An in-situ pre-ceramic steel heat treatment anti-oxidation coating, its preparation method and application method
By using a two-component in-situ pre-ceramic coating to perform a pre-ceramic reaction in the medium-temperature range, the problems of existing coatings being easily broken at low temperatures, lacking protection at medium temperatures, and exhibiting lag at high temperatures are solved, thus achieving full-process protection against oxidation and decarburization during the heat treatment of steel.
Patent Information
- Application Number
- CN202611357296.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing heat treatment protective coatings are easily damaged at low temperatures, offer no protection at medium temperatures, and have delayed ceramic formation at high temperatures. They cannot be matched with conventional segmented gradient heating heat treatment processes, resulting in defects such as increased oxidation thickness, weight loss, and surface decarburization on the steel surface.
The in-situ pre-formed ceramic coating, which uses two components for isolated storage, completes the pre-formation of ceramics in advance within the temperature-sensitive range of heat treatment. It utilizes the microcapsules to break the cell walls at 520~580℃ to initiate a mild exothermic oxidation reaction between elemental silicon powder and potassium nitrate, forming a continuous and dense protective film layer that is compatible with various gradient heating processes.
It achieves continuous and dense protection throughout the entire process from low temperature to high temperature, significantly reducing steel oxidation and decarburization, and improving the surface quality and yield of heat treatment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of heat treatment protection technology for metallic materials, and more particularly to an in-situ pre-ceramic steel heat treatment anti-oxidation coating, its preparation method, and its application method. Background Technology
[0002] The industrial heat treatment process for steel can generally be divided into a low-temperature dehydration and heat preservation stage, a medium-temperature stress relief and heat preservation stage, and a high-temperature austenitizing heat treatment stage. The conventional heating rate is controlled at 5~15℃ / min, and the process sequentially goes through a low-temperature dehydration stage from room temperature to 300℃, a medium-temperature transition heat preservation stage from 300~700℃, and a high-temperature long-term heat preservation stage from 850~1180℃.
[0003] During heat treatment, steel is exposed to an oxidizing atmosphere for extended periods, making it highly susceptible to defects such as surface oxidation thickening, weight loss, surface decarburization, and grain boundary oxidation. Existing protective coatings cannot provide continuous protection throughout the entire process. For example, patent CN112940544A discloses a high-temperature anti-oxidation coating for steel billets that uses a traditional aluminosilicate system, relying entirely on high-temperature, long-term sintering, resulting in high ceramicization temperatures and significant molding delays. In the low-temperature range of room temperature to 300℃, the free and bound water within the system vaporizes rapidly, resulting in a coating with no pre-cured strength, making it prone to blistering, peeling, and microcracks. In the medium-temperature sensitive range of 300~700℃, the system cannot form a dense structure, and the film remains loose and porous. Industrial heat treatment in this temperature range typically involves prolonged heat preservation, allowing oxygen and water vapor to continuously penetrate the substrate, causing severe oxidation and decarburization of the steel. Only when the temperature reaches above 850℃ does the coating begin to slowly sinter into ceramic, making the previously caused substrate damage irreparable. This ultimately leads to poor surface quality, high burn-off rate, and high scrap rate in the heat-treated steel. Patent CN103203938A discloses a self-heating coating for substrate surfaces and its preparation method, using an iron powder-activated carbon electrochemical corrosion reaction system to achieve exothermic reaction. However, its design and performance are completely unsuitable for the high-temperature heat treatment conditions of steel. This system relies on organic binders to encapsulate the active components. The film-forming substances have poor temperature resistance and will decompose and fail rapidly under high-temperature heat treatment conditions, causing the coating to lose protection for the active components. At the same time, its exothermic reaction has no temperature-controlled triggering mechanism. The active components will start to react when they come into contact with water or oxygen. The coating system is prone to premature reaction and clumping during storage. The heat generation process after coating is uncontrolled and cannot meet the stringent requirements of industrial heat treatment for process stability.
[0004] In addition, conventional air-drying protective coatings on the market rely solely on the physical film formation through water evaporation. The film has high porosity and poor thermal shock stability, making it prone to cracking and peeling during furnace heating, resulting in extremely low protective reliability.
[0005] In summary, existing heat treatment protective coatings generally suffer from structural defects such as easy breakage at low temperatures, lack of protection at medium temperatures, and delayed ceramization at high temperatures. They are unable to match conventional segmented gradient heating heat treatment processes, resulting in a persistent gap in medium-temperature protection. This is the core reason why the oxidation and decarburization defects in steel heat treatment cannot be eradicated. The industry urgently needs a comprehensive protective coating that can actively pre-ceramize within the sensitive medium-temperature range, is stable during storage and transportation, and has strong process adaptability. Summary of the Invention
[0006] To address the shortcomings of existing silicate protective coatings, such as low-temperature blistering and cracking, mid-temperature porosity and lack of protection, and delayed high-temperature ceramicization, as well as the poor high-temperature resistance and uncontrollable heat release of traditional self-exothermic coatings, this invention provides an in-situ pre-cemented steel heat treatment anti-oxidation coating, along with its preparation and application methods. This invention utilizes commercially available general-purpose raw materials, two-component isolated storage, and a furnace-triggered temperature-controlled thermal mechanism to complete pre-cementation in the temperature-sensitive range of heat treatment, completely filling the gap in mid-temperature protection. It achieves continuous and dense protection throughout the entire process from low to high temperatures, and is compatible with various conventional gradient-heating heat treatment processes.
[0007] To achieve the above objectives, the technical solution of the present invention is as follows: The first aspect of the present invention provides an in-situ pre-ceramic steel heat treatment anti-oxidation coating, the coating being composed of component A and component B, wherein the mass ratio of component A to component B is 100:(4~7). The A component is composed of the following raw materials by mass fraction: 42%~48% fused silica powder, 7%~9% α-alumina micro powder, 25%~29% potassium silicate water glass, 4%~6% anhydrous potassium metaborate, 2%~3% aluminum dihydrogen phosphate aqueous solution, 1.0%~1.8% lithium-based bentonite, and the balance being deionized water. Component B is a microcapsule powder, wherein the core material is composed of the following raw materials by mass fraction: 35%~45% elemental silica powder, 55%~65% potassium nitrate powder, and the capsule wall includes EVA resin and liquid paraffin accounting for 3%~8% of the capsule wall mass.
[0008] In the above technical solution, the particle size of the fused silica powder is further 800~1000 mesh; The particle size of the α-alumina micro powder is 600~800 mesh; The potassium silicate water glass has a solid content of 37% to 42% and a modulus of 2.9 to 3.1. The solid content of the aluminum dihydrogen phosphate aqueous solution is 38%~53%; The lithium-based bentonite has a particle size of 400-500 mesh.
[0009] In the above technical solution, the particle size of the elemental silicon powder is further specified as 600-800 mesh, industrial grade; The potassium nitrate powder has a particle size of 800-1000 mesh and is of industrial grade.
[0010] In the above technical solution, the EVA resin has a Vicat softening point of 85~95℃ and a vinyl acetate content of 18%~22% by mass. The melting temperature of the capsule wall is 520~580 ℃.
[0011] A second aspect of the present invention provides a method for preparing the above-mentioned in-situ pre-ceramic steel heat treatment anti-oxidation coating, comprising the following steps: I. Preparation of Component A: (1) Add lithium-based bentonite to deionized water and keep the temperature constant at 25~30℃. First, stir at 60~80 r / min for 35~45 min to complete the initial water absorption and swelling. Then, increase the speed to 280~300 r / min and stir for 15~25 min to carry out interlayer peeling and activation. Let it stand for 10~14 h to eliminate the hidden danger of slurry stratification in the later stage and obtain the pregel mother liquor. (2) Add aluminum dihydrogen phosphate aqueous solution to the pregel mother liquor obtained in step (1) under uniform stirring at 100~140 r / min for 25~30 min, and then add potassium silicate water glass at a uniform speed. After the addition is completed, stir at a constant temperature for 35~45 min to achieve molecular-level complexation of the two inorganic binders, avoid local gelation and agglomeration, and obtain composite binder. (3) Premix the fused silica powder and α-alumina micro powder evenly, and add them in equal amounts in three batches to the composite binder obtained in step (2). After each batch is added, stir at 350~450 r / min for 10~20 min. After all the materials are added, increase the stirring speed to 1200~1500 r / min and stir for 55~65 min. Finally, add anhydrous potassium metaborate and continue stirring at 1200~1500 r / min for 25~35 min to dissolve and disperse evenly. (4) Filtration to remove aggregated particles and mechanical impurities, and collection of filtrate; II. Preparation of Component B 1) Mix elemental silicon powder and potassium nitrate powder under a nitrogen atmosphere for 85-95 minutes, keeping the air and moisture out of the air throughout the process to prevent silicon powder from oxidizing and potassium nitrate from absorbing moisture and clumping, thus ensuring microscopic mixing uniformity. 2) Melt EVA resin in a reactor at a constant temperature of 115~120℃, add liquid paraffin as a coating rheology modifier, stir for 20~30min to obtain EVA molten coating liquid, and keep it at a controlled temperature for later use; 3) The mixed powder obtained in step 1) is fed into a fluidized bed coating machine. The bed is preheated to 480℃ for preheating and drying to remove water. EVA molten coating liquid is sprayed from top to bottom at a uniform speed using pressure atomization. The atomization pressure is controlled at 0.25~0.3 MPa. The coating is applied in 4 layers intermittently. After each layer is sprayed, it is kept warm and cured for 6~10 minutes to achieve a uniform, dense film without pinholes. The fluidized bed temperature is controlled at 480~500℃ throughout the process to avoid premature melting and cell wall breakage. 4) After granulation, cool to room temperature, sieve, transfer to vacuum aluminum foil packaging, fill with nitrogen, seal and store in the dark.
[0012] In the above technical solution, further, in step (4), the filtration step is: a two-stage filtration is adopted, the first stage is a 70~100 mesh pre-filtration, and the second stage is a 250~350 mesh fine filtration.
[0013] In the above technical solution, further, in step 4), the screening step is: sequentially passing through two levels of vibrating sieves of 50~70 mesh and 100~140 mesh.
[0014] The third aspect of the present invention provides a method for applying the above-mentioned in-situ pre-ceramic steel heat treatment anti-oxidation coating, wherein component A and component B are mixed evenly, sprayed onto the surface of the steel workpiece at room temperature, and after natural surface drying, the coating is placed in a heat treatment furnace along with the steel workpiece for heat treatment.
[0015] When the coating provided by this invention is applied, the microcapsule cell wall is broken when the temperature of the heat treatment furnace rises to the range of 520~580 ℃. The elemental silicon powder and potassium nitrate undergo a mild self-sustaining exothermic oxidation reaction, which drives the silicon-boron inorganic system to complete the pre-ceramic formation in situ. The rigid skeleton of the pre-ceramic is further densified and sintered in the subsequent high-temperature heat treatment range to form a continuous and complete protective film layer, thereby achieving anti-oxidation and anti-decarburization protection for steel throughout the entire heat treatment process.
[0016] The beneficial effects of this invention are as follows: This invention adopts a dual-component independent sealing structure, which provides excellent stability for dry powder storage. When the workpiece is heated to 520~580℃ in the furnace, the thermosensitive microcapsules break down, and the elemental silicon powder and potassium nitrate undergo a mild, self-sustaining exothermic oxidation reaction, driving the silicon-boron inorganic system to complete the pre-ceramic formation in situ. The rigid skeleton of the pre-ceramic is further densified and sintered in the subsequent high-temperature heat treatment zone to form a continuous and complete protective film layer, thereby achieving anti-oxidation and anti-decarburization protection for steel throughout the entire heat treatment process.
[0017] The raw materials used in this invention are readily available in the industry and are inexpensive; the process employs a room-temperature spraying process, requiring only natural surface drying, making the process simple and convenient to operate. Detailed Implementation
[0018] The following examples are intended to enable those skilled in the art to more fully understand the present invention, but do not limit the invention in any way.
[0019] The first aspect of this invention provides an in-situ pre-ceramic steel heat treatment anti-oxidation coating, which is composed of component A and component B, with a mass ratio of component A to component B of 100:(4~7). Component A consists of the following raw materials by mass fraction: 42%–48% fused silica powder, 7%–9% α-alumina micro powder, 25%–29% potassium silicate water glass, 4%–6% anhydrous potassium metaborate, 2%–3% aluminum dihydrogen phosphate aqueous solution, 1.0%–1.8% lithium-based bentonite, and the balance being deionized water; Specific requirements for the raw materials include: The particle size of the fused silica powder is 800~1000 mesh; The particle size of α-alumina micro powder is 600~800 mesh; The particle size of lithium-based bentonite is 400-500 mesh; The solid content of potassium silicate water glass is 37%~42%, and the modulus is 2.9~3.1; The solid content of aluminum dihydrogen phosphate aqueous solution is 38%~53%; Component B is a microcapsule powder, wherein the core material is composed of the following raw materials by mass fraction: 35%~45% elemental silica powder, 55%~65% potassium nitrate powder, and the capsule wall includes EVA resin and 3%~8% liquid paraffin by mass of the capsule wall; the specific requirements for the raw materials include: The particle size of elemental silica powder is 600-800 mesh, industrial grade; The potassium nitrate powder has a particle size of 800-1000 mesh and is of industrial grade. The Vicat softening point of EVA resin is 85~95℃, and the vinyl acetate content is 18%~22% by mass. Liquid paraffin is food grade; The melting temperature of the capsule wall is 520~580 ℃.
[0020] The functions of each of the above components are as follows: Fused silica powder: Constructs a high-temperature resistant rigid framework for the ceramic layer, with a low coefficient of thermal expansion and no abrupt crystal structure changes throughout the entire heat treatment temperature range, ensuring the dimensional stability of the film structure; α-Alumina micro powder: fills the gaps between powder particles, reduces the porosity of the coating, and improves the high-temperature density, strength, and oxygen barrier properties of the film. Potassium silicate water glass: It can uniformly disperse solid powder at room temperature and provide initial adhesion, while at high temperature it provides silicate precursors and participates in the construction of silicon-oxygen ceramic networks; Anhydrous potassium metaborate: Reduces the crosslinking activation energy of inorganic systems, assists in rapid liquid phase spreading at medium temperatures, and promotes rapid molding of pre-ceramic skeletons; Aqueous solution of aluminum dihydrogen phosphate: forms a chemical anchor bond with the steel substrate, improves the adhesion of the coating at room temperature, and avoids powdering and delamination in the early stage of furnace loading; Lithium-based bentonite: As a rheology suspending agent, it ensures the uniformity and stability of the slurry, prevents sedimentation and stratification, and ensures the consistency of spraying construction; Elemental silica powder and potassium nitrate powder: form a mild and controllable exothermic oxidation system. After contact, they release heat steadily, providing additional activation energy for the medium-temperature pre-ceramic reaction. EVA resin: The exothermic core material is completely isolated at room temperature, preventing premature reaction and agglomeration failure. It melts and breaks down only in the medium temperature range of 520~580℃, realizing the point-to-point, time-to-time, and controllable triggering of the pre-ceramic reaction.
[0021] A second aspect of the present invention provides a method for preparing the above-mentioned in-situ pre-ceramic steel heat treatment anti-oxidation coating, comprising the following steps: I. Preparation of Component A: (1) Add lithium-based bentonite to deionized water and keep the temperature constant at 25~30℃. First, stir at 60~80 r / min for 35~45 min to complete the initial water absorption and swelling. Then, increase the speed to 280~320 r / min and stir for 15~25 min to carry out interlayer peeling and activation. Let it stand for 10~14 h to eliminate the hidden danger of slurry stratification in the later stage and obtain the pregel mother liquor. (2) Add aluminum dihydrogen phosphate aqueous solution to the pregel mother liquor obtained in step (1) under uniform stirring at 100~140 r / min for 25~30 min, and then add potassium silicate water glass at a uniform speed. After the addition is completed, stir at a constant temperature for 35~45 min to achieve molecular-level complexation of the two inorganic binders, avoid local gelation and agglomeration, and obtain composite binder. (3) Premix the fused silica powder and α-alumina micro powder evenly, and add them in equal amounts in three batches to the composite binder obtained in step (2). After each batch is added, stir at 350~450 r / min for 10~20 min. After all the addition is completed, increase the stirring speed to 1200~1500 r / min and stir for 55~65 min. Finally, add anhydrous potassium metaborate and continue stirring at 1200~1500 r / min for 25~35 min to dissolve and disperse evenly. (4) Two-stage filtration is adopted. The first stage is 80-mesh primary filtration and the second stage is 300-mesh fine filtration to remove aggregated particles and mechanical impurities. The filtrate is transferred to a sterile and sealed storage tank, filled into light-proof plastic buckets under negative pressure, and stored in a sealed container at room temperature. II. Preparation of Component B 1) Mix elemental silicon powder and potassium nitrate powder under a nitrogen atmosphere for 85-95 minutes, keeping the air and moisture out of the air throughout the process to prevent silicon powder from oxidizing and potassium nitrate from absorbing moisture and clumping, thus ensuring microscopic mixing uniformity. 2) Melt EVA resin in a reactor at a constant temperature of 115~120℃, add liquid paraffin as a coating rheology modifier, stir for 20~30min to obtain EVA molten coating liquid, and keep it at a controlled temperature for later use; 3) The mixed powder obtained in step 1) is fed into a fluidized bed coating machine. The bed is preheated to 480~490℃ for preheating and drying to remove water. EVA molten coating liquid is sprayed from top to bottom at a uniform speed using pressure atomization. The atomization pressure is controlled at 0.25~0.3MPa. The coating is sprayed intermittently in 4 layers. After each layer is sprayed, it is kept warm and cured for 6~10 minutes to achieve a uniform, dense film without pinholes. The fluidized bed temperature is controlled at 480~500℃ throughout the process to avoid premature melting and cell wall breakage. 4) After granulation, cool to room temperature, then pass through two vibrating sieves of 60 mesh and 120 mesh in sequence, transfer to vacuum aluminum foil packaging, fill with nitrogen, seal and store in the dark.
[0022] In the above technical solution, further, in step (4), the filtration step is: a two-stage filtration is adopted, the first stage is a 70~100 mesh pre-filtration, and the second stage is a 250~350 mesh fine filtration.
[0023] In the above technical solution, further, in step 4), the screening step is: sequentially passing through two levels of vibrating sieves of 50~70 mesh and 100~140 mesh.
[0024] The third aspect of this invention provides a method for applying the above-mentioned in-situ pre-ceramic steel heat treatment anti-oxidation coating. Component A and component B are mixed uniformly at a mass ratio of 100:(4~7). Under room temperature conditions, the mixture is sprayed onto the surface of the steel workpiece. After natural surface drying, it is placed in a heat treatment furnace along with the steel workpiece for heat treatment. Components A and B are stored independently at room temperature, away from light and moisture, and are only mixed according to the mass ratio during on-site construction. The mixed slurry must be sprayed within 4 hours to prevent the microcapsules from absorbing water and becoming ineffective.
[0025] The antioxidant coating of the present invention will be further described below through specific embodiments.
[0026] Example 1 An in-situ pre-ceramic steel heat treatment anti-oxidation coating comprises component A and component B in a mass ratio of 100:5; wherein: Component A consists of the following raw materials by mass fraction: 43% 900-mesh fused silica powder, 7.5% 650-mesh α-alumina micro powder, 26% potassium silicate water glass with a modulus of 3.0 and a solid content of 40%, 5% anhydrous potassium metaborate, 2.6% aluminum dihydrogen phosphate aqueous solution with a solid content of 50%, 1.2% 400-mesh lithium-based bentonite, and 14.7% deionized water; Component B is a microcapsule powder. The core material is made by uniformly mixing 40% by mass of industrial elemental silica powder with a particle size of 700 mesh and 60% by mass of industrial potassium nitrate powder with a particle size of 900 mesh. The capsule wall contains EVA resin and 5% by mass of food-grade liquid paraffin. The EVA resin has a Vicat softening point of 90℃ and a vinyl acetate content of 19%.
[0027] The above-mentioned method for preparing the coating: Preparation of component A (1) Pre-swelling and activation pretreatment of bentonite: metered deionized water was injected into a jacketed temperature-controlled stirring reactor and the temperature was kept constant at 26℃. 400 mesh lithium-based bentonite was added and first dispersed and stirred at a low speed of 70 r / min for 36 min to complete the initial water absorption and swelling. Then the speed was increased to 300 r / min for high-speed shearing for 20 min to carry out interlayer exfoliation and activation. After standing and maturing for 12 h, a pre-gel mother liquor was obtained. (2) Composite adhesive compounding: Add 50% aluminum dihydrogen phosphate aqueous solution to the pregel mother liquor obtained in step (1) under uniform stirring at 120 r / min, and control the addition time to 26 min. Then add 3.0 modulus and 40% potassium silicate water glass at a uniform speed. After the addition is completed, stir at a constant temperature for 40 min to achieve molecular-level composite complexation of the two inorganic adhesives, avoid local gelation and agglomeration, and obtain composite adhesive. (3) Gradient feeding of solid powder + multi-stage dispersion: 900 mesh fused silica powder and 650 mesh α-alumina micro powder are premixed evenly and added into the kettle in three equal portions. After each batch of feeding, the mixture is stirred at a medium speed of 400 r / min for 15 min. After all the feeding is completed, the speed is increased to 1300 r / min for high-speed shearing dispersion for 60 min. Finally, anhydrous potassium metaborate is slowly added and the mixture is stirred at high speed for 30 min to dissolve and disperse evenly. (4) Fine filtration and sealed filling: After the entire system is stirred, two-stage fine filtration (80 mesh primary filtration + 300 mesh fine filtration) is used to remove agglomerated particles and mechanical impurities. The filtrate is transferred to a sterile sealed storage tank, filled into light-proof plastic buckets under negative pressure, and stored in a sealed container at room temperature.
[0028] Preparation of component B 1) Powder atmosphere protected premixing: 700 mesh elemental silicon powder and 900 mesh potassium nitrate powder are added into a nitrogen-sealed protective silo and mixed at low speed for 90 minutes using a three-dimensional swing mixer. The entire process is isolated from air and moisture to prevent silicon powder oxidation and potassium nitrate from absorbing moisture and clumping, thus ensuring microscopic mixing uniformity. 2) Preparation of EVA melt coating solution: Select EVA resin with a Vicat softening point of 90℃ and a vinyl acetate content of 19% by mass, melt it at a constant temperature in a closed reactor at 116℃, add 5% food-grade liquid paraffin as a coating rheology modifier, stir at low speed for 25 minutes to form a homogeneous EVA melt coating solution, and keep it at a controlled temperature for later use. (3) Fluidized bed gradient temperature control full coating granulation: The mixed powder is put into a low temperature fluidized bed coating machine, the bed is preheated to 480℃ for preheating and drying to remove water, and EVA molten coating liquid is sprayed from top to bottom at a uniform speed using pressure atomization. The atomization pressure is controlled at 0.26MPa, and the coating is sprayed intermittently in 4 layers. After each layer is sprayed, it is kept warm and solidified for 8 minutes to achieve a uniform and dense film without pinholes. The fluidized bed temperature is stable at 490℃ throughout the process to avoid premature melting and wall breakage. (4) Screening: After granulation, the mixture is cooled to room temperature and then screened through two stages of vibrating sieves: 60 mesh and 120 mesh. It is then transferred to vacuum aluminum foil packaging, filled with nitrogen, sealed, and stored in the dark.
[0029] Storage and application of the above-mentioned coatings Components A and B should be stored independently at room temperature, away from light and moisture. They should only be mixed on-site according to the mass ratio. Components A and B should be mixed evenly on-site at a mass ratio of 100:5. Under room temperature conditions, the mixture should be sprayed onto the surface of the steel workpiece. After natural surface drying, the mixture should be placed in a heat treatment furnace along with the steel workpiece for heat treatment. The mixed slurry must be sprayed within 4 hours.
[0030] Example 2 An in-situ pre-ceramic steel heat treatment anti-oxidation coating comprises component A and component B in a mass ratio of 100:6; wherein: Component A consists of the following raw materials by mass fraction: 45% 950-mesh fused silica powder, 8% 700-mesh α-alumina micro powder, 27% potassium silicate water glass with a modulus of 2.9 and a solid content of 40%, 4.5% anhydrous potassium metaborate, 2.8% aluminum dihydrogen phosphate aqueous solution with a solid content of 50%, 1.5% 450-mesh lithium-based bentonite, and 11.2% deionized water; Component B is a microcapsule powder. The core material is made by uniformly mixing 40% by mass of industrial elemental silica powder with a particle size of 750 mesh and 60% by mass of industrial potassium nitrate powder with a particle size of 950 mesh. The capsule wall contains EVA resin and 6% by mass of food-grade liquid paraffin. The EVA resin has a Vicat softening point of 92℃ and a vinyl acetate content of 20%.
[0031] The above-mentioned method for preparing the coating: Preparation of component A (1) Pre-swelling and activation pretreatment of bentonite: metered deionized water was injected into a jacketed temperature-controlled stirring reactor and the temperature was kept constant at 27°C. 450 mesh lithium-based bentonite was added and first dispersed and stirred at a low speed of 75 r / min for 40 min to complete the initial water absorption and swelling. Then the speed was increased to 300 r / min for high-speed shearing for 20 min to carry out interlayer exfoliation and activation. After standing and maturing for 12 h, a pre-gel mother liquor was obtained. (2) Composite adhesive compounding: Add 50% aluminum dihydrogen phosphate aqueous solution to the pregel mother liquor obtained in step (1) under uniform stirring at 120 r / min, and control the addition time to 27 min. Then add 3.1 modulus and 40% solid content potassium silicate water glass at a uniform speed. After the addition is completed, stir at a constant temperature for 40 min to achieve molecular-level composite complexation of the two inorganic adhesives, avoid local gelation and agglomeration, and obtain composite adhesive. (3) Gradient feeding of solid powder + multi-stage dispersion: 950 mesh fused silica powder and 700 mesh α-alumina micro powder are premixed evenly and added into the kettle in three equal portions. After each batch of feeding, the mixture is stirred at a medium speed of 400 r / min for 15 min. After all the feeding is completed, the speed is increased to 1400 r / min for high-speed shearing dispersion for 60 min. Finally, anhydrous potassium metaborate is slowly added and the mixture is stirred at high speed for 30 min to dissolve and disperse evenly. (4) Fine filtration and sealed filling: After the entire system is stirred, two-stage fine filtration (80 mesh primary filtration + 300 mesh fine filtration) is used to remove agglomerated particles and mechanical impurities. The filtrate is transferred to a sterile sealed storage tank, filled into light-proof plastic buckets under negative pressure, and stored in a sealed container at room temperature.
[0032] Preparation of component B 1) Powder atmosphere protected premixing: 750 mesh elemental silicon powder and 950 mesh potassium nitrate powder are added into a nitrogen-sealed protective silo and mixed at low speed for 90 minutes using a three-dimensional swing mixer. The entire process is isolated from air and moisture to prevent silicon powder oxidation and potassium nitrate from absorbing moisture and clumping, thus ensuring microscopic mixing uniformity. 2) Preparation of EVA melt coating solution: Select EVA thermosensitive resin with a Vicat softening point of 91℃ and a vinyl acetate content of 20% by mass, melt it at a constant temperature in a closed reactor at 118℃, add 6% food-grade liquid paraffin as a coating rheology modifier, stir at low speed for 25 minutes to form a homogeneous EVA melt coating solution, and keep it at a controlled temperature for later use. 3) Fluidized bed gradient temperature controlled full coating granulation: The mixed powder is put into a low temperature fluidized bed coating machine, the bed is preheated to 480℃ for preheating and drying to remove water, and EVA molten coating liquid is sprayed from top to bottom at a uniform speed using pressure atomization, controlling the atomization pressure to 0.28MPa, and coating is done in 4 layers intermittently. After each layer is sprayed, it is kept at the temperature for 8 minutes to achieve a uniform, dense film without pinholes. The fluidized bed temperature is kept stable at 495℃ throughout the process to avoid premature melting and cell wall breakage.
[0033] 4) Screening: After granulation, the product is cooled to room temperature and then screened through two stages of vibrating sieves: 60 mesh and 120 mesh. It is then transferred to vacuum aluminum foil packaging, filled with nitrogen, sealed, and stored in the dark.
[0034] Storage and application of the above-mentioned coatings Components A and B should be stored independently at room temperature, away from light and moisture. They should only be mixed on-site according to the mass ratio. Components A and B should be mixed evenly on-site at a mass ratio of 100:6. Under room temperature conditions, the mixture should be sprayed onto the surface of the steel workpiece. After natural surface drying, the mixture should be placed in a heat treatment furnace along with the steel workpiece for heat treatment. The mixed slurry must be sprayed within 4 hours.
[0035] Comparative Example 1 A conventional single-component coating was used as a control sample. The coating formulation, by mass percentage, consisted of: 46.9% borosilicate glass powder, 15.6% alumina, 12.5% sodium silicate aqueous solution (modulus 3.2), and 25% deionized water. The above materials were stirred and mixed evenly to prepare the control coating slurry.
[0036] The evaluation used a programmable muffle furnace as the heating furnace. Carbon steel billets with dimensions of 100mm×100mm×10mm were selected. At room temperature, the pre-ceramic heat treatment coatings of Examples 1-2 and the conventional heat treatment coating of Comparative Example 1 were uniformly coated on the surface of the billets, and then allowed to dry naturally. After drying, the coverage of the dry film at room temperature was observed first, and then the samples were sent into the muffle furnace to simulate the heat treatment heating process: the temperature was uniformly increased to 300℃ at room temperature and held for 30 minutes, then increased to 700℃ and held for 1 hour, and finally increased to 1180℃ and held for 2 hours. During the heat treatment process, the cracking and peeling of the coating were closely monitored and recorded at 700℃. After cooling to room temperature, the billets were weighed and the oxidation weight loss rate was calculated.
[0037] See Table 1 for details of the experiment.
[0038] Table 1
[0039] The comparative results show that during the room-temperature drying stage, both the pre-ceramic coatings of the two examples and the conventional coating can form a smooth and uniform dry film on the steel billet surface. However, when the heat treatment temperature reaches the critical range of 700℃, the performance shows a significant divergence: the pre-ceramic coatings of Examples 1 and 2 form a dense and uniform complete ceramic protective layer at this temperature, with a strong bond between the coating and the steel substrate, and no cracking or crazing defects. The corresponding high-temperature weight loss rates of the steel billet are only 1.21% and 1.28%, respectively, and the decarburized layer thickness of the steel is only 9μm and 10μm, respectively, which can effectively block oxygen penetration and significantly inhibit substrate decarburization. In contrast, the conventional coating of Comparative Example 1 shows obvious crazing at 700℃, and the integrity of the protective film layer is destroyed, failing to form a sealed isolation barrier. Its steel billet weight loss rate increases to 1.66%, oxidation intensifies, and the decarburized layer thickness reaches 36μm, far exceeding that of the coatings of the two examples. Its anti-oxidation and anti-decarburization capabilities are significantly reduced, making it difficult to meet the protection requirements of the steel heat treatment process. Overall, it can be seen that the pre-formed ceramic coatings of Examples 1-2 can form a dense ceramic protective layer at the medium temperature stage, which has both excellent high-temperature oxidation resistance and decarburization prevention effects, and its performance is significantly better than that of conventional coatings.
[0040] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the implementation. The scope of protection of the present invention should be determined by the scope defined in the claims. Other variations or modifications can be made based on the above description. Obvious variations or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. An in-situ pre-ceramic steel heat treatment anti-oxidation coating, characterized in that, The coating is composed of component A and component B, with a mass ratio of component A to component B of 100:(4~7). The A component is composed of the following raw materials by mass fraction: 42%~48% fused silica powder, 7%~9% α-alumina micro powder, 25%~29% potassium silicate water glass, 4%~6% anhydrous potassium metaborate, 2%~3% aluminum dihydrogen phosphate aqueous solution, 1.0%~1.8% lithium-based bentonite, and the balance being deionized water. Component B is a microcapsule powder, wherein the core material is composed of the following raw materials by mass fraction: 35%~45% elemental silica powder, 55%~65% potassium nitrate powder, and the capsule wall includes EVA resin and liquid paraffin accounting for 3%~8% of the capsule wall mass.
2. The in-situ pre-ceramic steel heat treatment anti-oxidation coating according to claim 1, characterized in that, The particle size of the fused silica powder is 800~1000 mesh; The particle size of the α-alumina micro powder is 600~800 mesh; The lithium-based bentonite has a particle size of 400-500 mesh.
3. The in-situ pre-ceramic steel heat treatment anti-oxidation coating according to claim 1, characterized in that, The potassium silicate water glass has a solid content of 37% to 42% and a modulus of 2.9 to 3.
1. The solid content of the aluminum dihydrogen phosphate aqueous solution is 38%~53%.
4. The in-situ pre-ceramic steel heat treatment anti-oxidation coating according to claim 1, characterized in that, The particle size of the elemental silicon powder is 600-800 mesh; The potassium nitrate powder has a particle size of 800-1000 mesh.
5. The in-situ pre-ceramic steel heat treatment anti-oxidation coating according to claim 1, characterized in that, The EVA resin has a Vicat softening point of 85~95℃ and a vinyl acetate content of 18%~22% by mass.
6. The in-situ pre-ceramic steel heat treatment anti-oxidation coating according to claim 1, characterized in that, The melting temperature of the capsule wall is 520~580 ℃.
7. A method for preparing an in-situ pre-ceramic steel heat treatment anti-oxidation coating according to any one of claims 1-6, characterized in that, Includes the following steps: I. Preparation of Component A: (1) Add lithium-based bentonite to deionized water, keep the temperature constant at 25~30℃, stir at 60~80 r / min for 35~45 min, then increase the speed to 280~320 r / min and stir for 15~25 min, let stand and mature for 10~14 h to obtain pregel mother liquor. (2) Add aluminum dihydrogen phosphate aqueous solution to the pregel mother liquor obtained in step (1) under the condition of uniform stirring at 100~140 r / min, and control the addition time to 25~30 min. Then add potassium silicate water glass at a uniform speed. After the addition is completed, stir at a constant temperature for 35~45 min to obtain composite adhesive. (3) Premix the fused silica powder and α-alumina micro powder evenly, and add them in equal amounts in three batches to the composite binder obtained in step (2). After each batch of material is added, stir at 350~450 r / min for 10~20 min. After all the materials are added, increase the stirring speed to 1200~1500 r / min and stir for 55~65 min. Finally, add anhydrous potassium metaborate and continue stirring at 1200~1500 r / min for 25~35 min. (4) Filter and collect the filtrate; II. Preparation of Component B 1) Mix elemental silicon powder and potassium nitrate powder under a nitrogen atmosphere for 85-95 minutes; 2) Melt EVA resin in a reactor at a constant temperature of 115~120℃, add liquid paraffin, and stir for 20~30 minutes to obtain EVA melt coating solution; 3) The mixed powder obtained in step 1) is fed into a fluidized bed coating machine. The bed is preheated to 480~490℃ for preheating and drying. EVA molten coating liquid is sprayed uniformly from top to bottom using pressure atomization. The atomization pressure is controlled at 0.25~0.3 MPa. The coating is carried out in 4 layers by intermittent spraying. After each layer is sprayed, it is kept warm and cured for 6~10 min. The fluidized bed temperature is controlled at 480~500℃ throughout the process. 4) After granulation, cool to room temperature and sieve.
8. The preparation method according to claim 7, characterized in that, In step (4), the filtration step is as follows: a two-stage filtration is adopted, the first stage is a 70~100 mesh pre-filtration, and the second stage is a 250~350 mesh fine filtration.
9. The preparation method according to claim 7, characterized in that, In step 4), the screening step is as follows: the material is sequentially screened through two levels of vibrating sieves, namely 50-70 mesh and 100-140 mesh.
10. A method for applying an in-situ pre-ceramic steel heat treatment anti-oxidation coating according to any one of claims 1-6 or an in-situ pre-ceramic steel heat treatment anti-oxidation coating prepared by the preparation method according to any one of claims 7-9, characterized in that, Mix component A and component B evenly, spray the mixture onto the surface of the steel workpiece at room temperature, and allow it to dry naturally before entering the heat treatment furnace along with the steel workpiece for heat treatment.
Citation Information
Patent Citations
Spontaneous heating coating for substrate surface and preparation method of spontaneous heating coating
CN103203938A
High-temperature-resistant long-time-heating anti-oxidation coating for high-alloy steel billet, and coating method thereof
CN112940544A