium carboxylic acid ion neutralization degree of 55 mol%. S2.2: Prepare a mixed organic solvent according to the mass ratio of tetrachloroethylene, isopropanol and toluene of 80:10:10. Add 15 parts by weight of the first ethylene-acrylic acid ionomer powder to the mixed organic solvent and stir for 40 minutes at 60°C and 300 rpm to prepare a first ionomer coating liquid with a solid content of 3 wt%. Add 100 parts by weight of calcined magnesium aluminum layered bimetallic oxide cores to a closed vacuum mixing and coating device equipped with a spray liquid addition device. Keep the particles slowly turning at 40°C. Atomize the first ionomer coating liquid into the particle bed in several times and simultaneously perform reduced pressure evaporation. Control the particle surface to prevent the formation of a continuous free liquid layer during each spraying process. After the first ionomer coating liquid is added, continue drying at 50°C under reduced pressure for 60 minutes. After the particle mass is basically constant, introduce dry nitrogen gas to cool to room temperature to obtain the first coated particles.

[0023] S3: Preparation of the locking outer layer; S3.1: Select an ethylene-acrylic acid copolymer with an acrylic structural unit mass fraction of 8% as the second ethylene-acrylic acid copolymer. Following the same method as step S2.1, control the molar ratio of NaOH in the NaOH aqueous solution to the carboxylic acid groups contained in the second ethylene-acrylic acid copolymer to be 0.15:1 to prepare a second ethylene-acrylic acid ionomer powder with a carboxylic acid sodium ion neutralization degree of 15 mol%. Select an ethylene-glycidyl methacrylate copolymer with a glycidyl methacrylate structural unit mass fraction of 5% as the locking component, and use N,N-dimethylbenzylamine as the ring-opening reaction promoter. S3.2: The second ethylene-acrylic acid ionomer powder and ethylene-glycidyl methacrylate copolymer are mixed at a mass ratio of 1:0.10, so that the total mass of the two is equal to the mass ratio of the calcined magnesium-aluminum layered bimetallic oxide core at 0.10:1. The second ethylene-acrylic acid ionomer powder is prepared into a second ionomer coating liquid with a solid content of 3wt% using a mixed organic solvent of tetrachloroethylene, isopropanol and toluene in a mass ratio of 80:10:10 at 60°C. The primary coated particles are placed in a closed rotary drum vacuum spray coating device, and the second ionomer coating liquid is atomized and sprayed in stages at 40°C while being simultaneously evaporated under reduced pressure, forming a second ethylene-acrylic acid ionomer pre-coating on the outside of the first ethylene-acrylic acid ionomer layer. The first layer involves dissolving ethylene-glycidyl methacrylate copolymer in xylene at 100°C to prepare a 3wt% solids solution. Then, 0.05wt% N,N-dimethylbenzylamine (based on the total mass of the second ethylene-acrylic acid ionomer and the ethylene-glycidyl methacrylate copolymer) is added. The resulting solution is then atomized and sprayed onto the particle surface in multiple stages, and xylene is removed under reduced pressure. Dry nitrogen is then introduced, and the temperature is raised to 120°C and held for 20 minutes to allow some unneutralized carboxylic acid groups to undergo a ring-opening reaction with the epoxy groups, forming a β-hydroxy ester covalently linked structure in the locked outer layer. The solution is then cooled to below 60°C and subjected to airflow classification to remove coarse agglomerates formed during spraying and the reaction process, resulting in a seawater-responsive filler.

[0024] S4: Preparation of seawater-resistant and corrosion-resistant deep-sea cable material; S4.1: Weigh out 55 parts by weight of high-density polyethylene, 30 parts by weight of metallocene polyethylene, 10 parts by weight of ethylene-octene copolymer, 8 parts by weight of seawater responsive filler obtained in step S3, 1.5 parts by weight of maleic anhydride grafted polyethylene, 1.5 parts by weight of carbon black, 0.2 parts by weight of antioxidant and 0.2 parts by weight of lubricant, wherein the melt index of metallocene polyethylene at 190℃ and 2.16kg is 0.5g / 10min, the melt index of ethylene-octene copolymer at 190℃ and 2.16kg is 2g / 10min, the antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, and the lubricant is polyethylene wax; S4.2: According to the raw materials weighed in step S4.1, the seawater responsive filler is dried under vacuum at 80°C for 4 hours. The high-density polyethylene, metallocene polyethylene, ethylene-octene copolymer and maleic anhydride grafted polyethylene are dried at 70°C for 4 hours. The seawater responsive filler, maleic anhydride grafted polyethylene and 11 parts by weight of high-density polyethylene are added to a high-speed mixer and premixed at 800 rpm for 3 minutes. Then, the remaining 44 parts by weight of high-density polyethylene, metallocene polyethylene, ethylene-octene copolymer, carbon black, antioxidant and lubricant are added and mixed at 800 rpm for 5 minutes to obtain the premix. S4.3: The premixed material is added to a co-rotating parallel twin-screw extruder for melt blending. The temperature of each zone of the twin-screw extruder is set to 160℃, the screw speed is 180rpm, and a vacuum exhaust is set after the melting zone with a vacuum degree of -0.08MPa. After cooling and pelletizing, the extrudate is dried under vacuum at 70℃ for 4h to obtain seawater-resistant and corrosion-resistant deep-sea cable material.

[0025] Example 2: A method for preparing a seawater-resistant and corrosion-resistant deep-sea cable material, comprising the following steps: S1: Preparation of calcined magnesium-aluminum layered bimetallic oxide cores; S1.1: Add 0.39 mol magnesium nitrate hexahydrate and 0.1 mol aluminum nitrate nonahydrate to an appropriate amount of deionized water, stir until completely dissolved, and then use deionized water to make up to 500 mL, so that the molar ratio of Mg to Al is 3.9:1, to obtain a mixed salt solution. Dissolve NaOH and Na2CO3 separately in an appropriate amount of deionized water and mix them to prepare a 500 mL mixed alkaline solution with a NaOH concentration of 2 mol / L and a Na2CO3 concentration of 0.2 mol / L. S1.2: Add 500 mL of deionized water to the reaction vessel and heat to 62.5 °C. Stir at 500 rpm. Add 500 mL of mixed salt solution to the reaction vessel at a uniform rate over 60 min. At the same time, add mixed alkali solution and adjust the addition rate of mixed alkali solution to maintain the pH of the system at 10. After the mixed salt solution is added, stop adding mixed alkali solution and continue stirring at 500 rpm for 1 h to obtain coprecipitated slurry. S1.3: The co-precipitated slurry was placed in a closed hydrothermal reactor and aged at 95℃ for 10h. Then it was filtered and the obtained filter cake was repeatedly washed with deionized water until the pH of the last washing liquid was 7.0±0.2 and the conductivity was not higher than 100μS / cm. The obtained filter cake was dried at 90℃ for 10h and pulverized to obtain carbonate-type magnesium-aluminum layered bimetallic hydroxide. The carbonate-type magnesium-aluminum layered bimetallic hydroxide was placed in a muffle furnace and heated to 490℃ at a heating rate of 3℃ / min and held at that temperature for 2.5h. After calcination, it was cooled to below 100℃ with the furnace, removed and placed in a desiccator to cool to room temperature and lightly pulverized so that the D50 of the obtained particles was 15μm as measured by a laser particle size analyzer, thus obtaining the calcined magnesium-aluminum layered bimetallic oxide core.

[0026] S2: Preparation of the first ethylene-acrylic acid ionomer layer; S2.1: An ethylene-acrylic acid copolymer with an acrylic structural unit mass fraction of 18.5% was selected as the first ethylene-acrylic acid copolymer. Based on the total amount of carboxylic acid groups in the first ethylene-acrylic acid copolymer being 1 mol, 0.65 mol of NaOH was added. The NaOH was pre-prepared into a NaOH aqueous solution with a mass fraction of 20 wt%. The first ethylene-acrylic acid copolymer was added to a co-rotating twin-screw extruder for melting. In the melting section, a NaOH aqueous solution with a mass fraction of 20% was added for neutralization reaction. The molar ratio of NaOH in the NaOH aqueous solution to the carboxylic acid groups in the first ethylene-acrylic acid copolymer was 0.65:1. After the reaction section, the moisture was removed by vacuum degassing. The extrudate was air-cooled, pelletized, and pulverized at low temperature, and then dried under vacuum at 70℃ for 8 hours to ensure that the moisture content was not higher than 0.5 wt%, thus obtaining a first ethylene-acrylic acid ionomer powder with a carboxylic acid sodium ion neutralization degree of 65 mol%. S2.2: Prepare a mixed organic solvent with tetrachloroethylene, isopropanol and toluene in a mass ratio of 80:10:10. Add 22.5 parts by weight of the first ethylene-acrylic acid ionomer powder to it and stir for 50 min at 67.5℃ and 400 rpm to prepare a first ionomer coating liquid with a solid content of 4 wt%. Place 100 parts by weight of calcined magnesium aluminum layered bimetallic oxide cores in a closed vacuum mixing and coating equipment with a spray liquid addition device. Perform atomized spraying and simultaneous reduced pressure evaporation at 50℃. During each spraying process, control the particle surface to prevent the formation of a continuous free liquid layer. After the first ionomer coating liquid is added, continue to dry under reduced pressure at 60℃ for 60 min. After the particle mass is basically constant, cool to obtain the first coated particles.

[0027] S3: Preparation of the locking outer layer; S3.1: An ethylene-acrylic acid copolymer with an acrylic structural unit mass fraction of 11.5% was selected as the second ethylene-acrylic acid copolymer. Following the same method as step S2.1, the molar ratio of NaOH in the NaOH aqueous solution to the carboxylic acid groups contained in the second ethylene-acrylic acid copolymer was controlled to be 0.2:1. A second ethylene-acrylic acid ionomer powder with a carboxylic acid sodium ion neutralization degree of 20 mol% was prepared. An ethylene-glycidyl methacrylate copolymer with a glycidyl methacrylate structural unit mass fraction of 8.5% was selected as the locking component, and N,N-dimethylbenzylamine was used as the ring-opening reaction promoter. S3.2: The second ethylene-acrylic acid ionomer powder and ethylene-methacrylate glycidyl ester copolymer were mixed at a mass ratio of 1:0.125, so that the total mass of the two was equal to the mass ratio of the calcined magnesium-aluminum layered bimetallic oxide core at 0.12:1. The second ethylene-acrylic acid ionomer powder was prepared into a second ionomer coating liquid with a solid content of 4wt% using a mixed organic solvent of tetrachloroethylene, isopropanol, and toluene in a mass ratio of 80:10:10 at 67°C. The second ionomer was then atomized and sprayed onto the surface of the primary coated particles in stages at 50°C, with simultaneous vacuum evaporation. Glycidyl methacrylate copolymer was dissolved in xylene at 110°C to prepare a solution with a solid content of 5.5 wt%. N,N-dimethylbenzylamine, accounting for 0.075 wt% of the total mass of the second ethylene-acrylic acid ionomer and ethylene-methacrylate glycidyl methacrylate copolymer, was added. The resulting solution was then sprayed onto the particle surface and xylene was removed under reduced pressure. The mixture was then heated to 130°C under dry nitrogen protection and held for 30 min. After cooling to below 60°C, airflow classification was performed to remove coarse agglomerates formed during the spraying and reaction process, resulting in a seawater responsive filler.

[0028] S4: Preparation of seawater-resistant and corrosion-resistant deep-sea cable material; S4.1: Weigh out 62.5 parts by weight of high-density polyethylene, 32.5 parts by weight of metallocene polyethylene, 12.5 parts by weight of ethylene-octene copolymer, 9 parts by weight of seawater responsive filler obtained in step S3, 2.75 parts by weight of maleic anhydride grafted polyethylene, 2.25 parts by weight of carbon black, 0.5 parts by weight of antioxidant and 0.5 parts by weight of lubricant, wherein the melt index of metallocene polyethylene at 190℃ and 2.16kg is 1.25g / 10min, the melt index of ethylene-octene copolymer at 190℃ and 2.16kg is 3.5g / 10min, the antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, and the lubricant is polyethylene wax; S4.2: According to the raw materials weighed in step S4.1, the seawater responsive filler is dried under vacuum at 80°C for 4 hours. The high-density polyethylene, metallocene polyethylene, ethylene-octene copolymer and maleic anhydride grafted polyethylene are dried at 70°C for 4 hours. The seawater responsive filler, maleic anhydride grafted polyethylene and 12.5 parts by weight of high-density polyethylene are added to a high-speed mixer and premixed at 800 rpm for 3 minutes. Then, the remaining 50 parts by weight of high-density polyethylene, metallocene polyethylene, ethylene-octene copolymer, carbon black, antioxidant and lubricant are added and mixed at 800 rpm for 5 minutes to obtain the premix. S4.3: The premixed material is added to a co-rotating parallel twin-screw extruder for melt blending. The temperature of each zone of the twin-screw extruder is set to 172.5℃, the screw speed is 250rpm, and a vacuum exhaust is set after the melting zone with a vacuum degree of -0.08MPa. After cooling and pelletizing, the extrudate is dried under vacuum at 70℃ for 4h to obtain seawater-resistant and corrosion-resistant deep-sea cable material.

[0029] Example 3: A method for preparing a seawater-resistant and corrosion-resistant deep-sea cable material, comprising the following steps: S1: Preparation of calcined magnesium-aluminum layered bimetallic oxide cores; S1.1: Add 0.42 mol magnesium nitrate hexahydrate and 0.1 mol aluminum nitrate nonahydrate to an appropriate amount of deionized water, stir until completely dissolved, and then use deionized water to make up to 500 mL, so that the molar ratio of Mg to Al is 4.2:1, to obtain a mixed salt solution. Dissolve NaOH and Na2CO3 separately in an appropriate amount of deionized water and mix them to prepare a 500 mL mixed alkaline solution with a NaOH concentration of 2 mol / L and a Na2CO3 concentration of 0.2 mol / L. S1.2: Add 500 mL of deionized water to the reaction vessel and heat to 70 °C. Stir at 500 rpm. Add 500 mL of mixed salt solution to the reaction vessel at a uniform rate over 60 min. At the same time, add mixed alkali solution and adjust the addition rate of mixed alkali solution to maintain the pH of the system at 10.5. After the mixed salt solution is added, stop adding mixed alkali solution and continue stirring at 500 rpm for 1 h to obtain coprecipitated slurry. S1.3: The co-precipitated slurry was placed in a closed hydrothermal reactor and aged at 110℃ for 12h. Then it was filtered and the obtained filter cake was repeatedly washed with deionized water until the pH of the last washing liquid was 7.0±0.2 and the conductivity was not higher than 100μS / cm. The obtained filter cake was dried at 90℃ for 10h and pulverized to obtain carbonate-type magnesium-aluminum layered bimetallic hydroxide. The carbonate-type magnesium-aluminum layered bimetallic hydroxide was placed in a muffle furnace and heated to 500℃ at a heating rate of 3℃ / min and held at that temperature for 3h. After calcination, it was cooled to below 100℃ with the furnace, removed and placed in a desiccator to cool to room temperature and lightly pulverized so that the D50 of the obtained particles was 20μm as measured by a laser particle size analyzer, thus obtaining the calcined magnesium-aluminum layered bimetallic oxide core.

[0030] S2: Preparation of the first ethylene-acrylic acid ionomer layer; S2.1: An ethylene-acrylic acid copolymer with an acrylic structural unit mass fraction of 22% was selected as the first ethylene-acrylic acid copolymer. Based on the total amount of carboxylic acid groups in the first ethylene-acrylic acid copolymer being 1 mol, 0.75 mol of NaOH was added. The NaOH was pre-prepared into a NaOH aqueous solution with a mass fraction of 20 wt%. The first ethylene-acrylic acid copolymer was added to a co-rotating twin-screw extruder for melting. In the melting section, a NaOH aqueous solution with a mass fraction of 20% was added for neutralization reaction. The molar ratio of NaOH in the NaOH aqueous solution to the carboxylic acid groups in the first ethylene-acrylic acid copolymer was 0.75:1. After the reaction section, the moisture was removed by vacuum degassing. The extrudate was air-cooled, pelletized, and pulverized at low temperature, and then dried under vacuum at 70℃ for 8 hours to ensure that the moisture content was not higher than 0.5 wt%, thus obtaining a first ethylene-acrylic acid ionomer powder with a sodium carboxylic acid ion neutralization degree of 75 mol%. S2.2: Prepare a mixed organic solvent with tetrachloroethylene, isopropanol and toluene in a mass ratio of 80:10:10. Add 30 parts by weight of the first ethylene-acrylic acid ionomer powder to it and stir for 60 minutes at 75°C and 500 rpm to prepare a first ionomer coating liquid with a solid content of 5 wt%. Place 100 parts by weight of calcined magnesium aluminum layered bimetallic oxide cores in a closed vacuum mixing and coating equipment with a spray liquid addition device. Atomize and spray in stages at 60°C while simultaneously evaporating under reduced pressure. During each spraying process, control the particle surface to prevent the formation of a continuous free liquid layer. After the first ionomer coating liquid is sprayed, continue to dry under reduced pressure at 70°C for 60 minutes. After the particle mass is basically constant, cool to obtain the first coated particles.

[0031] S3: Preparation of the locking outer layer; S3.1: Select an ethylene-acrylic acid copolymer with an acrylic structural unit mass fraction of 15% as the second ethylene-acrylic acid copolymer. Following the same method as step S2.1, control the molar ratio of NaOH in the NaOH aqueous solution to the carboxylic acid groups contained in the second ethylene-acrylic acid copolymer to be 0.25:1 to prepare a second ethylene-acrylic acid ionomer powder with a carboxylic acid sodium ion neutralization degree of 25 mol%. Select an ethylene-glycidyl methacrylate copolymer with a glycidyl methacrylate structural unit mass fraction of 12% as the locking component, and use N,N-dimethylbenzylamine as the ring-opening reaction promoter. S3.2: The second ethylene-acrylic acid ionomer powder and ethylene-glycidyl methacrylate copolymer were mixed at a mass ratio of 1:0.15, so that the total mass of the two was equal to the mass ratio of the calcined magnesium-aluminum layered bimetallic oxide core of 0.15:1. The second ethylene-acrylic acid ionomer powder was prepared into a second ionomer coating liquid with a solid content of 5wt% using a mixed organic solvent of tetrachloroethylene, isopropanol and toluene in a mass ratio of 80:10:10 at 75°C. The coating was then atomized and sprayed in stages at 60°C with simultaneous vacuum evaporation to coat the ethylene-glycidyl methacrylate copolymer. The hydroglycerol copolymer was dissolved in xylene at 120°C to prepare a solution with a solid content of 8 wt%. N,N-dimethylbenzylamine, accounting for 0.10 wt% of the total mass of the second ethylene-acrylic acid ionomer and ethylene-methacrylate glycidyl copolymer, was added. The resulting solution was then sprayed onto the particle surface and the xylene was removed under reduced pressure. The mixture was then heated to 140°C under dry nitrogen protection and held for 40 min. After cooling to below 60°C, airflow classification was performed to remove the coarse agglomerates formed during the spraying and reaction process, thus obtaining the seawater responsive filler.

[0032] S4: Preparation of seawater-resistant and corrosion-resistant deep-sea cable material; S4.1: Weigh out 70 parts by weight of high-density polyethylene, 35 parts by weight of metallocene polyethylene, 15 parts by weight of ethylene-octene copolymer, 10 parts by weight of seawater responsive filler obtained in step S3, 4 parts by weight of maleic anhydride grafted polyethylene, 3 parts by weight of carbon black, 0.8 parts by weight of antioxidant and 0.8 parts by weight of lubricant, wherein the melt index of metallocene polyethylene at 190℃ and 2.16kg is 2g / 10min, the melt index of ethylene-octene copolymer at 190℃ and 2.16kg is 5g / 10min, the antioxidant is composed of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, and the lubricant is polyethylene wax; S4.2: According to the raw materials weighed in step S4.1, the seawater responsive filler is dried under vacuum at 80°C for 4 hours. The high-density polyethylene, metallocene polyethylene, ethylene-octene copolymer and maleic anhydride grafted polyethylene are dried at 70°C for 4 hours. The seawater responsive filler, maleic anhydride grafted polyethylene and 14 parts by weight of high-density polyethylene are added to a high-speed mixer and premixed at 800 rpm for 3 minutes. Then, the remaining 56 parts by weight of high-density polyethylene, metallocene polyethylene, ethylene-octene copolymer, carbon black, antioxidant and lubricant are added and mixed at 800 rpm for 5 minutes to obtain the premix. S4.3: The premixed material is added to a co-rotating parallel twin-screw extruder for melt blending. The temperature of each zone of the twin-screw extruder is set to 185℃, the screw speed is 320rpm, and a vacuum exhaust is set after the melting zone with a vacuum degree of -0.08MPa. After cooling and pelletizing, the extrudate is dried under vacuum at 70℃ for 4h to obtain seawater-resistant and corrosion-resistant deep-sea cable material.

[0033] Comparative Example 1, compared with Example 2, replaces the calcined magnesium-aluminum layered bimetallic oxide core in step S2 with an equal mass of uncalcined carbonate-type magnesium-aluminum layered bimetallic hydroxide. The uncalcined carbonate-type magnesium-aluminum layered bimetallic hydroxide is from the same batch as the carbonate-type magnesium-aluminum layered bimetallic hydroxide used in Example 2 to prepare the calcined magnesium-aluminum layered bimetallic oxide core. The remaining raw materials, raw material amounts, and preparation methods are the same as in Example 2.

[0034] Comparative Example 2, compared with Example 2, omitted the spraying of the xylene solution of ethylene-glycidyl methacrylate copolymer in step S3.2 and the subsequent ring-opening reaction promoted by N,N-dimethylbenzylamine. The ethylene-glycidyl methacrylate copolymer was replaced by an equal mass of the second ethylene-acrylic acid ionomer, and combined with the original second ethylene-acrylic acid ionomer to prepare the second ionomer coating liquid. The rest of the preparation method was the same as in Example 2.

[0035] Comparative Example 3, compared with Example 2, replaced the first ethylene-acrylic acid ionomer powder with a sodium carboxylate ion neutralization degree of 65 mol% in step S2.1 with the first ethylene-acrylic acid ionomer powder prepared using the same first ethylene-acrylic acid copolymer and a sodium carboxylate ion neutralization degree of 20 mol%, and replaced the first ethylene-acrylic acid ionomer powder in step S2.2 by the same mass. The remaining raw materials, raw material amounts and preparation methods were the same as in Example 2.

[0036] Preparation of test specimens for seawater corrosion resistance test: 1. The cable materials obtained in Examples 1-3 and Comparative Examples 1-3 were hot-pressed into sheets with a thickness of 2±0.1mm under the same conditions. The sheets were cut into 50mm×50mm cover sheets. At the same time, low-carbon steel sheets of the same batch with a size of 50mm×50mm×1mm were selected as the metal substrate to simulate the internal metal structure of the cable. The metal substrate was cleaned with anhydrous ethanol and deionized water in sequence, dried to constant weight, and the initial mass m0 was recorded. Then, the corresponding cable material sheets were hot-pressed onto the surface of the metal steel sheets. The periphery of the sheets was sealed with seawater resistant epoxy sealant. Then, a through-hole with a diameter of 0.5mm was made in the center of the cable material cover layer to simulate the micro-defect state of the cable, and test sample 1 was obtained.

[0037] 2. The cable materials obtained according to Examples 1-3 and Comparative Examples 1-3 were prepared into two sets of test specimens 2 according to GB / T1040.3-2006 standard. One set was used to measure the initial tensile strength Rm0, and the other set was used to measure the tensile strength Rm1 after seawater treatment.

[0038] 3. Cut the cable materials obtained from Examples 1-3 and Comparative Examples 1-3 into pieces with a volume of 1.5 cm³. 3 The small square was used as test sample 3.

[0039] Seawater corrosion resistance test: Artificial seawater was prepared according to ASTM D1141-98 (2021) standard. Test samples 1-3 were immersed in artificial seawater and then placed together in a high-pressure artificial seawater test vessel and kept at 60°C and 30MPa for 45 days.

[0040] Remove the cable sheet from the surface of test specimen 1, clean the corrosion products on the surface of the metal specimen according to ASTM G1-25, dry and weigh it, record the mass m1 after the test, and calculate the metal mass loss rate = (m0-m1) / m0×100%; Take out test specimen 2 and perform tensile strength test according to GB / T1040.3-2006 standard. Record the tensile strength as Rm1 and calculate the tensile strength reduction rate = (Rm0-Rm1) / Rm0×100%; The volume expansion rate of test sample 3 before and after immersion was measured. The volume of test sample 3 was determined by the liquid buoyancy method. Three parallel samples were set up for each test. The average value of the test results was recorded and made into a table, as shown in Table 1.

[0041] Table 1: Seawater Corrosion Resistance of Cable Materials

[0042] As shown in Table 1, Examples 1-3 outperformed the comparative examples in terms of tensile property retention, metal corrosion resistance, and dimensional stability under high-pressure seawater treatment. This indicates that the seawater-responsive filler constructed in this invention helps reduce the migration of seawater into the interior through local defects in the material and improves the material's corrosion protection against internal metal structures, while maintaining good initial tensile properties and mechanical property stability after seawater treatment. Among them, Example 2 showed better performance in initial tensile strength, mechanical property retention after seawater treatment, and metal corrosion resistance, while Example 3 had a lower volume expansion rate, indicating that the functional component content specified in this invention can achieve a good balance between mechanical properties, corrosion resistance, and dimensional stability.

[0043] In Comparative Example 1, replacing the calcined magnesium-aluminum layered bimetallic oxide core with uncalcined carbonate-type magnesium-aluminum layered bimetallic hydroxide significantly reduced both seawater corrosion resistance and dimensional stability, indicating that the structural memory properties obtained after calcination are a crucial basis for the effectiveness of seawater-responsive fillers. When seawater enters the material along its free volume, through micro-defects in processing, or at localized breaks, and comes into contact with the calcined magnesium-aluminum layered bimetallic oxide core, the calcined magnesium-aluminum layered bimetallic oxide can react with water and Cl-. - SO4 2- Under the influence of anions, restricted hydration reconstruction occurs, which reduces the effective flux of corrosive anions migrating into the internal metal structure during the restoration of the layered structure, thereby improving the watertight barrier performance of the cable material and reducing seawater corrosion of the internal metal structure.

[0044] In Comparative Example 2, the removal of the ethylene-glycidyl methacrylate copolymer and its associated carboxylic acid-epoxy covalent locking structure significantly reduced all properties, particularly the retention of tensile strength and dimensional stability after high-pressure seawater treatment. This indicates that the epoxy groups in the ethylene-glycidyl methacrylate copolymer undergo a partial ring-opening reaction with the unneutralized carboxylic acid groups in the second ethylene-acrylic acid ionomer, forming a certain degree of covalent bonding in the locking outer layer. This restricts large-scale interdiffusion between the first ethylene-acrylic acid ionomer layer and the locking outer layer during subsequent melt processing and long-term seawater treatment, while also improving the interfacial stability between the seawater-responsive filler and the polyolefin matrix. Therefore, this locking outer layer not only helps maintain the radial functional zoning of the responsive filler but also reduces defects and stress concentration at the filler interface, enabling the cable material to maintain good initial tensile strength and mechanical properties after seawater treatment.

[0045] In Comparative Example 3, reducing the sodium ion neutralization degree of the first ethylene-acrylic acid ionomer layer resulted in a relatively limited decrease in initial tensile strength. However, the corrosion resistance, retention of tensile properties after seawater treatment, and dimensional stability all significantly deteriorated. This indicates that the main function of the first ethylene-acrylic acid ionomer layer with a higher sodium ion neutralization degree is not simply to improve the initial mechanical properties of the material, but rather to provide more carboxylate sites after seawater enters the material, thus increasing the Ca2+ content. 2+ Mg 2+ It can undergo multivalent ion exchange with polymers and form ion aggregation regions, thereby restricting the movement of local polymer chain segments and changes in free volume, and inhibiting the further migration of moisture and corrosive ions.

[0046] In summary, this invention, through the restricted hydration reconstruction of the calcined magnesium-aluminum layered bimetallic oxide core, the multivalent ion locking of the first ethylene-acrylic acid ionomer layer, and the coordination between the locking outer layers formed by the participation of ethylene-glycidyl methacrylate copolymer, enables the cable material to maintain good mechanical properties and dimensional stability under normal conditions. Furthermore, it generates a local response after seawater enters the material through micro-defects, thereby reducing the risk of high-voltage seawater continuing to migrate through local defects in the material and improving the material's resistance to seawater corrosion, dimensional stability, and ability to retain mechanical properties after long-term seawater exposure.

[0047] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A seawater-resistant and corrosion-resistant deep-sea watertight cable material, characterized in that, Based on parts by weight, it includes the following components: 55-70 parts by weight of high-density polyethylene, 30-35 parts by weight of metallocene polyethylene, 10-15 parts by weight of ethylene-octene copolymer, 8-10 parts by weight of seawater responsive filler, 1.5-4 parts by weight of maleic anhydride grafted polyethylene, 1.5-3 parts by weight of carbon black, 0.2-0.8 parts by weight of antioxidant and 0.2-0.8 parts by weight of lubricant; Among them, the melt index of metallocene polyethylene at 190℃ and 2.16kg is 0.5-2g / 10min, and the melt index of ethylene-octene copolymer at 190℃ and 2.16kg is 2-5g / 10min; The seawater responsive packing consists of a calcined magnesium-aluminum layered bimetallic oxide core, a first ethylene-acrylic acid ionomer layer covering the outside of the calcined magnesium-aluminum layered bimetallic oxide core, and a locking outer layer covering the outside of the first ethylene-acrylic acid ionomer layer. The sodium ion neutralization degree of the carboxylic acid groups in the first ethylene-acrylic acid ionomer layer is 55-75 mol%. The locked outer layer is composed of a second ethylene-acrylic acid ionomer with a sodium ion neutralization degree of 15-25 mol% and an ethylene-glycidyl methacrylate copolymer. Some of the unneutralized carboxylic acid groups in the second ethylene-acrylic acid ionomer undergo a ring-opening esterification reaction with the epoxy groups in the ethylene-glycidyl methacrylate copolymer to form covalent bonds.

2. The seawater-resistant and corrosion-resistant deep-sea cable material as described in claim 1, characterized in that, In the seawater responsive packing, the locking outer layer is composed of a second ethylene-acrylic acid ionomer and an ethylene-glycidyl methacrylate copolymer in a mass ratio of 1:(0.1-0.15), and some unneutralized carboxylic acid groups undergo a ring-opening reaction with epoxy groups. Based on the mass of each solid component fed during preparation, the mass ratio of the calcined magnesium-aluminum layered bimetallic oxide core, the first ethylene-acrylic acid ionomer used to form the first ethylene-acrylic acid ionomer layer, and the second ethylene-acrylic acid ionomer and ethylene-glycidyl methacrylate copolymer used to form the locking outer layer is 1:(0.15-0.3):(0.1-0.15), and the D50 of the calcined magnesium-aluminum layered bimetallic oxide core is 10-20 μm.

3. The seawater-resistant and corrosion-resistant deep-sea watertight cable material according to claim 1, characterized in that, The calcined magnesium-aluminum layered bimetallic oxide core is obtained by calcining carbonate-type magnesium-aluminum layered bimetallic hydroxide at 480-500℃ for 2-3 hours. The molar ratio of Mg to Al in the carbonate-type magnesium-aluminum layered bimetallic hydroxide is (3.6-4.2):

1.

4. The seawater-resistant and corrosion-resistant deep-sea watertight cable material according to claim 1, characterized in that, The first ethylene-acrylic acid copolymer forming the first ethylene-acrylic acid ionomer layer has a mass fraction of 15-22% acrylic acid structural units, the second ethylene-acrylic acid copolymer used to prepare the second ethylene-acrylic acid ionomer in the locking outer layer has a mass fraction of 8-15% acrylic acid structural units, and the ethylene-glycidyl methacrylate copolymer has a mass fraction of 5-12% glycidyl methacrylate structural units.

5. A method for preparing a seawater-resistant and corrosion-resistant deep-sea cable material, characterized in that, Includes the following steps: S1: Magnesium nitrate hexahydrate and aluminum nitrate nonahydrate were prepared into a mixed salt solution, and then co-precipitated with an alkaline solution to prepare carbonate-type magnesium-aluminum layered bimetallic hydroxide, which was then calcined to obtain calcined magnesium-aluminum layered bimetallic oxide core. S2: Dissolve the pre-prepared and dried first ethylene-acrylic acid ionomer powder with a sodium carboxylate ion neutralization degree of 55-75 mol% in a mixed organic solvent to obtain a first ionomer coating liquid. Spray the first ionomer coating liquid onto the surface of the calcined magnesium-aluminum layered bimetallic oxide core in multiple atomizations. Simultaneously evaporate the mixed organic solvent under reduced pressure during the spraying process to deposit the first ethylene-acrylic acid ionomer onto the surface of the calcined magnesium-aluminum layered bimetallic oxide core to obtain a single-coated particle. S3: Dissolve the pre-prepared and dried second ethylene-acrylic acid ionomer powder with a sodium carboxylate ion neutralization degree of 15-25 mol% in a mixed organic solvent to obtain a second ionomer coating liquid. Spray the second ionomer coating liquid onto the surface of the first-coated particles in stages while simultaneously evaporating the mixed organic solvent under reduced pressure to form a second ethylene-acrylic acid ionomer pre-coating layer. Add N,N-dimethylbenzylamine to a xylene solution of ethylene-glycidyl methacrylate copolymer and mix evenly. Then, spray the resulting solution onto the surface of the second ethylene-acrylic acid ionomer pre-coating layer in stages. After removing the xylene, heat and cool to obtain seawater responsive filler. S4: By weight, 8-10 parts of seawater-responsive filler are melt-blended with 55-70 parts of high-density polyethylene, 30-35 parts of metallocene polyethylene, 10-15 parts of ethylene-octene copolymer, 1.5-4 parts of maleic anhydride-grafted polyethylene, 1.5-3 parts of carbon black, 0.2-0.8 parts of antioxidant and 0.2-0.8 parts of lubricant, extruded and granulated to obtain seawater-resistant and corrosion-resistant deep-sea cable material.

6. The preparation method according to claim 5, characterized in that, In step S1, magnesium nitrate hexahydrate and aluminum nitrate nonahydrate are prepared into a mixed salt solution with a Mg to Al molar ratio of (3.6-4.2):

1. The solution is then co-precipitated with a mixed alkaline solution containing NaOH and Na2CO3 under conditions of 55-70℃ and pH 9.5-10.

5. The molar concentration ratio of aluminum nitrate nonahydrate in the mixed salt solution to NaOH and Na2CO3 in the mixed alkaline solution is 1:10:

1. This yields a carbonate-type magnesium-aluminum layered bimetallic hydroxide, which is then aged at 80-110℃ for 8-12 hours, washed, dried, and calcined at 480-500℃ for 2-3 hours.

7. The preparation method according to claim 5, characterized in that, In steps S2 and S3, the mixed organic solvent used to dissolve the first ethylene-acrylic acid ionomer and the second ethylene-acrylic acid ionomer is composed of tetrachloroethylene, isopropanol, and toluene, with a mass ratio of tetrachloroethylene, isopropanol, and toluene of 80:10:

10. The solid content of the first ionomer coating solution and the second ionomer coating solution is 3-5 wt%, and the dissolution temperature is 60-75℃. The coating process in steps S2 and S3 is carried out under particle temperature of 40-60℃ and reduced pressure conditions, using a method of multi-stage atomized spraying and simultaneous evaporation of the mixed organic solvent.

8. The preparation method according to claim 5, characterized in that, In step S3, the ethylene-glycidyl methacrylate copolymer solution is prepared by dissolving the ethylene-glycidyl methacrylate copolymer in xylene, with a solid content of 3-8 wt%. The amount of N,N-dimethylbenzylamine used accounts for 0.05-0.1% of the total mass of the second ethylene-acrylic acid ionomer and the ethylene-glycidyl methacrylate copolymer. After removing xylene, the reaction is carried out at 120-140℃ for 20-40 min.

9. The preparation method according to claim 5, characterized in that, In step S4, the temperature of each zone of the twin-screw extruder is 160-185℃, the screw speed is 180-320rpm, and a vacuum exhaust is set after the melting section.

10. A deep-sea watertight cable resistant to seawater corrosion, characterized in that, It includes a conductive functional cable core, an insulation layer, a radial water-blocking layer, an inner sheath layer, an armor layer, and an outer sheath layer arranged from the inside out. The inner sheath layer and the outer sheath layer are both formed by extrusion of the seawater-resistant and corrosion-resistant deep-sea watertight cable material as described in any one of claims 1-4. The radial water-blocking layer is a metal-plastic composite tape, a longitudinally wrapped welded metal sheath, or a combination thereof. The armor layer is one of galvanized steel wire, aluminum alloy wire, or fiber-reinforced armor layer.