An inorganic pigment for coloring thermotropic liquid crystal polyester dopes and its preparation method

By using a phased pH control and ethanol rinsing method, an inorganic pigment with a core-shell-coupling layer structure was prepared. This solved the problems of metal ion migration, uneven dispersion, and agglomeration in the coloring of inorganic pigments in thermotropic liquid crystal polyester dopes. It also achieved excellent dispersion and compatibility of the pigment in TLCP melt-spun fibers, thereby improving the color stability and strength of the fibers.

CN123107418APending Publication Date: 2026-11-17GUANGDONG XINGJU MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611177327.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing inorganic pigments used in thermotropic liquid crystal polyester dope coloring suffer from problems such as metal ion migration and catalytic degradation, interfacial incompatibility leading to uneven dispersion, easy dissolution interference and hard agglomeration during preparation, and pigment agglomerates clogging the spinneret during melt spinning.

Method used

By employing a phased pH control strategy, a silica seed layer is deposited in a pH range close to the low dissolution pH of the pigment. Subsequently, a dense shell layer is grown by accelerated condensation under acidic conditions. Combined with an extremely low amount of polyvinylpyrrolidone and a specific ratio of aryl and epoxy-containing bissilane coupling agents, the interaction between the pigment surface and the TLCP aromatic skeleton and thermal stress buffering are ensured. Free tetraethyl orthosilicate monomers are removed by ethanol rinsing to prevent irreversible hard agglomeration.

Benefits of technology

Submicron-level dispersion of inorganic pigments in TLCP melt-spun fibers was achieved, ensuring color stability, dispersion uniformity, and interfacial compatibility, avoiding spinning breakage and fiber strength reduction, and meeting the quality requirements of fiber-grade spinning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure REF-OBJ-1785892789193-000001
    Figure REF-OBJ-1785892789193-000001
  • Figure REF-OBJ-1785892789193-000002
    Figure REF-OBJ-1785892789193-000002
Patent Text Reader

Abstract

This application discloses an inorganic pigment for coloring thermotropic liquid crystal polyester dopes and its preparation method. The preparation method includes: wet grinding of inorganic pigment powder with a low amount of polyvinylpyrrolidone; adding ethanol to prepare a slurry under an inert atmosphere; adjusting the pH in stages and adding tetraethyl orthosilicate sequentially, first depositing a seed layer under weak acidity to block the dissolution channels of metal ions, and then growing a dense silica shell under stronger acidity; subsequently adding a specific proportion of aryl and epoxy-containing bissilane coupling agents under acidic conditions for a grafting reaction; filtering and rinsing the filter cake with ethanol to remove free silicon-containing species; and finally drying and deagglomerating. This application suppresses ion dissolution interference through staged deposition, prevents chemical bridging hard agglomeration through ethanol rinsing, and improves interfacial compatibility through bissilane design, meeting the stringent requirements for submicron pigment dispersion and spinneret passage in fiber-grade TLCP melt spinning processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer material coloring technology, specifically to an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and its preparation method. Background Technology

[0002] Thermotropic liquid crystal polyester (TLCP) is a class of high-performance engineering plastics whose molecular chains spontaneously orient to form an ordered liquid crystal structure in the molten state. It possesses high strength and modulus, low coefficient of linear expansion, and excellent heat and chemical resistance. Besides injection molding applications, TLCP can be melt-spun into high-performance fibers, which are widely used in high-temperature filter materials, protective textiles, composite reinforcing fibers, optical fiber reinforcements, and special cables. Solution dyeing is a process that adds colorants to the melt during TLCP melt spinning to achieve fiber coloring. Compared to post-dyeing, it offers advantages such as high color fastness, uniform color, shorter process, and environmental friendliness. Inorganic pigments are the preferred colorant type for TLCP solution dyeing due to their excellent chemical stability, lightfastness, and weather resistance at high temperatures.

[0003] The processing temperature of TLCP is typically in the range of 280–340°C, and its melt exhibits low viscosity and high shear sensitivity due to its ordered liquid crystal structure, making it extremely sensitive to the surface chemical state of the pigments used for filling. In such a harsh processing environment, inorganic pigments face multiple core challenges: transition metal ions in the pigment lattice may migrate to the TLCP matrix at high temperatures, catalyzing transesterification and thermo-oxidative degradation reactions of the polyester chains; severe interfacial incompatibility exists between the polar hydrophilic properties of the inorganic pigment surface and the highly aromatic hydrophobic framework of TLCP, leading to uneven pigment dispersion; and submicron-sized particles are highly susceptible to irreversible agglomeration throughout the entire process of pigment powder preparation, storage, and use.

[0004] Therefore, it is necessary to provide an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and a method for preparing the same. Summary of the Invention

[0005] To address the technical problems existing in the coloring of TLCP dosings with inorganic pigments, such as metal ion migration and catalytic degradation, uneven dispersion due to interfacial incompatibility, easy dissolution interference and hard agglomeration during preparation, and pigment agglomerates clogging the spinneret during melt spinning, leading to spinneret breakage and fiber strength reduction, this application provides an inorganic pigment for coloring thermotropic liquid crystal polyester dosings and its preparation method.

[0006] The first aspect of this application provides a method for preparing inorganic pigments for coloring thermotropic liquid crystal polyester raw materials, comprising the following steps: wet grinding inorganic pigment powder, polyvinylpyrrolidone, and deionized water until the median particle size D50 is 0.2–1.5 μm, wherein the amount of polyvinylpyrrolidone used is 0.05%–0.20% of the mass of the inorganic pigment powder; adding ethanol to the slurry obtained by grinding under an inert atmosphere to obtain a water-alcohol mixed slurry, and adjusting the pH of the water-alcohol mixed slurry to 5.0. ~6.5, add tetraethyl orthosilicate to react, adjust the pH of the system to 4.0~5.0, add tetraethyl orthosilicate to react, then adjust the pH of the system to 3.0~4.0, add aryl-containing trialkoxysilane and epoxy-containing trialkoxysilane to react, the mass ratio of the aryl-containing trialkoxysilane to the epoxy-containing trialkoxysilane is (1.5~5):1, filter the obtained slurry, wash the filter cake with ethanol; dry the washed filter cake and deagglomerate to obtain inorganic pigment.

[0007] This preparation method employs a staged pH control strategy. First, a silica seed layer is deposited within the pH range close to the low dissolution pH of the pigment (5.0–6.5) to preferentially block metal ion exposure sites and dissolution channels. Subsequently, under acidic conditions (4.0–5.0), the condensation growth of a dense shell is accelerated, fundamentally avoiding the competitive coordination interference between metal ion dissolution and silanol groups, ensuring the density and barrier function of the shell. By controlling the dosage of polyvinylpyrrolidone at extremely low levels (0.05%–0.20%), the dynamic stability of grinding is maintained while preventing excessive organic matter from being embedded in the shell, forming inclusion defects and ion diffusion channels. The introduction of aryl and epoxy-containing bissilane coupling agents in specific proportions allows the pigment surface to simultaneously possess π-π stacking interactions with the TLCP aromatic skeleton and thermal stress buffering and reactive bonding functions. The filter cake is washed with ethanol, which removes free tetraethyl orthosilicate monomers and silane oligomers by taking advantage of ethanol's excellent solubility. This eliminates the precursors that form Si-O-Si chemical bridges during the drying stage, effectively preventing irreversible hard agglomeration and ensuring submicron-level dispersion of pigments in TLCP melt-spun fibers.

[0008] Furthermore, the pH of the slurry is adjusted to 5.0–7.0 during grinding; wet grinding uses 0.2–0.8 mm zirconia grinding beads. This pH range keeps the absolute value of the zeta potential on the surface of most inorganic pigments within the boundary region of dispersion stability. Combined with the steric hindrance effect of a small amount of polyvinylpyrrolidone, stable grinding operation is maintained under the dynamic conditions of the sand mill.

[0009] Furthermore, in the step of adding tetraethyl orthosilicate, the reaction temperature is 35–55°C when the pH is 5.0–6.5, and the amount of tetraethyl orthosilicate added is 2%–6% of the mass of the inorganic pigment powder; the reaction temperature is 45–65°C when the pH is 4.0–5.0, and the amount of tetraethyl orthosilicate added is 5%–15% of the mass of the inorganic pigment powder; the total amount of tetraethyl orthosilicate added is 7%–21% of the mass of the inorganic pigment powder. The mild conditions in the first stage achieve preferential site blocking, and the acid catalysis and sufficient dosage in the second stage ensure that the thickness of the dense shell meets the requirements for effective barrier.

[0010] Furthermore, the reaction temperature for adding aryl-containing and epoxy-containing trialkoxysilanes is 55–75 °C. This temperature ensures complete hydrolysis and grafting of the silanes, while allowing most of the epoxy groups in the epoxy-containing silanes to undergo ring-opening under acid catalysis to form flexible diol segments, leaving only a small amount of residual epoxy for subsequent processing and bonding.

[0011] Furthermore, the volume fraction of ethanol in the water-alcohol mixture is 25%–50%; before filtration, the slurry is diluted to a solid content of 5%–15%, and the ethanol rinsing volume is 300–600 mL per 100 g of inorganic pigment powder; the drying temperature is 50–110℃, and the vacuum degree is -0.06–-0.09 MPa. Dilution increases the particle spacing and reduces the probability of collision; sufficient ethanol rinsing thoroughly removes free silicon-containing species; and low-temperature vacuum drying inhibits the dehydration condensation of residual silanol groups.

[0012] The second aspect of this application provides an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials, which is prepared using the above-described preparation method and comprises inorganic pigment core particles, wherein the inorganic pigment core particles are coated with a silica shell.

[0013] This inorganic pigment employs a multi-layered surface structure design with a core-shell-coupling layer. The silica shell provides a chemical barrier, while the silane coupling layer enables interface adaptation and stress buffering. This allows the pigment to exhibit excellent color stability, dispersion uniformity, and interface compatibility during the high-temperature forming process of TLCP melt-spun fibers, meeting the stringent requirements for pigment dispersion quality in fiber-grade spinning.

[0014] Furthermore, the inorganic pigment is selected from one or more of rutile titanium dioxide, iron oxide red, iron oxide yellow, iron oxide black, copper chromite, cobalt blue spinel, and chromium oxide green. Specifically, copper chromite containing readily soluble transition metal ions (such as copper ions) is particularly suitable.

[0015] Furthermore, the aryl-containing trialkoxysilane is selected from one or more of phenyltrimethoxysilane and phenyltriethoxysilane; the epoxy-containing trialkoxysilane is γ-glycidoxypropyltrimethoxysilane. Specifically, the phenyl group of phenyltrimethoxysilane forms a T-type π-π stack with the aromatic ring of the TLCP fiber matrix, and the ring-opening of γ-glycidoxypropyltrimethoxysilane provides a flexible spacer segment containing an ortho-diol to buffer the thermal stress of fiber stretching.

[0016] Furthermore, the silica shell coating amount is 2.4% to 5.5% of the core particle mass. This coating amount ensures the effectiveness of the ion diffusion barrier while avoiding excessively thick and rigid shells that could lead to cracking under the thermal stress of TLCP melt spinning and fiber stretching.

[0017] This application has the following beneficial effects: The first stage involves depositing a seed layer in a low dissolution pH range to block the channels. The second stage involves growing a dense layer under acidic conditions, which avoids the formation of defects by dissolving metal ions embedded in the silica network, ensuring that the shell is dense and has complete barrier function, thus significantly reducing the color difference of the pigment in TLCP melt-spun fibers.

[0018] Arylsilanes significantly reduce the interfacial tension between pigments and the TLCP aromatic skeleton through π-π stacking, achieving uniform dispersion in the fiber matrix; the diol segments formed by the ring opening of epoxy silanes buffer the thermal expansion mismatch stress during fiber stretching and prevent microcracks in the shell layer; the residual epoxy forms a covalent anchor during spinning to inhibit interfacial debonding in the fiber.

[0019] By diluting and rinsing with sufficient ethanol, free tetraethyl orthosilicate monomers and oligomers in the interparticle gaps are thoroughly removed, eliminating the precursors that form Si-O-Si chemical bridges through drying and dehydration condensation. This significantly reduces the agglomeration index, ensuring submicron-level dispersion of pigments in the fiber matrix and meeting the requirements for melt spinning spinneret passage and uniform fiber coloring.

[0020] The amount of grinding aid PVP is strictly limited to 0.05% to 0.20% to avoid excessive PVP being embedded in the shell to form organic inclusion phases and rapid ion diffusion channels, thereby improving the shell density and thermal stability and preventing pigment discoloration and mechanical property degradation during long-term thermal aging of fibers. Detailed Implementation

[0021] The present application will be further described in detail below with reference to the embodiments and examples. It should be understood that these embodiments and examples are for illustrative purposes only and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to enable a more thorough and comprehensive understanding of the disclosure of the present application. It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various modifications or alterations without departing from the spirit of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. Furthermore, numerous specific details are set forth in the following description to provide a fuller understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.

[0022] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0023] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings: The terms "and / or," "or / and," and "and / or" as used herein include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or," "or / and," and "and / or," it should be understood that in this application, the technical solution undoubtedly includes technical solutions connected by "logical AND," and also undoubtedly includes technical solutions connected by "logical OR." For example, "A and / or B" includes three parallel solutions: A, B, and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, a technical solution that is connected by "logical OR"), as well as any and all combinations of A, B, C, and D, that is, combinations of any two or three of A, B, C, and D, and also combinations of all four of A, B, C, and D (that is, a technical solution that is connected by "logical AND").

[0024] In this application, the terms "multiple", "various", "multiple times", "multi-dimensional", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.

[0025] The terms “combinations of,” “any combination of,” and “any combination of” used in this article include all suitable combinations of any two or more of the listed items.

[0026] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0027] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0028] In this application, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, the selected numerical distributions within the aforementioned numerical intervals are considered continuous and include the two endpoints (i.e., the minimum and maximum values) of the numerical range, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints. In this document, this is equivalent to listing every integer. For example, if t is an integer selected from 1 to 10, it means that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10. Furthermore, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges to which they are included.

[0029] In some preferred embodiments, the inorganic pigment core particles may be selected from any one or more of rutile titanium dioxide, iron oxide red, iron oxide yellow, iron oxide black, copper chromite, cobalt blue spinel, and chromium oxide green.

[0030] In some preferred embodiments, the number average molecular weight of the polyvinylpyrrolidone can be arbitrarily selected between 10,000, 15,000, 20,000, 30,000, 40,000, 50,000, and 60,000; and its dosage can be selected from any one of 0.05%, 0.08%, 0.10%, 0.12%, 0.15%, 0.18%, and 0.20% of the mass of the inorganic pigment powder.

[0031] In some preferred embodiments, the particle size of the zirconia grinding beads used in the wet grinding process can be arbitrarily selected from 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, and 0.8 mm, and the linear velocity can be arbitrarily selected from 8 m / s, 9 m / s, 10 m / s, 11 m / s, and 12 m / s.

[0032] In some preferred embodiments, the volume fraction of ethanol in the water-alcohol mixture can be arbitrarily selected from 25%, 30%, 35%, 40%, 45%, and 50%.

[0033] In some preferred embodiments, the reaction temperature for the first stage shell deposition can be arbitrarily selected between 35°C, 40°C, 45°C, 50°C, and 55°C, and the reaction time can be arbitrarily selected between 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, and 45 min; the amount of tetraethyl orthosilicate added can be selected from any one of 2%, 3%, 4%, 5%, and 6% of the mass of the inorganic pigment powder.

[0034] In some preferred embodiments, the reaction temperature for the second-stage shell deposition can be arbitrarily selected between 45°C, 50°C, 55°C, 60°C, and 65°C, and the reaction time can be arbitrarily selected between 30 min, 45 min, 60 min, 80 min, 100 min, and 120 min; the amount of tetraethyl orthosilicate added can be selected from any one of 5%, 8%, 10%, 12%, and 15% of the mass of the inorganic pigment powder; and the total amount of tetraethyl orthosilicate added can be selected from any one of 8%, 10%, 12%, 14%, 16%, 18%, and 20% of the mass of the inorganic pigment powder.

[0035] In some preferred embodiments, the tetraethyl orthosilicate is added dropwise in the form of an ethanol solution with a volume fraction of 10%, 15%, 20%, or 25%, and the dropping rate can be 0.5 mL / min, 1.0 mL / min, 1.5 mL / min, 2.0 mL / min, 2.5 mL / min, or 3.0 mL / min per 100 g of inorganic pigment powder.

[0036] In some preferred embodiments, the aryl-containing trialkoxysilane is selected from either phenyltrimethoxysilane or phenyltriethoxysilane, and the amount added can be selected from any one of 0.5%, 1.0%, 1.2%, 1.5%, 2.0%, 2.5%, and 3.0% of the inorganic pigment powder by weight; the epoxy-containing trialkoxysilane is γ-glycidyl etheroxypropyltrimethoxysilane, and the amount added can be selected from any one of 0.2%, 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, and 1.5% of the inorganic pigment powder by weight; the mass ratio of the two can be arbitrarily selected between 1.5:1, 2:1, 2.5:1, 3:1, 4:1, and 5:1.

[0037] In some preferred embodiments, the temperature of the bissilane coupling modification can be arbitrarily selected between 55°C, 60°C, 65°C, 70°C, and 75°C, and the reaction time can be arbitrarily selected between 30 min, 45 min, 60 min, 80 min, 100 min, and 120 min.

[0038] In some preferred embodiments, the solid content of the slurry diluted before filtration can be arbitrarily selected from 5%, 8%, 10%, 12%, and 15%; the ethanol rinsing volume can be 300mL, 350mL, 400mL, 450mL, 500mL, 550mL, and 600mL per 100g of inorganic pigment raw powder.

[0039] In some preferred embodiments, the drying temperature can be arbitrarily selected between 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, and 110°C; the vacuum degree can be arbitrarily selected between -0.06MPa, -0.07MPa, -0.08MPa, and -0.09MPa; and the drying time can be arbitrarily selected between 3h, 5h, 8h, 10h, 12h, and 16h.

[0040] Example 1

[0041] This embodiment provides an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and its preparation method.

[0042] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 705 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g (4.0 g in the first stage, 10.0 g in the second stage); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.2 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.6 g.

[0043] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0044] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0045] (3) First-stage shell deposition: Dissolve 4.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Activate the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0046] (4) Second-stage shell deposition: Dissolve 10.0 g TEOS in 60 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 60 min.

[0047] (5) Bissilane coupling modification: 1.2 g PhTMS and 0.6 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued for 60 min at 65℃, pH 3.5, and 400 rpm.

[0048] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0049] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0050] Example 2

[0051] This embodiment provides an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and its preparation method.

[0052] Difference from Example 1: The inorganic pigment powder in this example is iron oxide red, the pH is adjusted to 6.5 during the grinding stage, and the grinding time is 2 hours.

[0053] Raw materials for preparation: Iron oxide red pigment (industrial grade, initial D50 2-4μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 705 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g (4.0 g in the first stage, 10.0 g in the second stage); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.2 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.6 g.

[0054] Preparation method: (1) Wet grinding: Add 100 g of iron oxide red pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.5±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2 h until the volumetric median particle size D50 = 0.4-0.6 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0055] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0056] (3) First-stage shell deposition: Dissolve 4.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Activate the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0057] (4) Second-stage shell deposition: Dissolve 10.0 g TEOS in 60 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 60 min.

[0058] (5) Bissilane coupling modification: 1.2 g PhTMS and 0.6 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued for 60 min at 65℃, pH 3.5, and 400 rpm.

[0059] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0060] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0061] Example 3

[0062] This embodiment provides an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and its preparation method.

[0063] Difference from Example 1: This example increases the amount of silica shell coating and the amount of silane coupling agent.

[0064] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 830 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 20.0 g (6.0 g in the first stage, 14.0 g in the second stage); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.5 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.8 g.

[0065] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0066] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0067] (3) First-stage shell deposition: Dissolve 6.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Activate the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry at a uniform rate over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0068] (4) Second-stage shell deposition: Dissolve 14.0 g TEOS in 85 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 80 min.

[0069] (5) Bissilane coupling modification: 1.5 g PhTMS and 0.8 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued to be stirred for 70 min at 65℃, pH 3.5, and 400 rpm.

[0070] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 5 portions of anhydrous ethanol (100 mL each, totaling 500 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After five rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0071] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0072] Example 4

[0073] This embodiment provides an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and its preparation method.

[0074] Difference from Example 1: This example adjusts the ratio of bissilanes and increases the proportion of phenylsilanes.

[0075] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 705 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g (4.0 g in the first stage, 10.0 g in the second stage); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.5 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.3 g.

[0076] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0077] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0078] (3) First-stage shell deposition: Dissolve 4.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Activate the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0079] (4) Second-stage shell deposition: Dissolve 10.0 g TEOS in 60 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 60 min.

[0080] (5) Bissilane coupling modification: 1.5 g PhTMS and 0.3 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued for 60 min at 65℃, pH 3.5, and 400 rpm.

[0081] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0082] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0083] Example 5

[0084] This embodiment provides an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and its preparation method.

[0085] Difference from Example 1: The inorganic pigment powder in this example is titanium dioxide, the grinding time is shortened, and the total amount of TEOS and the amount of silane are adjusted accordingly.

[0086] Raw materials for preparation: Rutile titanium dioxide (industrial grade, initial D50 0.3~0.5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 690 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 10.0 g (3.0 g for stage 1, 7.0 g for stage 2); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.0 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.5 g.

[0087] Preparation method: (1) Wet grinding: Add 100 g of titanium dioxide raw powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 1 h until the median particle size D50 = 0.2-0.3 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0088] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0089] (3) First-stage shell deposition: Dissolve 3.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Turn on the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry at a uniform rate over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0090] (4) Second-stage shell deposition: Dissolve 7.0 g TEOS in 45 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 60 min.

[0091] (5) Bissilane coupling modification: 1.0 g PhTMS and 0.5 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued for 60 min at 65℃, pH 3.5, and 400 rpm.

[0092] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0093] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0094] Example 6

[0095] This embodiment provides an inorganic pigment for coloring thermotropic liquid crystal polyester raw materials and its preparation method.

[0096] Difference from Example 1: This example adjusts the temperature and time of each stage of the reaction.

[0097] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 705 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g (4.0 g in the first stage, 10.0 g in the second stage); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.2 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.6 g.

[0098] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0099] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0100] (3) First-stage shell deposition: Dissolve 4.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Start the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 50±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry at a uniform rate over 20 min using the dropping funnel. After the addition is complete, continue stirring for 20 min at 50℃, pH 5.8, and 400 rpm.

[0101] (4) Second-stage shell deposition: Dissolve 10.0 g TEOS in 60 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 60±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 60℃, pH 4.0, and 400 rpm for 45 min.

[0102] (5) Bissilane coupling modification: 1.2 g PhTMS and 0.6 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 70±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued to be stirred for 50 min at 70℃, pH 3.5, and 400 rpm.

[0103] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0104] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0105] Comparative Example 1 This comparative example provides a method for preparing inorganic pigments.

[0106] The difference from Example 1 is that the silica shell deposition process was omitted in this comparative example, and the silane coupling modification was carried out directly in the water-alcohol medium.

[0107] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 615 mL in total; Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.2 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.6 g.

[0108] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0109] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0110] (3) Silane coupling modification: The pH of the system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. 1.2 g PhTMS and 0.6 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and added to the reaction system over 5 min. The reaction was stirred continuously for 60 min at 65℃, pH 3.5, and 400 rpm.

[0111] (4) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0112] (5) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0113] Comparative Example 2 This comparative example provides a method for preparing inorganic pigments.

[0114] Difference from Example 1: This comparative example uses a one-step method to deposit a silica shell and does not perform staged pH control.

[0115] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 705 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g; Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.2 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.6 g.

[0116] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0117] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0118] (3) One-step shell deposition: The pH of the system was directly adjusted to 4.0±0.2 using glacial acetic acid, and the temperature was raised to 55±2℃. 14.0 g of TEOS was dissolved in 90 mL of anhydrous ethanol and added dropwise to the reaction system at a uniform rate over 60 min. After the addition was complete, the reaction was stirred for another 90 min at 55℃, pH 4.0, and 400 rpm.

[0119] (4) Bissilane coupling modification: 1.2 g PhTMS and 0.6 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued for 60 min at 65℃, pH 3.5, and 400 rpm.

[0120] (5) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0121] (6) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0122] Comparative Example 3 This comparative example provides a method for preparing inorganic pigments.

[0123] Difference from Example 1: In this comparative example, deionized water was used instead of ethanol for rinsing in the rinsing step.

[0124] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 700 g in total (including grinding and rinsing); Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 305 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g (4.0 g in the first stage, 10.0 g in the second stage); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.2 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.6 g.

[0125] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0126] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0127] (3) First-stage shell deposition: Dissolve 4.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Activate the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0128] (4) Second-stage shell deposition: Dissolve 10.0 g TEOS in 60 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 60 min.

[0129] (5) Bissilane coupling modification: 1.2 g PhTMS and 0.6 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued for 60 min at 65℃, pH 3.5, and 400 rpm.

[0130] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature while stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of deionized water (100 mL each, totaling 400 mL). Each time, pour the deionized water evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drips.

[0131] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0132] Comparative Example 4 This comparative example provides a method for preparing inorganic pigments.

[0133] Difference from Example 1: This comparative example does not add aryl-containing PhTMS, but only uses KH-560 containing epoxy groups for coupling modification, while keeping the total amount of silane the same.

[0134] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.12 g; Anhydrous ethanol (analytical grade, ≥99.5%): 705 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g (4.0 g in the first stage, 10.0 g in the second stage); γ-glycidoxypropyltrimethoxysilane (KH-560, purity ≥97%): 1.8 g.

[0135] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.12 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0136] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0137] (3) First-stage shell deposition: Dissolve 4.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Activate the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0138] (4) Second-stage shell deposition: Dissolve 10.0 g TEOS in 60 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 60 min.

[0139] (5) Monosilane coupling modification: Dissolve 1.8 g KH-560 in 15 mL anhydrous ethanol and mix thoroughly. Adjust the pH of the reaction system to 3.5±0.2 with glacial acetic acid and adjust the temperature to 65±2℃. Add the silane-ethanol solution to the reaction system over 5 min while stirring at 400 rpm. Continue stirring the reaction at 65℃, pH 3.5, and 400 rpm for 60 min.

[0140] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0141] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0142] Comparative Example 5 This comparative example provides a method for preparing inorganic pigments.

[0143] The difference from Example 1: In this comparative example, the amount of PVP K30 was increased to 0.60 g in the wet milling stage.

[0144] Raw materials for preparation: Copper chromite pigment (copper chromite, industrial grade, initial D50 3~5μm): 100 g; Deionized water (conductivity ≤5μS / cm): 300 g; Polyvinylpyrrolidone (PVP K30, number average molecular weight 40,000): 0.60 g; Anhydrous ethanol (analytical grade, ≥99.5%): 705 mL in total; Tetraethyl orthosilicate (TEOS, analytical grade, silica content ≥28.4%): 14.0 g (4.0 g in the first stage, 10.0 g in the second stage); Phenylacetyltrimethoxysilane (PhTMS, purity ≥97%): 1.2 g; γ-glycidyl etheroxypropyltrimethoxysilane (KH-560, purity ≥97%): 0.6 g.

[0145] Preparation method: (1) Wet grinding: Add 100 g of copper chromite pigment powder and 0.60 g of PVP K30 to 300 g of deionized water and stir for pre-dispersion for 10 min. Adjust the pH of the slurry to 6.0±0.2 with 5 wt% dilute ammonia. Load the slurry into the grinding cylinder of a horizontal sand mill, add 0.3-0.5 mm zirconia grinding beads (70% filling rate), set the axis speed of the sand mill to 10 m / s, and start the circulation pump for circulating grinding. Grind continuously for 2.5 h until the volumetric median particle size D50 = 0.3-0.5 μm and D90 < 1.0 μm. Separate the grinding beads through an 80-mesh sieve and collect the pigment grinding slurry.

[0146] (2) Medium preparation: Transfer the pigment grinding slurry to a 2 L four-necked double-walled glass reactor. Purge with nitrogen (flow rate 200 mL / min) for 10 min to remove air from the reactor. Slowly add 200 mL of anhydrous ethanol while stirring at 300 rpm, and stir for 10 min to mix thoroughly to obtain a water-ethanol mixture slurry. Maintain the nitrogen protective atmosphere until the entire reaction is complete.

[0147] (3) First-stage shell deposition: Dissolve 4.0 g TEOS in 30 mL of anhydrous ethanol and place the solution in a constant-pressure dropping funnel. Activate the constant-temperature circulation in the reactor jacket to raise the slurry temperature to 45±2℃. Adjust the pH to 5.8±0.2 using 5 wt% dilute ammonia. At a stirring speed of 400 rpm, add the TEOS-ethanol solution dropwise into the slurry over 20 min using the dropping funnel. After the addition is complete, continue stirring at 45℃, pH 5.8, and 400 rpm for 25 min.

[0148] (4) Second-stage shell deposition: Dissolve 10.0 g TEOS in 60 mL of anhydrous ethanol and place the solution in another constant-pressure dropping funnel. Adjust the pH of the system to 4.0±0.2 with glacial acetic acid, and simultaneously raise the temperature to 55±2℃. Add the TEOS-ethanol solution dropwise to the reaction system at a constant rate of 400 rpm over 40 min. After the addition is complete, continue stirring at 55℃, pH 4.0, and 400 rpm for 60 min.

[0149] (5) Bissilane coupling modification: 1.2 g PhTMS and 0.6 g KH-560 were dissolved together in 15 mL of anhydrous ethanol and mixed thoroughly. The pH of the reaction system was adjusted to 3.5±0.2 with glacial acetic acid, and the temperature was adjusted to 65±2℃. The silane-ethanol solution was added to the reaction system over 5 min while stirring at 400 rpm. The reaction was continued for 60 min at 65℃, pH 3.5, and 400 rpm.

[0150] (6) Dilution and rinsing: After the reaction is complete, stop heating and allow the mixture to cool naturally to room temperature with stirring. Add an appropriate amount of deionized water to dilute the slurry to a solid content of 10% and stir for 5 minutes. Transfer the diluted slurry to a Buchner funnel and perform vacuum filtration. After the filter cake has initially formed, rinse the filter cake sequentially with 4 portions of anhydrous ethanol (100 mL each, totaling 400 mL). Each time, pour the ethanol evenly onto the surface of the filter cake and allow it to penetrate naturally before starting vacuum suction. After four rinses, continue vacuum suction for 5 minutes until there are no obvious drops.

[0151] (7) Drying and De-agglomeration: Transfer the washed filter cake to a stainless steel tray in a vacuum drying oven and spread it evenly to a thickness not exceeding 10 mm. Set the drying temperature to 80℃ and the vacuum degree to -0.08 MPa, and dry for 8 h. The dried powder is then de-agglomerated using an air jet mill with the following airflow parameters: inlet pressure 0.6 MPa and classifier speed 6000 rpm. Collect the de-agglomerated product powder and seal it in packaging.

[0152] The materials prepared in the above embodiments and comparative examples were tested according to the following methods.

[0153] Particle size distribution was determined using a laser diffractometer, following GB / T 19077-2016 "Particle Size Analysis - Laser Diffraction Method". A suitable amount of pigment sample was added to deionized water to prepare a suspension. After ultrasonic dispersion for 5 min, the volumetric particle size distribution was measured, and the median particle size (D50 and D90) was recorded. Agglomeration index = D50 - product / D50 - grinding; where D50 - grinding is the D50 value of the wet-milled product, and D50 - product is the D50 value of the final product after drying and deagglomeration.

[0154] X-ray fluorescence spectrometry (XRF) was used: Following GB / T 16597-1996, the pigment sample was pressed into thin slices to determine the Si element content. The Si content was calculated using the formula: Si% = Si% × 60.08 / 28.09. An untreated pigment powder was used as a blank control; the difference was the amount of coated silica.

[0155] The determination was performed according to HG / T 3851-2006. Pigment samples were wet-ground and pressed with barium sulfate to prepare contrasting photographs; another batch of pigment was placed in a muffle furnace at 310℃ for 30 min and then cooled, and used to prepare test pieces with barium sulfate. The L*, a*, and b values ​​were measured using a spectrophotometer, and the total color difference ΔE was calculated according to the CIELAB color difference formula.

[0156] Preparation of TLCP-colored fiber samples: Modified pigment was dry-mixed with TLCP chips at a mass fraction of 2%, and then co-extruded and granulated using a twin-screw extruder to prepare a coloring masterbatch. The coloring masterbatch was mixed with pure TLCP chips in a certain proportion (final pigment content 2wt%), and after vacuum drying (140℃×6 h), it was fed into a single-screw melt spinning machine. Spinning process parameters: screw zone temperature 280–340℃, spinneret orifice diameter 0.3 mm, number of orifices 24, length-to-diameter ratio 2:1, spinning speed 500 m / min. The nascent fibers underwent two-stage hot drawing (first-stage drawing temperature 250–270℃, second-stage drawing temperature 270–290℃, total draw ratio 3–6 times), and after heat setting, the colored fibers were wound and collected. Simultaneously, pure TLCP blank control fibers were prepared using the same process.

[0157] The fiber breaking strength was tested using a single-fiber tensile strength tester according to GB / T 14344-2022. Test conditions: clamping length 20 mm, tensile speed 20 mm / min, 20 filaments were tested per sample and the average value was taken. Breaking strength retention rate = (breaking strength of dyed TLCP fiber / breaking strength of pure TLCP control fiber) × 100%.

[0158] The surface of the colored fibers and the cross-section after liquid nitrogen quenching were observed using scanning electron microscopy (SEM). Ten fields of view (magnification × 2000) were randomly selected along the fiber axis, and the number of pigment aggregates with a diameter > 3 μm was counted. Level 1: 0 aggregates / field; Level 2: 1–2 aggregates / field; Level 3: 3–5 aggregates / field; Level 4: > 5 aggregates / field. The number of spinning breaks per 1000 m of fiber was also recorded.

[0159] The colored fiber bundle sample was placed in a 310℃ hot air circulating oven and cooled at 0.5 h, 1 h, 2 h and 4 h respectively. The color difference ΔE* between the sample at each time point and the sample at 0 h was measured.

[0160] For copper-containing pigments, 1 g of dried pigment powder was weighed and placed in a 250 mL Erlenmeyer flask. 100.0 mL of a pH 4.0 acetate-sodium acetate buffer solution (0.1 mol / L) was added. The flask was sealed and placed in a constant-temperature shaker at 80°C and 150 r / min for 2 h of extraction. After extraction, the flask was cooled to room temperature and centrifuged at 10,000 r / min for 15 min. The supernatant was filtered through a 0.22 μm microporous membrane, and the Cu concentration in the filtrate was determined by inductively coupled plasma optical emission spectrometry (ICP-OES). Each sample was measured in triplicate, and the average value was taken. The amount of copper ions dissolved was expressed as the Cu concentration in the filtrate (ppm, i.e., mg / L).

[0161] Table 1. Comparative test results of pigment powder properties in the examples and comparative examples.

[0162] Table 2 Comparison of TLCP fiber sample performance (pigment addition amount 2 wt%)

[0163] Comparing the test data of Example 1 and Comparative Example 1, it can be seen that Comparative Example 1 did not undergo silica shell deposition. The copper ions in the pigment core were directly exposed to the melt during the high-temperature processing of TLCP, catalyzing the transesterification and thermo-oxidative degradation of the polyester chain, and simultaneously worsening the fiber spinnability. After heat treatment at 310℃ for 30 min, the color difference ΔE of its powder reached as high as 3.54, far exceeding the acceptable limit of 2.0; the breaking strength retention rate of the colored TLCP fiber was only 71.5%, and the dispersibility rating dropped to level 3. In contrast, Example 1, by depositing a silica shell with sufficient coating, significantly reduced the amount of copper ion leaching from 63 ppm in Comparative Example 2 to 13 ppm, effectively inhibiting the diffusion of metal ions into the matrix. This resulted in a heat-treated color difference of 1.27, fundamentally improving both mechanical properties and dispersibility, with a color difference ΔE of only 2.53 after 4 hours of long-term aging.

[0164] Comparing Example 1 and Comparative Example 2, both used the same total TEOS amount, but Comparative Example 2 employed a one-step acidic deposition method. Under pH 4.0 conditions, a large amount of copper ions dissolved from the pigment surface, reaching 63 ppm. These dissolved metal ions competitively coordinated with silanol groups, embedding into the silica network to form Cu-O-Si hybrid defects, disrupting the continuity and density of the shell. This defective shell could not provide a complete ion diffusion barrier, leading to a deterioration in its heat-treated color difference ΔE to 2.21, and a 4-hour long-term color difference ΔE of TLCP-colored fibers reaching as high as 5.47, with a degradation rate far faster than in Example 1. Example 1 first formed a seed layer under weak acidity to block the dissolution channels, and then rapidly grew a dense layer under acidity, suppressing dissolution interference at its source and ensuring shell quality.

[0165] Comparing Example 1 and Comparative Example 3, the shell deposition quality of both is comparable (copper ion leaching amounts are 13 ppm and 14 ppm, respectively). However, Comparative Example 3 used deionized water rinsing. Due to the large absolute amount of residual free TEOS monomers and oligomers in the system, deionized water has extremely poor solubility for these hydrophobic silicon-containing species. The residual precursors undergo dehydration condensation during the drying stage, forming Si-O-Si chemical bridges between particles. The aggregation index of Comparative Example 3 increased sharply to 3.30, and the D50-product deteriorated to 1.32 μm, failing to disperse uniformly in the TLCP fiber matrix, exhibiting a dispersibility level of 4 and a significant decrease in mechanical properties (breaking strength retention rate of 78.3%). The ethanol rinsing strategy of Example 1 effectively removed the free precursors, controlling the aggregation index at an excellent level of 1.21.

[0166] Comparing Example 1 and Comparative Example 4, it can be seen that Comparative Example 4 only uses aliphatic epoxy silanes and lacks phenyl groups that specifically interact with the TLCP aromatic skeleton. Due to the limited reduction in interfacial tension between the aliphatic ether segments and the highly aromatic skeleton, the pigment dispersion in the melt is only grade 2, and the interfacial adhesion is weaker than in Example 1. Weak interfacial bonding makes it more prone to debonding during long-term thermal aging, exposing the pigment surface in the fiber and accelerating ion diffusion. This results in a 4-hour long-term color difference ΔE* of 4.23 in Comparative Example 4, significantly faster than the degradation in Example 1 (2.53). The phenyl groups in Example 1 achieve substantial improvement in the interface through π-π stacking.

[0167] Comparing Example 1 and Comparative Example 5, it can be seen that Comparative Example 5 used an excessive amount of PVP (0.6%), with a large amount of PVP embedded in the silica shell to form an organic inclusion phase. The organic inclusions reduced the shell density, providing a rapid channel for ion diffusion, resulting in a slight increase in the copper ion dissolution rate of Comparative Example 5 to 18 ppm and an increase in the heat treatment color difference ΔE to 1.87. Simultaneously, the changes in the organic inclusions at high temperatures also accelerated the degradation of long-term thermal aging performance, with a 4-hour color difference ΔE as high as 4.52, far inferior to Example 1.

[0168] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0169] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A method for preparing an inorganic pigment for coloring thermotropic liquid crystal polyester dopes, characterized in that, Includes the following steps: The inorganic pigment powder, polyvinylpyrrolidone, and deionized water are wet-milled until the median particle size (D50) is 0.2–1.5 μm. The amount of polyvinylpyrrolidone used is 0.05%–0.20% of the mass of the inorganic pigment powder. Ethanol was added to the slurry obtained from grinding under an inert atmosphere to obtain a water-alcohol mixed slurry. The pH of the water-alcohol mixed slurry was adjusted to 5.0-6.5, and tetraethyl orthosilicate was added to react. The pH of the system was then adjusted to 4.0-5.0, and tetraethyl orthosilicate was added to react. The pH of the system was then adjusted to 3.0-4.0, and aryl-containing trialkoxysilane and epoxy-containing trialkoxysilane were added to react. The mass ratio of the aryl-containing trialkoxysilane to the epoxy-containing trialkoxysilane was (1.5-5):

1. The resulting slurry was filtered, and the filter cake was washed with ethanol. The washed filter cake is dried and deagglomerated to obtain the inorganic pigment.

2. The preparation method according to claim 1, characterized in that, The pH of the slurry is adjusted to 5.0–7.0 during grinding; the wet grinding uses 0.2–0.8 mm zirconia grinding beads.

3. The preparation method according to claim 1, characterized in that, In the step of adding tetraethyl orthosilicate, the reaction temperature is 35-55℃ when the pH is 5.0-6.5, and the amount of tetraethyl orthosilicate added is 2%-6% of the mass of the inorganic pigment powder; the reaction temperature is 45-65℃ when the pH is 4.0-5.0, and the amount of tetraethyl orthosilicate added is 5%-15% of the mass of the inorganic pigment powder; the total amount of tetraethyl orthosilicate added is 7%-21% of the mass of the inorganic pigment powder.

4. The preparation method according to claim 1, characterized in that, The reaction temperature for adding aryl-containing and epoxy-containing trialkoxysilanes is 55–75 °C.

5. The preparation method according to claim 1, characterized in that, The volume fraction of ethanol in the water-alcohol mixture is 25%–50%; the slurry is diluted to a solid content of 5%–15% before filtration, and the ethanol rinsing volume is 300–600 mL per 100 g of inorganic pigment powder; the drying temperature is 50–110℃, and the vacuum degree is -0.06–-0.09 MPa.

6. An inorganic pigment for coloring thermotropic liquid crystal polyester dopes, characterized in that, Prepared using the preparation method according to any one of claims 1-5, comprising inorganic pigment core particles, wherein the inorganic pigment core particles are coated with a silica shell.

7. The inorganic pigment according to claim 6, characterized in that, The inorganic pigment core particles are selected from one or more of rutile titanium dioxide, iron oxide red, iron oxide yellow, iron oxide black, copper chromite, cobalt blue spinel, and chromium oxide green.

8. The inorganic pigment according to claim 6, characterized in that, The aryl-containing trialkoxysilane is selected from one or more of phenyltrimethoxysilane and phenyltriethoxysilane; the epoxy-containing trialkoxysilane is γ-glycidoxypropyltrimethoxysilane.

9. The inorganic pigment according to claim 6, characterized in that, The coating amount of the silica shell is 2.4% to 5.5% of the mass of the inorganic pigment core particles.

10. The application of an inorganic pigment as described in any one of claims 6-9 in the coloring of thermotropic liquid crystal polyester raw materials.