A UV-resistant ink and its preparation method
By using nano-cerium oxide loaded with zinc oxide as a UV absorber in inks, the problems of low UV resistance and unstable light transmittance of inks were solved, achieving improvements in UV resistance and mechanical properties of inks while maintaining good transparency and dispersibility.
Patent Information
- Application Number
- CN202611495775.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing inks are unstable in terms of UV resistance, light transmittance, and mechanical properties. In traditional methods, excessive addition of UV absorbers can affect curing, and excessive addition of inorganic fillers can lead to a decrease in transparency.
Nano-cerium oxide is used as an ultraviolet absorber. Zinc oxide particles are loaded onto it using its mesoporous structure. Ultraviolet rays are scattered through Mie scattering and reflection. The dispersion stability in non-polar resin is improved by hydrophobic modification. The sustained release effect of the mesoporous structure is combined to enhance the ultraviolet absorption effect.
By reducing the total amount of UV absorber, the UV resistance and mechanical properties of the ink are significantly improved, while maintaining good transparency and dispersibility, thus avoiding the defects of traditional methods.
Smart Images

Figure CN123107450A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of specialty ink preparation technology, and in particular to a UV-resistant ink and its preparation method. Background Technology
[0002] In traditional printing, electronics manufacturing, and outdoor signage, inks are exposed to natural light for extended periods. The ultraviolet (UV) radiation in natural light is sufficient to cause irreversible damage to printed images, including fading, ink film powdering and peeling, and decreased material performance. With the rapid development of the materials industry, the printing industry has developed methods to improve the UV resistance of inks by introducing benzophenone and benzotriazole UV absorbers into the ink system to directly absorb UV radiation and convert it into heat. Currently, the most direct and effective way to improve ink's lightfastness is to increase the amount of UV absorber added. However, excessive addition of traditional organic UV absorbers can negatively impact the UV curing of the ink; excessive addition of traditional inorganic fillers can significantly reduce ink transparency and increase the risk of unstable ink dispersion. Rare earth oxides possess a unique 4f unfilled electron layer structure, which can directly capture UV photon energy through ff transitions or charge transfer effects, avoiding photochemical reactions. However, rare earth oxides are hydrophilic and have poor compatibility in nonpolar systems, easily leading to aggregation. Therefore, there is an urgent need to develop an ink that can significantly improve UV resistance and mechanical properties. Summary of the Invention
[0004] The purpose of this invention is to provide a UV-resistant ink and its preparation method, so as to solve the technical problems of low UV resistance, unstable light transmittance and mechanical properties of inks in the prior art.
[0005] To solve the above-mentioned technical problems, the present invention provides a UV-resistant ink, the ink comprising: 2-10 parts of nano-cerium oxide, 20-30 parts of epoxy acrylic resin, 20-40 parts of polyester acrylic resin, 50-70 parts of acrylate, 0.5-2 parts of defoamer, 0.3-1.5 parts of dispersant, 1-1.5 parts of leveling agent, and 0.5-1 part of photoinitiator;
[0006] The nano-cerium oxide has a mesoporous structure;
[0007] The mesoporous structure of the nano-cerium oxide contains zinc oxide.
[0008] The above components are listed in parts by mass.
[0009] Furthermore, the particle size of the nano-cerium oxide is 20nm-50nm.
[0010] When the particle size of nano-cerium oxide is between 20nm and 50nm, it is close to the wavelength of ultraviolet light. When ultraviolet light shines on the surface of nano-cerium oxide, Mie scattering will occur. Ultraviolet light is simultaneously reflected and scattered significantly on the particle surface. Nano-cerium oxide particles can effectively achieve physical shielding against ultraviolet light.
[0011] Nano-cerium oxide possesses excellent absorption capacity across the entire ultraviolet range; the smaller the particle size, the stronger the ultraviolet absorption performance. Furthermore, its visible light transmittance is significantly higher than that of commercially available ultraviolet absorbers, resulting in better film transparency. Therefore, this application uses nano-cerium oxide as the primary ultraviolet absorber. Adding nano-cerium oxide can improve the UV resistance of the ink while reducing the total amount of ultraviolet absorber added. Simultaneously, this application creatively employs nano-cerium oxide with a mesoporous structure, loading another ultraviolet absorber—zinc oxide particles—within its mesoporous structure. Zinc oxide, loaded within the mesoporous structure, cannot absorb ultraviolet light, thus reducing the amount of ultraviolet absorber in the system before and during the initial stage of film formation. This ensures that the photoinitiator fully absorbs ultraviolet energy, improving excitation efficiency, significantly increasing the crosslinking density of the resin, and ultimately enhancing the ink's abrasion resistance, adhesion, and other mechanical properties. After film formation, the nano-cerium oxide absorbs ultraviolet light and converts it into heat energy. At this time, the zinc oxide particles, attached to the mesopores by van der Waals forces, are slowly released, increasing the variety and total amount of ultraviolet absorbers in the cured ink system, significantly improving the ink's UV resistance during use.
[0012] Furthermore, the nano-cerium oxide is selected from native nano-cerium oxide and hydrophobically modified nano-cerium oxide.
[0013] Native nano-cerium oxide, as a rare earth metal oxide, contains a certain amount of hydroxyl groups on its surface, exhibiting weak hydrophilicity. Hydrophobic modification can significantly improve the dispersion stability and uniformity of nano-cerium oxide in non-polar resins, avoiding UV shielding blind spots caused by localized particle agglomeration. This is beneficial for improving the UV resistance of inks and reducing the risk of ink cracking. Therefore, the nano-cerium oxide used in this technical solution is preferably hydrophobically modified nano-cerium oxide.
[0014] Furthermore, the pore size of the mesoporous structure is 10nm-30nm.
[0015] The mesoporous structure of nano-cerium oxide is loaded with zinc oxide. Therefore, the pore size of the mesoporous structure is preferably 10nm-30nm. This ensures that there is enough space to load zinc oxide particles, and at the same time, it can limit the size of the loaded zinc oxide particles to be close to the ultraviolet wavelength, so that the zinc oxide particles can also have the function of physical shielding against ultraviolet rays after being released.
[0016] Preferably, the defoamer is selected from silicone defoamers and mineral oil defoamers;
[0017] The dispersants were selected from BASF 4310 and KMT-3331;
[0018] The leveling agent is selected from BYK-354, anjeka4330, and anjeka4420.
[0019] Preferably, the photoinitiator is selected from 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone.
[0020] On the other hand, the present invention also provides a method for preparing the above-mentioned UV-resistant ink, the method comprising the following steps: (The following components are all in parts by mass)
[0021] Step 1: Take 20-30 parts of epoxy acrylic resin, 20-40 parts of polyester acrylic resin, and 50-70 parts of acrylate and stir slowly until they are evenly mixed to obtain the first mixture.
[0022] Step 2: Add 2-10 parts of zinc oxide-loaded nano-cerium oxide and 0.3-1.5 parts of dispersant to the first mixture in sequence, stir for 15-20 minutes to obtain the second mixture;
[0023] Step 3: Add 0.5-2 parts of defoamer, 1-1.5 parts of leveling agent, and 0.5-1 parts of photoinitiator to the second mixture, and stir thoroughly to obtain UV-resistant ink.
[0024] Furthermore, the preparation method of the zinc oxide-loaded nano-cerium oxide includes the following specific steps:
[0025] Step A1: Keep the nano-cerium oxide in a negative pressure environment for 0.5-1h, then continuously inject a 5%-15% zinc acetate solution into the nano-cerium oxide with a mesoporous structure, and keep it under negative pressure for 1-2h. Take it out to obtain nano-cerium oxide particles loaded with zinc acetate.
[0026] Step A2: The zinc acetate-loaded cerium oxide nanoparticles are baked at 250℃-300℃ for 1-2 hours to obtain the zinc oxide-loaded cerium oxide nanoparticles.
[0027] Preferably, the nano-cerium oxide is hydrophobically modified nano-cerium oxide;
[0028] The preparation steps of the hydrophobically modified nano-cerium oxide are as follows:
[0029] Step B1: Dry the original nano-cerium oxide at 120°C under vacuum for 2 hours to obtain pretreated nano-cerium oxide;
[0030] Step B2: Mix the silane coupling agent with anhydrous ethanol and deionized water at a mass ratio of (1-3):8:1 and adjust the pH to 4-5. Stir at room temperature for 20-30 minutes to obtain the first reaction suspension.
[0031] Step B3: Prepare a 10% concentration suspension by mixing the pretreated nano-cerium oxide with anhydrous ethanol, then add it to the first reaction suspension, and stir continuously at 50℃-80℃ for 5-10 hours to obtain the second reaction suspension.
[0032] The mass ratio of the added silane coupling agent to nano-cerium oxide is (3-10):100;
[0033] Step B4: After centrifuging the second reaction suspension, the resulting filter residue is washed alternately with anhydrous ethanol and deionized water to obtain the hydrophobic modified nano-cerium oxide.
[0034] Preferably, the silane coupling agent is selected from KH550, KH570, KH590, and vinyltrimethoxysilane.
[0035] By adopting the above technical solution, the present invention has the following beneficial effects:
[0036] This invention provides a UV-resistant ink and its preparation method, using nano-cerium oxide loaded with zinc oxide particles as a UV absorber. On one hand, nano-cerium oxide, as a rare earth metal oxide, possesses a unique 4f electron layer structure, allowing for more efficient UV absorption through electron transitions. On the other hand, nano-cerium oxide has a mesoporous structure, within which a large number of zinc oxide particles are loaded, allowing for slow release. This reduces the amount of UV absorber in the ink system during the initial curing stage, increases the excitation efficiency of the photoinitiator in absorbing UV light, improves the crosslinking density of the ink resin, and enhances the mechanical properties of the ink. Furthermore, the slow-release effect of the mesoporous structure increases the types and total amount of UV absorbers in the ink system after curing, significantly improving the ink's scattering and absorption of UV light, thus enhancing the ink's UV resistance. Attached Figure Description
[0037] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0038] Figure 1 A flowchart illustrating the preparation method of the UV-resistant ink provided by this invention;
[0039] Figure 2 This is a line graph comparing the UV test results of the inks obtained in Example 1 and Example 2;
[0040] Figure 3 The bar chart shows the UV test results of the four groups of inks obtained in Example 3 and the inks obtained in Example 1. Detailed Implementation
[0041] The present invention will be further explained below with reference to specific embodiments.
[0042] The UV-resistant ink is prepared using the method provided by this invention, and the specific steps are as follows:
[0043] Step 1: Take nano-cerium oxide with a mesoporous structure, let it stand under negative pressure for 0.5-1h, and then continuously inject a zinc acetate solution with a mass fraction of 5%-15%; keep it immersed under negative pressure for 1-2h to obtain nano-cerium oxide loaded with zinc acetate; then bake the nano-cerium oxide loaded with zinc acetate at 250℃-300℃ for 1-2h to obtain nano-cerium oxide loaded with zinc oxide.
[0044] Step 2: Take 20-30 parts of epoxy acrylic resin, 20-40 parts of polyester acrylic resin, and 50-70 parts of acrylate and stir at a speed of 80r / min-100r / min for 30min-60min until they are evenly mixed to obtain the first mixture.
[0045] Step 3: Add 2-10 parts of zinc oxide-loaded nano-cerium oxide and 0.3-1.5 parts of dispersant to the first mixture in sequence, stir for 15-20 minutes to obtain the second mixture;
[0046] The dispersants were selected from BASF 4310 and KMT-3331;
[0047] Step 4: Add 0.5-2 parts of defoamer, 1-1.5 parts of leveling agent, and 0.5-1 parts of photoinitiator to the second mixture, and stir thoroughly to obtain UV-resistant ink.
[0048] The defoamer is selected from silicone-based defoamers and mineral oil-based defoamers;
[0049] The leveling agent is selected from BYK-354, anjeka4330, and anjeka4420.
[0050] The photoinitiator is selected from 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone.
[0051] All components are listed in parts by mass.
[0052] Performance testing:
[0053] First, the ink to be tested is printed on PC plastic sheet using pad printing. Five pieces are tested for each performance item, and the average value is taken.
[0054] Adhesion test:
[0055] On the surface of the printed sample, an Erichsen 295 cross-cut tester was used to draw 100 lines at 1mm intervals. 3M tape was then applied to the cross-cut surface for 3 minutes, and then removed at a 60° angle within 0.5-1 second. The grade was determined based on the degree of ink removal, classifying the sample from Class 0 to Class 5. Specific criteria are shown in Table 1 below.
[0056] Table 1 Adhesion Test Judgment Criteria
[0057] Determine the level Class0 Class1 Class2 Class3 Class4 Class5 Area of detachment 0% ≤5% 5%-15% 15%-35% 35%-65% ≥65%
[0058] Solvent resistance test:
[0059] Eight layers of gauze containing 0.5 ml of anhydrous ethanol were used, with a strength of 9.8 ± 0.05 N / cm. 2 Under load, the device reciprocates 200 times at a speed of 0.5 times / s, pausing every 20 reciprocations to check for damage or discoloration on the ink surface.
[0060] UV resistance test:
[0061] The tests and evaluations were conducted in accordance with GB / T22771-2008 Test and Evaluation of Light Aging Resistance of Printed Matter and Printing Ink.
[0062] Haze test:
[0063] According to GB2410-80 Test Method for Light Transmittance and Haze of Transparent Plastics, a haze meter is used to measure the haze value of the sample.
[0064] Example 1
[0065] As attached Figure 1 As shown, this embodiment verifies that the UV-resistant ink is obtained using the preparation method provided by the present invention.
[0066] Step 1: Take 200g of hydrophobically modified nano-cerium oxide with mesoporous structure, let it stand under negative pressure for 1h, and then continuously inject 15% zinc acetate solution by mass; keep it immersed under negative pressure for 2h to obtain nano-cerium oxide loaded with zinc acetate; then bake the nano-cerium oxide loaded with zinc acetate at 250℃ for 1.5h to obtain nano-cerium oxide loaded with zinc oxide.
[0067] Step 2: Take 300g of epoxy acrylic resin, 200g of polyester acrylic resin, and 600g of acrylate and stir at 80r / min for 30min until they are evenly mixed to obtain the first mixture.
[0068] Step 3: Add 80g of zinc oxide-loaded nano-cerium oxide and 10g of dispersant KMT-3331 to the first mixture in sequence, stir for 20min to obtain the second mixture;
[0069] Step 4: Add 10g of defoamer HH-203, 15g of leveling agent BYK-354, and 5g of 1-hydroxycyclohexylphenyl ketone to the second mixture, and stir thoroughly to obtain UV-resistant ink.
[0070] Example 2
[0071] As attached Figure 2 As shown, this embodiment verifies the effect of adding native nano-cerium oxide on ink performance.
[0072] Step 1: Take 200g of native nano-cerium oxide with mesoporous structure, let it stand under negative pressure for 1h, and then continuously inject 15% zinc acetate solution by mass; keep it immersed under negative pressure for 2h to obtain nano-cerium oxide loaded with zinc acetate; then bake the nano-cerium oxide loaded with zinc acetate at 250℃ for 1.5h to obtain nano-cerium oxide loaded with zinc oxide.
[0073] Step 2: Take 300g of epoxy acrylic resin, 200g of polyester acrylic resin, and 600g of acrylate and stir at 80r / min for 30min until they are evenly mixed to obtain the first mixture.
[0074] Step 3: Add 80g of zinc oxide-loaded nano-cerium oxide and 10g of dispersant KMT-3331 to the first mixture in sequence, stir for 20min to obtain the second mixture;
[0075] Step 4: Add 10g of defoamer HH-203, 15g of leveling agent BYK-354, and 5g of 1-hydroxycyclohexylphenyl ketone to the second mixture, and stir thoroughly to obtain UV-resistant ink. The mechanical properties, appearance inspection defect rate, and UV resistance test results of the ink obtained in this example are compared with those of Example 1 in Table 2: Appearance inspection confirmed the defect rate at 50pcs.
[0076] Table 2. Ink performance test results obtained in Examples 1 and 2
[0077] sample Adhesion Solvent-resistant friction UV test Haze (%) Appearance defect inspection Example 1 Class0 No change Greater than level 7 1.0 0.6% granules Example 2 Class0 No change Level 5 2.3 7.8% particle group
[0078] As shown in Table 2, the adhesion and solvent resistance test results of the ink prepared using virgin nano-cerium oxide are basically consistent with those of Example 1. However, in the appearance inspection, it was found that 7.8% of the ink obtained in Example 2 showed particle cluster defects on the surface of the printed product, and the haze was low. This may be because virgin nano-cerium oxide itself contains a certain amount of hydroxyl groups, which have weak hydrophilicity and are prone to agglomeration in the ink resin system, resulting in an overall decrease in ink haze. When the agglomerated particles are large, particulate foreign matter will form on the surface after the ink cures. In addition, in Table 2 and Appendix Figure 2 It can also be seen that the inks obtained in Example 1 all achieved a UV resistance level of 7, and some samples even reached a UV resistance level of 8, which is significantly better than the UV resistance level of the inks obtained in Example 2. This is because the native nano-cerium oxide agglomerated within the ink system, resulting in uneven distribution of the UV absorber. When exposed to UV conditions for a long time, the inks obtained in Example 2 showed localized discoloration and aging earlier, and even surface cracking. Therefore, the technical solution provided in this application recommends the preferred use of hydrophobically modified nano-cerium oxide to prepare UV-resistant inks.
[0079] Example 3
[0080] As attached Figure 3 As shown, this embodiment verifies the effect of adding different amounts of zinc oxide-loaded nano-cerium oxide on ink performance.
[0081] Step 1: Take 400g of hydrophobically modified nano-cerium oxide with mesoporous structure, let it stand under negative pressure for 1h, and then continuously inject 15% zinc acetate solution by mass; keep it immersed under negative pressure for 2h to obtain nano-cerium oxide loaded with zinc acetate; then bake the nano-cerium oxide loaded with zinc acetate at 250℃ for 1.5h to obtain nano-cerium oxide loaded with zinc oxide.
[0082] Step 2: Take 1.2 kg of epoxy acrylic resin, 0.8 kg of polyester acrylic resin, and 2.4 kg of acrylate and stir at 80 r / min for 50 min until they are evenly mixed to obtain the first mixture;
[0083] Step 3: First, divide the first mixture into 4 equal groups, and add nano-cerium oxide loaded with zinc oxide and 10g of dispersant KMT-3331 in sequence. The amount of nano-cerium oxide loaded with zinc oxide added to the 4 groups of the first mixture is 40g, 60g, 100g and 150g respectively. Stir for 20min to obtain 4 groups of second mixtures.
[0084] Step 4: 10g of defoamer HH-203, 15g of leveling agent BYK-354, and 5g of 1-hydroxycyclohexylphenyl ketone were added to the four groups of second mixtures, respectively. After thorough stirring, four groups of UV-resistant inks were obtained, labeled as 3-1, 3-2, 3-3, and 3-4. The performance test results of the four groups of inks obtained in this example and the inks obtained in Example 1 are shown in Table 3.
[0085] Table 3. Ink performance test results obtained in Example 3 and Example 1
[0086] Test sample Adhesion Solvent-resistant friction UV test Haze (%) before UV test Haze (%) after UV test 3-1 Class0 No change Level 5 1.2 1.5 3-2 Class0 No change Greater than level 6 1.1 1.3 3-3 Class0 No change Greater than level 7 1.0 1.9 3-4 Class0 No change Greater than level 7 1.2 2.0 Example 1 Class0 No change Greater than level 7 1.0 1.3
[0087] As shown in Table 3, the UV resistance continuously improves with increasing addition of mesoporous cerium oxide nanoparticles loaded with zinc oxide, while other performance tests remain largely consistent. However, when the addition amount reaches 100g or more, the ink haze significantly increases after UV testing due to the continuous release of zinc oxide loaded in the mesoporous structure of the cerium oxide nanoparticles compared to other conditions. This is because the excessive release of zinc oxide particles enhances the scattering of visible light by combining with the cerium oxide nanoparticles, thus affecting the ink haze.
[0088] Comparative Example 1
[0089] This comparative example uses nano-cerium oxide without zinc oxide loading to prepare ink.
[0090] Step 1: Take 300g of epoxy acrylic resin, 200g of polyester acrylic resin, and 600g of acrylate and stir at 80r / min for 30min until they are evenly mixed to obtain the first mixture.
[0091] Step 2: Add 80g of nano-cerium oxide and 10g of dispersant KMT-3331 to the first mixture in sequence, stir for 20min to obtain the second mixture;
[0092] Step 3: Add 10g of defoamer HH-203, 15g of leveling agent BYK-354, and 5g of 1-hydroxycyclohexylphenyl ketone to the second mixture, and stir thoroughly to obtain the sample ink, labeled as D1.
[0093] Comparative Example 2
[0094] This comparative example uses the method of directly adding nano-cerium oxide and nano-zinc oxide to prepare ink.
[0095] Step 1: Take 300g of epoxy acrylic resin, 200g of polyester acrylic resin, and 600g of acrylate and stir at 80r / min for 30min until they are evenly mixed to obtain the first mixture.
[0096] Step 2: Add 60g of nano-cerium oxide, 20g of nano-zinc oxide, and 10g of dispersant KMT-3331 to the first mixture in sequence, stir for 20 minutes, and obtain the second mixture;
[0097] Step 3: Add 10g of defoamer HH-203, 15g of leveling agent BYK-354, and 5g of 1-hydroxycyclohexylphenyl ketone to the second mixture, and stir thoroughly to obtain the sample ink, labeled D2. The performance test results of the inks obtained in Comparative Example 1 and Comparative Example 2 are compared with those in Example 1 in Table 4 below:
[0098] Table 4 Comparison of ink performance test results between Comparative Examples 1 and 2 and Example 1
[0099] Test sample Adhesion Solvent-resistant friction UV test Haze D1 Class1 160 scratches Level 6 1.3 D2 Class1 120 scratches Level 6 1.8 Example 1 Class0 No change Greater than level 7 1.0
[0100] As shown in Table 4, ink D1 prepared by adding an equal weight of unloaded zinc oxide nano-cerium oxide exhibits inferior UV resistance and various mechanical properties compared to the ink obtained in Example 1. This may be because excessive UV absorber was added during the initial curing stage of the ink, affecting the photoinitiator's ability to fully absorb UV energy, resulting in incomplete resin crosslinking, reduced ink adhesion and solvent resistance, and cracking issues after prolonged exposure to UV light.
[0101] Although nano-cerium oxide and nano-zinc oxide were added to ink D2 obtained in Comparative Example 2, the nano-zinc oxide was not loaded into the mesoporous structure. This resulted in the addition of excessive ultraviolet absorber in the early stage of ink curing, which interfered with the normal excitation effect of photoinitiator, causing incomplete resin crosslinking and reducing the adhesion and solvent resistance of the ink after curing.
[0102] As can be seen from the two comparative examples above, nano-cerium oxide itself possesses excellent ultraviolet absorption capabilities. Its mesoporous structure can also store a portion of zinc oxide, preventing excessive ultraviolet absorbers in the ink system during the initial curing stage, which could adversely interfere with the excitation of the photoinitiator. In the later stages of ink curing, it uniformly releases zinc oxide particles, enhancing ultraviolet absorption and blocking. Both are indispensable and interact with each other. The mesoporous nano-cerium oxide and the loaded zinc oxide particles have a synergistic effect, achieving a technical effect that, while significantly improving the ink's UV resistance, also helps to improve the ink's mechanical properties—a feat unexpected by those skilled in the art.
[0103] In summary, the UV-resistant ink provided by this invention creatively employs mesoporous cerium oxide nanoparticles loaded with zinc oxide. While ensuring ink transmittance, it not only enhances the ink's absorption capacity for ultraviolet light but also increases the physical scattering effect of ultraviolet light, thereby significantly improving the ink's UV resistance. Simultaneously, it reduces the interference of ultraviolet absorbers on the photoinitiator during the early curing stage, increases the crosslinking density of the ink, and greatly enhances its mechanical properties. The preparation method provided by this invention is simple, environmentally friendly, and has broad application prospects.
[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A UV-resistant ink, characterized in that, The ink comprises: 2-10 parts of nano-cerium oxide, 20-30 parts of epoxy acrylic resin, 20-40 parts of polyester acrylic resin, 50-70 parts of acrylate, 0.5-2 parts of defoamer, 0.3-1.5 parts of dispersant, 1-1.5 parts of leveling agent, and 0.5-1 part of photoinitiator; The nano-cerium oxide has a mesoporous structure; The mesoporous structure of the nano-cerium oxide contains zinc oxide. The above components are listed in parts by mass.
2. The UV-resistant ink according to claim 1, characterized in that, The particle size of the nano-cerium oxide is 20nm-50nm.
3. The UV-resistant ink according to claim 1, characterized in that, The nano-cerium oxide is selected from virgin nano-cerium oxide and hydrophobically modified nano-cerium oxide.
4. The UV-resistant ink according to claim 1, characterized in that, The pore size of the mesoporous structure is 10nm-30nm.
5. The UV-resistant ink according to claim 1, characterized in that, The defoamer is selected from silicone defoamers and mineral oil defoamers; The dispersants were selected from BASF 4310 and KMT-3331; The leveling agent is selected from BYK-354, anjeka4330, and anjeka4420.
6. The UV-resistant ink according to claim 1, characterized in that, The photoinitiator is selected from 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone.
7. The method for preparing UV-resistant ink according to any one of claims 1-6, characterized in that, The preparation method includes the following steps: Step 1: Take 20-30 parts of epoxy acrylic resin, 20-40 parts of polyester acrylic resin, and 50-70 parts of acrylate and stir slowly until they are evenly mixed to obtain the first mixture. Step 2: Add 2-10 parts of zinc oxide-loaded nano-cerium oxide and 0.3-1.5 parts of dispersant to the first mixture in sequence, stir for 15-20 minutes to obtain the second mixture; Step 3: Add 0.5-2 parts of defoamer, 1-1.5 parts of leveling agent, and 0.5-1 parts of photoinitiator to the second mixture, and stir thoroughly to obtain UV-resistant ink.
8. The preparation method according to claim 7, characterized in that, The method for preparing zinc oxide-loaded nano-cerium oxide includes the following specific steps: Step A1: Keep the nano-cerium oxide in a negative pressure environment for 0.5-1h, and then continuously inject a 5%-15% zinc acetate solution into the nano-cerium oxide with a mesoporous structure, and immerse it under negative pressure for 1-2h. After taking it out, nano-cerium oxide particles loaded with zinc acetate are obtained. Step A2: The zinc acetate-loaded cerium oxide nanoparticles are baked at 250℃-300℃ for 1-2 hours to obtain the zinc oxide-loaded cerium oxide nanoparticles.
9. The preparation method according to claim 7, characterized in that, The nano-cerium oxide is hydrophobically modified nano-cerium oxide; The preparation steps of the hydrophobically modified nano-cerium oxide are as follows: Step B1: Dry the original nano-cerium oxide at 120°C under vacuum for 2 hours to obtain pretreated nano-cerium oxide; Step B2: Mix the silane coupling agent with anhydrous ethanol and deionized water at a mass ratio of (1-3):8:1 and adjust the pH to 4-5. Stir at room temperature for 20-30 minutes to obtain the first reaction suspension. Step B3: Prepare a 10% concentration suspension by mixing the pretreated nano-cerium oxide with anhydrous ethanol, then add it to the first reaction suspension, and stir continuously at 50℃-80℃ for 5-10 hours to obtain the second reaction suspension. The mass ratio of the added silane coupling agent to nano-cerium oxide is (3-10):100; Step B4: After centrifuging the second reaction suspension, the resulting filter residue is washed alternately with anhydrous ethanol and deionized water to obtain the hydrophobic modified nano-cerium oxide.
10. The preparation method according to claim 9, characterized in that, The silane coupling agent is selected from KH550, KH570, KH590, and vinyltrimethoxysilane.