Formulation and preparation method of high temperature resistant ceramic flame retardant heat insulation cable material
Through the synergistic effect of modified kaolin and other components, a dense ceramic network is rapidly formed, which solves the problem of insufficient heat insulation of ceramicized cable materials at high temperatures, achieving efficient heat insulation and flame retardancy, while maintaining good mechanical and processing properties at room temperature.
Patent Information
- Application Number
- CN202611377769.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ceramicized polyolefin cable materials are difficult to form a dense heat insulation layer at high temperatures, and they have fast heat transfer, poor mechanical properties and processing performance at room temperature, and some flame retardant systems also release smoke and toxic gases.
The material comprises kaolin, zinc borate, low-temperature glass powder, modified red phosphorus, nano-montmorillonite, and hollow glass microspheres. Through treatment with a silane coupling agent, kaolin and polymer matrix are well compatible, rapidly forming a dense ceramic network at high temperatures. Red phosphorus decomposes and promotes carbonization to form a framework, while nano-montmorillonite enhances the density of the carbon layer, providing flame retardancy and isolating oxygen.
It rapidly forms a hard ceramic shell in a fire, significantly slowing down temperature transfer and preventing short-circuit failure, while maintaining good flexibility and processability, providing excellent flame retardant and thermal insulation protection.
Smart Images

Figure CN123107340A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer material processing and application technology, specifically referring to the formulation, preparation method and application method of high temperature resistant ceramic flame retardant heat insulation cable material. Background Technology
[0002] Traditional polyolefin cable sheath materials are prone to melting and dripping under high temperatures in fires, failing to form an effective thermal barrier and causing the cable to rapidly lose insulation protection and short-circuit failure. Existing ceramicized polyolefin cable materials can partially sinter in flames to form a ceramic shell, thus maintaining cable integrity to some extent. However, the resulting ceramic layer is usually relatively porous and has rapid heat transfer, making it difficult to provide sufficient thermal insulation protection. In addition, the large amount of inorganic fillers added to increase the ceramicization rate can severely reduce the material's room temperature mechanical properties and processing performance, and some flame-retardant systems release large amounts of smoke and toxic gases during combustion. In the prior art, Chinese patents CN115850843A and CN118620319A disclose "B1-grade medium-voltage fire-resistant ceramicized shell type halogen-free flame-retardant polyolefin cable material" and "ceramicized high flame-retardant polyolefin cable material," respectively. Both enhance the fire resistance of the cable by using a silicone rubber substrate or filling it with large amounts of metal hydroxides such as aluminum hydroxide and magnesium hydroxide. However, these solutions are costly and complex in process. Although they can form a shell at high temperatures, their thermal conductivity is relatively high, making it difficult to meet high insulation requirements. To meet the need for continuous power supply in extreme fire environments, there is an urgent need for a ceramicized cable material that possesses both excellent flame retardancy and insulation properties, capable of rapidly forming a dense, heat-insulating ceramic layer at high temperatures and reducing the hazards of smoke toxicity. Summary of the Invention
[0003] To address the problem of insufficient thermal insulation in existing ceramic fire-resistant cables, this invention provides a high-temperature resistant ceramic flame-retardant thermal insulation cable material formulation and its preparation method.
[0004] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: This invention provides a high-insulation ceramicized polyolefin cable powder, wherein the high-temperature resistant ceramicized flame-retardant heat-insulating cable powder is made from the following components in the indicated mass ratios: 50-80 parts of matrix resin; 30-55 parts of ceramicized filler; 10-25 parts of compounded flame retardant; 8-20 parts of heat insulation enhancer; and 2-10 parts of composite additives. The modified kaolin is surface-treated with a silane coupling agent to improve its compatibility with the polymer matrix; the low-temperature glass powder is an inorganic glass micropowder with a melting point in the range of 400~600℃; the surface-modified red phosphorus refers to red phosphorus micropowder that has been ultra-finely ground and coated with silane or resin; the nano-montmorillonite is preferably organically intercalated modified nano-montmorillonite; the hollow glass microspheres are hollow glass microspheres with a particle size of 10~50μm; the calcined alumina is alumina micropowder obtained by high-temperature calcination, which has high refractoriness and infrared reflectivity. The silane coupling agent is preferably γ-glycidyl etheroxypropyltrimethoxysilane (KH-560), accounting for about 2% of the total filler; the antioxidant is a combination of hindered phenolic antioxidant 1010 and phosphite antioxidant 168; the lubricant is zinc stearate lubricant, etc.
[0005] Preferably, the high-temperature resistant ceramic flame-retardant heat-insulating cable material formulation is pretreated by the following method: the thermoplastic polyurethane elastomer is dried at 65~75℃ for 2~4 hours; kaolin is added to about 3% silane coupling agent ethanol solution and stirred for 2 hours, then filtered and dried to obtain surface-modified kaolin; red phosphorus powder is ground to 700 mesh fineness and coated with silane coupling agent (such as KH560, about 5% of the red phosphorus mass) to obtain modified red phosphorus.
[0006] Preferably, the ceramicized heat-insulating and reinforcing compound flame retardant in the high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation is prepared as follows: The dried thermoplastic polyurethane elastomer and ethylene-vinyl acetate copolymer are added to a mixer and mixed at 80-100°C. After the resin melts, modified kaolin, zinc borate, low-temperature glass powder, modified red phosphorus, and nano-montmorillonite are added sequentially. Mixing continues, and the temperature is gradually increased to approximately 115°C. Then, hollow glass microspheres, calcined alumina, and additives such as silane coupling agents, antioxidants, and lubricants are added. The mixture is mixed until the torque is stable and the material is evenly dispersed to obtain the compounded flame-retardant ceramicized filler.
[0007] This invention also provides an application of the above-mentioned high-temperature resistant ceramic flame-retardant heat-insulating cable material formulation in the preparation of ceramic polyolefin fire-resistant cables.
[0008] Preferably, the method of application is as follows: 50-110 parts of the mixed high thermal insulation ceramicized compound flame retardant and 50-80 parts of the matrix resin are extruded and granulated through a twin-screw extruder. During the extrusion process, the temperature of each zone is controlled as follows: feeding zone about 65°C, melting zone about 125°C, mixing zone about 140°C, and die head zone about 135°C. The screw speed is maintained at 200-250 rpm, and the melt pressure is 8-12 MPa. After the extruded strip is cooled and solidified in a water bath, it is granulated. The resulting granules are dried in hot air at 50°C for 4 hours until the moisture content is less than 0.5%, thus obtaining ceramicized polyolefin particles.
[0009] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention achieves a balance between rapid ceramic formation at high temperatures and efficient heat insulation through the synergistic effect of its components. The ceramic system composed of kaolin, zinc borate, and low-temperature glass powder can form a low-melting eutectic phase at approximately 400–600°C, rapidly sintering the inorganic components into a dense and continuous ceramic network. The resulting ceramic protective layer exhibits high mechanical strength, with a bending strength of 15–20 MPa, enabling it to maintain the integrity of the cable structure in flames. In the flame-retardant system, the coated fine red phosphorus decomposes upon heating, releasing phosphate, which promotes polymer carbonization into a skeletal carbon layer. The inorganic sheets formed by the peeling of nano-montmorillonite during carbonization are embedded in the carbon layer, improving the strength and density of the residual char and providing catalytic flame retardancy and oxygen isolation for thermal decomposition products. The cable material provided by this invention can rapidly form a hard and heat-insulating ceramic shell to protect the cable in a fire, significantly delaying temperature transfer and preventing short-circuit failure. Simultaneously, the material possesses good flexibility and processing properties under normal conditions and can be extruded into cable sheaths. Attached Figure Description
[0010] Figure 1 This is a process flow diagram of the formulation and preparation method of the high-temperature resistant ceramic flame-retardant heat-insulating cable material of the present invention.
[0011] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof. Detailed Implementation
[0012] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0013] The present invention will be further described below with reference to specific embodiments: Example 1 Weigh 40g of thermoplastic polyurethane elastomer granules and place them in an electric constant temperature oven. Set the temperature to 70℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the granules is reduced to below 0.5%. Weigh 25g of ethylene-vinyl acetate copolymer granules and place them in an electric constant temperature oven. Set the temperature to 65℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the EVA granules is reduced to below 0.5%.
[0014] Prepare a 3% silane coupling agent KH-560 ethanol solution. Take 2g of KH-560 and add it to 64.7g of anhydrous ethanol. Stir well and add 20g of kaolin to the solution. Stir at room temperature for 2 hours, then dry in an oven at 100℃ for 1 hour. After pulverizing, pass through a 200-mesh sieve to obtain modified kaolin. Grind 12g of red phosphorus powder to a fineness of 700 mesh or higher, add 0.6g of KH-560 silane coupling agent for coating modification, stir well, and dry in an oven at 80℃ for 1 hour to obtain surface-modified red phosphorus.
[0015] Place 15g of low-temperature glass powder, 8g of zinc borate, 5g of organic intercalated modified nano-montmorillonite, 8g of hollow glass microspheres, and 5g of low-sodium microcrystalline calcined alumina into a drying oven and dry at 80℃ for 1 hour to remove surface moisture. Weigh out 0.5g of antioxidant 1010, 0.5g of antioxidant 168, 2g of zinc stearate, and the remaining 1.4g of KH560 silane coupling agent, mix them evenly, and set aside.
[0016] Add 40g of pretreated thermoplastic polyurethane elastomer and 25g of ethylene-vinyl acetate copolymer to a mixer, set the initial temperature to 80℃, and mix for 3 minutes until the material is completely melted. Then add 20g of pretreated modified kaolin, 8g of zinc borate, 15g of low-temperature glass powder, 12g of surface-modified red phosphorus, and 5g of nano-montmorillonite. Raise the temperature of the mixer to 115℃ and mix for 10 minutes to ensure uniform dispersion of the ceramic component and the flame retardant system. Finally, add 8g of pretreated hollow glass microspheres, 5g of calcined alumina, and the reserved 1.4g of KH-560 silane coupling agent, 0.5g of antioxidant 1010, 0.5g of antioxidant 168, and 2g of zinc stearate. Continue mixing for 5-7 minutes until the mixer torque is balanced. Stop mixing and remove the mixed material.
[0017] A co-rotating twin-screw extruder was used to extrude and granulate the internally mixed material. The extruder temperature was controlled in the following zones: feeding zone: 65℃, melting zone: 125℃, mixing zone: 140℃, and die head zone: 135℃. The screw speed was set to 220 rpm, and the melt pressure was controlled at 10 MPa. The internally mixed material was evenly added to the feeding port and extruded to obtain continuous strips. The extruded strips were then sent to a water tank for cooling, with the water temperature controlled at 28℃ for 5 minutes to allow the strips to completely solidify. The cooled strips were then sent to a pelletizer to cut them into particles with a diameter of 2-3 mm. The cut particles were then placed in a hot air drying oven at 50℃ for 4 hours to obtain ceramicized polyolefin samples.
[0018] Example 2 Weigh 50g of thermoplastic polyurethane elastomer granules and place them in an electric constant temperature oven. Set the temperature to 70℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the granules is reduced to below 0.5%. Weigh 20g of ethylene-vinyl acetate copolymer granules and place them in an electric constant temperature oven. Set the temperature to 65℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the EVA granules is reduced to below 0.5%.
[0019] Prepare a 3% silane coupling agent KH-560 ethanol solution. Take 2g of KH-560 and add it to 64.7g of anhydrous ethanol. Stir well and add 15g of kaolin to the solution. Stir at room temperature for 2 hours, then dry in an oven at 100℃ for 1 hour. After pulverizing, pass through a 200-mesh sieve to obtain modified kaolin. Grind 8g of red phosphorus powder to a mesh size of 700 or higher, add 0.6g of KH-560 silane coupling agent for coating modification, stir well, and dry in an oven at 80℃ for 1 hour to obtain surface-modified red phosphorus.
[0020] Place 10g of low-temperature glass powder, 5g of zinc borate, 3g of organic intercalated modified nano-montmorillonite, 5g of hollow glass microspheres, and 3g of low-sodium microcrystalline calcined alumina into a drying oven and dry at 80℃ for 1 hour to remove surface moisture. Weigh out 0.5g of antioxidant 1010, 0.5g of antioxidant 168, 2g of zinc stearate, and the remaining 1.4g of KH-560 silane coupling agent, mix them evenly, and set aside.
[0021] Add 50g of pretreated thermoplastic polyurethane elastomer and 20g of ethylene-vinyl acetate copolymer to a mixer, set the initial temperature to 80℃, and mix for 3 minutes until the material is completely melted. Then add 15g of pretreated modified kaolin, 5g of zinc borate, 10g of low-temperature glass powder, 8g of surface-modified red phosphorus, and 3g of nano-montmorillonite. Raise the temperature of the mixer to 115℃ and mix for 10 minutes to ensure uniform dispersion of the ceramic component and the flame retardant system. Finally, add 5g of pretreated hollow glass microspheres, 3g of calcined alumina, and the reserved 1.4g of KH-560 silane coupling agent, 0.5g of antioxidant 1010, 0.5g of antioxidant 168, and 2g of zinc stearate. Continue mixing for 5-7 minutes until the mixer torque is balanced. Stop mixing and remove the mixed material.
[0022] A co-rotating twin-screw extruder was used to extrude and granulate the internally mixed material. The extruder temperature was controlled in the following zones: feeding zone: 65℃, melting zone: 125℃, mixing zone: 140℃, and die head zone: 135℃. The screw speed was set to 220 rpm, and the melt pressure was controlled at 10 MPa. The internally mixed material was evenly added to the feeding port and extruded to obtain continuous strips. The extruded strips were then sent to a water tank for cooling, with the water temperature controlled at 28℃ for 5 minutes to allow the strips to completely solidify. The cooled strips were then sent to a pelletizer to cut them into particles with a diameter of 2-3 mm. The cut particles were then placed in a hot air drying oven at 50℃ for 4 hours to obtain ceramicized polyolefin samples.
[0023] Example 3 Weigh 30g of thermoplastic polyurethane elastomer granules and place them in an electric constant temperature oven. Set the temperature to 70℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the granules is reduced to below 0.5%. Weigh 30g of ethylene-vinyl acetate copolymer granules and place them in an electric constant temperature oven. Set the temperature to 65℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the EVA granules is reduced to below 0.5%.
[0024] Prepare a 3% silane coupling agent KH-560 ethanol solution. Take 2g of KH-560 and add it to 64.7g of anhydrous ethanol. Stir well and add 25g of kaolin to the solution. Stir at room temperature for 2 hours, then dry in an oven at 100℃ for 1 hour. After pulverizing, pass through a 200-mesh sieve to obtain modified kaolin. Grind 15g of red phosphorus powder to a fineness of 700 mesh or higher, add 0.6g of KH-560 silane coupling agent for coating modification, stir well, and dry in an oven at 80℃ for 1 hour to obtain surface-modified red phosphorus.
[0025] Place 20g of low-temperature glass powder, 10g of zinc borate, 8g of organic intercalated modified nano-montmorillonite, 12g of hollow glass microspheres, and 8g of low-sodium microcrystalline calcined alumina into a drying oven and dry at 80℃ for 1 hour to remove surface moisture. Weigh out 0.5g of antioxidant 1010, 0.5g of antioxidant 168, 2g of zinc stearate, and the remaining 1.4g of KH-560 silane coupling agent, mix them evenly, and set aside.
[0026] Add 30g of pretreated thermoplastic polyurethane elastomer and 30g of ethylene-vinyl acetate copolymer to a mixer, set the initial temperature to 80℃, and mix for 3 minutes until the material is completely melted. Then add 25g of pretreated modified kaolin, 10g of zinc borate, 20g of low-temperature glass powder, 15g of surface-modified red phosphorus, and 8g of nano-montmorillonite. Raise the temperature of the mixer to 115℃ and mix for 10 minutes to ensure uniform dispersion of the ceramic component and the flame retardant system. Finally, add 12g of pretreated hollow glass microspheres, 8g of calcined alumina, and the reserved 1.4g of KH-560 silane coupling agent, 0.5g of antioxidant 1010, 0.5g of antioxidant 168, and 2g of zinc stearate. Continue mixing for 5-7 minutes until the mixer torque is balanced. Stop mixing and remove the mixed material.
[0027] A co-rotating twin-screw extruder was used to extrude and granulate the internally mixed material. The extruder temperature was controlled in the following zones: feeding zone: 65℃, melting zone: 125℃, mixing zone: 140℃, and die head zone: 135℃. The screw speed was set to 220 rpm, and the melt pressure was controlled at 10 MPa. The internally mixed material was evenly added to the feeding port and extruded to obtain continuous strips. The extruded strips were then sent to a water tank for cooling, with the water temperature controlled at 28℃ for 5 minutes to allow the strips to completely solidify. The cooled strips were then sent to a pelletizer to cut them into particles with a diameter of 2-3 mm. The cut particles were then placed in a hot air drying oven at 50℃ for 4 hours to obtain ceramicized polyolefin samples.
[0028] Comparative Example 1 Weigh 40g of thermoplastic polyurethane elastomer granules and place them in an electric constant temperature oven. Set the temperature to 70℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the granules is reduced to below 0.5%. Weigh 25g of ethylene-vinyl acetate copolymer granules and place them in an electric constant temperature oven. Set the temperature to 65℃ and dry for 3 hours. After removing them, place them in a desiccator to cool to room temperature for later use, ensuring that the moisture content of the EVA granules is reduced to below 0.5%.
[0029] Prepare a 3% silane coupling agent KH-560 ethanol solution. Take 2g of KH-560 and add it to 64.7g of anhydrous ethanol. Stir well and add 20g of kaolin to the solution. Stir at room temperature for 2 hours, then dry in an oven at 100℃ for 1 hour. After pulverizing, pass through a 200-mesh sieve to obtain modified kaolin. Grind 12g of red phosphorus powder to a fineness of 700 mesh or higher, add 0.6g of KH-560 silane coupling agent for coating modification, stir well, and dry in an oven at 80℃ for 1 hour to obtain surface-modified red phosphorus.
[0030] Place 15g of low-temperature glass powder, 8g of zinc borate, 5g of organic intercalated modified nano-montmorillonite, and 5g of low-sodium microcrystalline calcined alumina into a drying oven and dry at 80℃ for 1 hour to remove surface moisture. Weigh out 0.5g of antioxidant 1010, 0.5g of antioxidant 168, 2g of zinc stearate, and the remaining 1.4g of KH-560 silane coupling agent, mix them evenly, and set aside.
[0031] Add 40g of pretreated thermoplastic polyurethane elastomer and 25g of ethylene-vinyl acetate copolymer to a mixer, set the initial temperature to 80℃, and mix for 3 minutes until the material is completely melted. Then add 20g of pretreated modified kaolin, 8g of zinc borate, 15g of low-temperature glass powder, 12g of surface-modified red phosphorus, and 5g of nano-montmorillonite. Raise the temperature of the mixer to 115℃ and mix for 10 minutes to ensure uniform dispersion of the ceramicized components and the flame-retardant system. Finally, add 5g of pretreated calcined alumina, 1.4g of KH-560 silane coupling agent, 0.5g of antioxidant 1010, 0.5g of antioxidant 168, and 2g of zinc stearate. Continue mixing for 5-7 minutes until the mixer torque is balanced. Stop mixing and remove the mixed material.
[0032] A co-rotating twin-screw extruder was used to extrude and granulate the internally mixed material. The extruder temperature was controlled in the following zones: feeding zone: 65℃, melting zone: 125℃, mixing zone: 140℃, and die head zone: 135℃. The screw speed was set to 220 rpm, and the melt pressure was controlled at 10 MPa. The internally mixed material was evenly added to the feeding port and extruded to obtain continuous strips. The extruded strips were then sent to a water tank for cooling, with the water temperature controlled at 28℃ for 5 minutes to allow the strips to completely solidify. The cooled strips were then sent to a pelletizer to cut them into particles with a diameter of 2-3 mm. The cut particles were then placed in a hot air drying oven at 50℃ for 4 hours to obtain ceramicized polyolefin samples.
[0033] Table 1 shows the performance test results of the composite materials prepared in the above embodiments. .
[0034] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
[0035] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention; the actual structure is not limited thereto. In conclusion, if those skilled in the art are inspired by this description and design similar structures and embodiments without departing from the spirit of the invention, such designs should fall within the protection scope of the present invention.
Claims
1. A formula for high-temperature resistant, ceramicized, flame-retardant, and heat-insulating cable material, characterized in that: The high-temperature resistant ceramic flame-retardant heat-insulating cable material formula consists of the following raw materials in parts by weight: 50-80 parts of matrix resin; 30-55 parts of ceramic filler; 10-25 parts of compound flame retardant; 8-20 parts of heat insulation enhancer; and 2-10 parts of composite additives. The matrix resin is a mixture of thermoplastic polyurethane elastomer and ethylene-vinyl acetate copolymer in any proportion; the ceramicized filler is modified kaolin and inorganic low-temperature glass micropowder treated with silane coupling agent; the compounded flame retardant is red phosphorus micropowder coated with silane or resin and organically intercalated modified nano-montmorillonite; the heat insulation reinforcing agent is hollow glass microspheres and calcined alumina; the composite additives are silane coupling agent, composite antioxidant, and zinc stearate lubricant.
2. The high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation according to claim 1, characterized in that, The ceramicized polyolefin powder is prepared as follows: thermoplastic polyurethane elastomer is dried at 65-75°C for 2-4 hours; modified kaolin is added to a silane coupling agent solution for surface treatment and then dried; red phosphorus is ground to a fineness of 700 mesh or higher and coated with a silane coupling agent; the pretreated thermoplastic polyurethane elastomer and ethylene-vinyl acetate copolymer are added to a mixer and melt-mixed at 80-100°C; then modified kaolin, zinc borate, low-temperature glass powder, surface-modified red phosphorus and nano-montmorillonite are added sequentially; the temperature is raised to about 115°C and mixing is continued; then hollow glass microspheres, calcined alumina, silane coupling agent, antioxidant and lubricant are added, and mixing is continued until the torque is stable to obtain the high thermal insulation ceramicized polyolefin mixture.
3. The high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation according to claim 2, characterized in that, The melting point of the low-temperature glass powder is 400–600°C.
4. The high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation according to claim 2, characterized in that, The hollow glass microspheres have a particle size of 10–50 μm and a wall thickness of 1–2 μm.
5. The high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation according to claim 2, characterized in that, The surface-modified red phosphorus is red phosphorus with a particle size of 700 mesh or larger, and is modified by coating with a silane coupling agent.
6. The high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation according to claim 2, characterized in that, The nano-montmorillonite has undergone organic intercalation modification, with an average sheet diameter of 100–500 nm and a sheet thickness of approximately 1 nm.
7. The high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation according to claim 2, characterized in that, The antioxidant is a composite antioxidant of hindered phenolic antioxidant 1010 and phosphite antioxidant 168, with a mass ratio of 1:
1.
8. The application of the high-temperature resistant ceramicized flame-retardant heat-insulating cable material formulation according to claim 1 in the preparation of ceramicized polyolefin fire-resistant cables.
9. The application according to claim 8, characterized in that... The application method is as follows: the mixed material is melt-extruded and granulated through a co-rotating twin-screw extruder. The extrusion process adopts zoned temperature control, wherein the temperature of the feeding zone is 65℃, the temperature of the melting zone is 125℃, the temperature of the mixing zone is 140℃, and the temperature of the die head zone is 135℃. The screw speed is 200-250 rpm. After the extruded strip is cooled with water, it is cut into pellets, and then the pellets are dried with hot air at 50℃ for 4 hours to obtain ceramicized polyolefin particles.
10. The application according to claim 8, characterized in that: The dosage of the high-temperature resistant ceramic flame-retardant heat-insulating cable material formula is 150 parts.
Citation Information
Patent Citations
Ceramic crusting type halogen-free flame-retardant polyolefin fire-resistant cable material for B1-level medium-voltage fire-resistant power cable and preparation method of ceramic crusting type halogen-free flame-retardant polyolefin fire-resistant cable material
CN115850843A
Ceramic high-flame-retardant polyolefin cable material and preparation method thereof
CN118620319A