An environmentally friendly low-temperature curing PVC anti-stone chip primer and its preparation method

By precisely matching PVC paste resin and chlorovinyl acetate copolymer resin and compounding with bio-based plasticizers, combined with nano/micro-sized calcium carbonate fillers and gradient cooling process, the problems of high-temperature curing, plasticizer migration and insufficient adhesion of PVC anti-stone chip coatings have been solved, achieving low-temperature curing and environmental protection.

CN123107465APending Publication Date: 2026-11-17SHANDONG YUANTENG NEW MATERIAL TECH CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611632428.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing PVC anti-stone impact vehicle underbody coatings suffer from problems such as high curing temperature, plasticizer migration and insufficient environmental friendliness, and poor adhesion to aluminum materials used in new energy vehicles. Furthermore, traditional preparation processes can easily lead to premature desealing and failure of cashew phenol-blocked isocyanates.

Method used

By precisely matching and compounding PVC paste resin and chloroacetic acid copolymer resin in a specific ratio, combined with the bio-based plasticizer epoxidized soybean oil and tributyl acetyl citrate, using nano/micro-sized calcium carbonate graded filler, and through gradient cooling process and vacuum filling and storage technology, the cashew phenol blocked isocyanate is effectively cross-linked at 120℃ to form a high-density coating.

Benefits of technology

It achieves complete curing at a low temperature of 120℃, and the coating has excellent mechanical properties and stone impact resistance. At the same time, it realizes the environmental protection of bio-based plasticizers and improves storage stability, thus solving the shortcomings of existing technologies.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

An environmentally friendly, low-temperature curing PVC anti-stone-impact primer and its preparation method are disclosed, belonging to the field of coating technology. The environmentally friendly, low-temperature curing PVC anti-stone-impact primer comprises the following components in parts by weight: 20-40 parts PVC paste resin; 5-10 parts vinyl acetate copolymer resin; 25-45 parts bio-based plasticizer; 1-8 parts cashew phenol blocked isocyanate; 0.5-5 parts heat stabilizer; 0.5-3 parts thixotropic agent; 15-40 parts filler; and 1-5 parts hygroscopic agent. The average degree of polymerization of the PVC paste resin is 1200-1800; the vinyl acetate content in the vinyl acetate copolymer resin is 14-18 wt%; and the mass ratio of the PVC paste resin to the vinyl acetate copolymer resin is (3-5):1. The coating of this invention can be cured at a low temperature of 120℃, possessing both excellent mechanical properties and anti-stone-impact properties, while simultaneously achieving environmental friendliness of the bio-based plasticizer and improved storage stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coating technology, specifically relating to an environmentally friendly low-temperature curing PVC anti-stone-impact primer and its preparation method. Background Technology

[0002] PVC anti-stone impact underbody coating is a type of solvent-free coating made primarily of polyvinyl chloride (PVC) resin, combined with plasticizers, fillers, and various additives. It is mainly used on the underbody and wheel arches of automobiles to provide chassis corrosion protection, stone impact resistance, vibration damping, and noise reduction.

[0003] Existing PVC anti-stone chip coatings for vehicle underbody typically use PVC paste resin as a matrix, which is plasticized with plasticizers and melted by heating to form a film. The curing temperature is generally above 140℃, which presents problems such as excessively high curing temperature, plasticizer migration, and insufficient environmental friendliness. Furthermore, existing solutions exhibit poor adhesion matching to different substrates (especially aluminum for new energy vehicles), and the preparation process easily leads to premature desealing and failure of cashew phenol-blocked isocyanates. Moreover, as the automotive industry moves towards lightweighting and energy conservation, the painting and baking line temperatures for some models can no longer reach 140℃. Developing low-temperature curing PVC anti-stone chip coatings with lower curing temperatures (e.g., around 120℃) has become a pressing technical challenge for the industry.

[0004] Chinese patent CN115851047B discloses a low-density anti-stone chip coating for aluminum car bodies. Its components include 10-25 parts PVC paste resin, 10-15 parts PVC blended resin, 1-5 parts epoxy cashew phenol-blocked isocyanate, 1-5 parts polyurethane cashew phenol-blocked isocyanate, 0.5-1 part thermally expandable microspheres, 25-50 parts filler, 15-30 parts plasticizer, and 3-5 parts hygroscopic agent. While this conventional solution achieves the basic functions of PVC anti-stone chip coatings, it still has the following shortcomings: the curing temperature is relatively high (usually above 140℃), which is not conducive to energy saving and consumption reduction; the plasticizer is mainly petroleum-based plasticizers such as dioctyl phthalate (DOP), which poses problems of plasticizer migration and environmental impact; the adhesion compatibility with different substrates (especially aluminum materials for new energy vehicles) is poor; and the conventional preparation process does not consider the temperature sensitivity of cashew phenol-blocked isocyanate, which can easily lead to premature desealing and failure.

[0005] In summary, the development of an environmentally friendly PVC anti-stone-impact primer that can be cured at a low temperature of 120℃ and possesses both excellent mechanical properties and stone-impact resistance, along with a preparation method that can prevent premature desealing of cashew phenol-blocked isocyanates, has significant practical application value. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the present invention aims to provide an environmentally friendly low-temperature curing PVC anti-stone-impact primer and its preparation method. The primer can be cured at a low temperature of 120°C, possesses excellent mechanical properties and anti-stone-impact properties, and simultaneously achieves environmental protection of bio-based plasticizers and improved storage stability.

[0007] To achieve the above objectives, according to one aspect of the present invention, an environmentally friendly low-temperature curing PVC anti-stone chip primer is provided, comprising the following components in parts by weight: 20-40 parts of PVC paste resin; 5-10 parts of vinyl acetate copolymer resin; 25-45 parts of bio-based plasticizer; 1-8 parts of cashew nut shell blocked isocyanate; 0.5-5 parts of heat stabilizer; 0.5-3 parts of thixotropic agent; 15-40 parts of filler; and 1-5 parts of hygroscopic agent; wherein the average degree of polymerization of the PVC paste resin is 1200-1800; the vinyl acetate content in the vinyl acetate copolymer resin is 14-18 wt%; and the mass ratio of the PVC paste resin to the vinyl acetate copolymer resin is (3-5):1.

[0008] In this invention, the average degree of polymerization of the PVC paste resin is 1200-1800, the vinyl acetate content in the chlorovinyl acetate copolymer resin is 14-18 wt%, and the mass ratio of the two is (3-5):1. In this process, the 14–18 wt% vinyl acetate segments in the vinyl acetate copolymer resin provide internal plasticizing, disrupting the regularity of the PVC molecular chains and reducing interchain polar forces, thereby lowering the plasticizing temperature of the system. Simultaneously, the PVC paste resin with a degree of polymerization of 1200–1800 forms a three-dimensional physical entanglement network with sufficiently long molecular chains, providing a mechanical framework for the coating and compensating for the strength loss in the vinyl acetate copolymer resin due to the increased vinyl acetate content. The two are compounded at a mass ratio of (3–5):1, ensuring that the flexible intervening effect of the vinyl acetate copolymer resin is just sufficient to open up the molecular chain network of the PVC paste resin, giving the chain segments free volume, without excessively damaging the network integrity. This allows the system to achieve complete plasticization at a low temperature of 120℃, precisely crossing the critical point of transition from the glassy to the rubbery state, while maintaining sufficient physical entanglement points to preserve mechanical strength. All three are indispensable, working together to achieve a synergistic unity between low-temperature plasticization and mechanical properties.

[0009] In this invention, the bio-based plasticizer is a mixture of epoxidized soybean oil and tributyl acetylglucosamine in a mass ratio of (1-3):(1-1.5). Epoxidized soybean oil provides epoxy groups, which undergo a cross-linking reaction with the isocyanate groups released after the deblocking of cashew phenol-blocked isocyanates during the low-temperature curing process, thereby increasing the cross-linking density and cohesive strength of the coating. Tributyl acetylglucosamine provides excellent low-temperature plasticizing efficiency, reducing the glass transition temperature of PVC resin. The two work synergistically in a specific ratio, enabling the coating to achieve complete plasticization at a low temperature of 120°C.

[0010] In this invention, the filler is a mixture of nano-calcium carbonate and heavy calcium carbonate in a mass ratio of (0.2~1.5):1; the average particle size of the nano-calcium carbonate is 20~100nm, and the average particle size of the heavy calcium carbonate is 1~10μm. The nano-calcium carbonate fills the voids between the heavy calcium carbonate particles, forming a graded filling structure, significantly improving the density and stone-impact resistance of the coating; simultaneously, the high specific surface area of ​​the nano-calcium carbonate can adsorb bio-based plasticizers, effectively inhibiting the migration and precipitation of plasticizers during long-term use of the coating, thus providing the coating with stone-impact resistance.

[0011] In this invention, the cashew nut shell phenol-blocked isocyanate has a blocking rate of 90-95% based on the initial molar number of isocyanate groups. The cashew nut shell phenol-blocked isocyanate deblocks and releases isocyanate groups at 120°C. This application precisely matches the deblocking temperature of the cashew nut shell phenol-blocked isocyanate with the curing temperature of the coating, ensuring that the cashew nut shell phenol-blocked isocyanate deblocks and functions precisely during curing, while remaining blocked during storage. The released isocyanate groups form chemical bonds with active hydrogen groups on the substrate surface, and simultaneously undergo cross-linking reactions with polar groups in the vinyl chloride copolymer resin and epoxy groups in epoxidized soybean oil, significantly improving the adhesion between the coating and the substrate and the cohesive strength of the coating. Cashew nut shell phenol is bio-based, replacing the traditional nonylphenol blocker, thus achieving environmental friendliness.

[0012] The cashew phenol-blocked isocyanate of this invention can be prepared using the following general method: Under nitrogen protection, cashew phenol (preferably Cardolite NX-2026, hydroxyl value 180-195 mg KOH / g) and an organic solvent are added to a reaction vessel equipped with a mechanical stirrer, thermometer, and reflux condenser, and stirred until the cashew phenol is completely dissolved. The temperature is raised to 60-65°C, a catalyst is added, and then isocyanate is slowly added dropwise, controlling the molar ratio of phenolic hydroxyl groups to isocyanate groups (-NCO) to be (1.1-1.3):1. After the addition is complete, the reaction is maintained at reflux, and samples are taken every hour. The residual -NCO content in the system is determined by di-n-butylamine titration. The blocking rate is calculated using the following formula: Closure rate (%) = (1 - residual NCO moles / initial NCO moles) × 100%; After the reaction is complete, the organic solvent is removed by vacuum distillation at 45-50℃, and then the free TDI is removed by thin-film evaporation at 60℃ under high vacuum. After cooling to room temperature, a yellow viscous liquid is obtained, which is cashew phenol blocked isocyanate.

[0013] The organic solvent is selected from one or more of ethyl acetate, butyl acetate, acetone, and butanone, preferably ethyl acetate. The catalyst is selected from one of stannous octoate, dibutyltin dilaurate (DBTDL), and DABCO T12, and is used in an amount of 0.05 to 0.2 wt% of the isocyanate mass.

[0014] In this invention, the heat stabilizer is a calcium-zinc composite heat stabilizer; the thixotropic agent is organobentonite; and the hygroscopic agent is calcium oxide. This application systematically integrates this with a specific resin system, a specific plasticizer compound system, and cashew nut shell blocked isocyanate. In particular, calcium oxide, as a hygroscopic agent, absorbs trace amounts of moisture in the system, preventing the cashew nut shell blocked isocyanate from prematurely degrading due to hydrolysis during storage, thus achieving a synergistic effect of storage protection.

[0015] According to another aspect of the present invention, a method for preparing an environmentally friendly low-temperature curing PVC anti-stone chip primer is also provided, comprising the following steps: (1) Add the formulated amount of bio-based plasticizer and heat stabilizer to the dispersion vessel, heat to 80-95℃, add PVC paste resin and chlorinated vinyl acetate copolymer resin under stirring conditions, disperse evenly, and obtain resin premix; (2) Cool the resin premix to 50-70°C, add thixotropic agent, filler and hygroscopic agent to it, and stir and disperse at 1000-2000 rpm for 30-60 minutes to obtain a mixture; (3) Cool the mixture to 25-45°C, add cashew phenol blocked isocyanate, stir at 500-1000 rpm for 10-30 minutes, then degas under vacuum for 15-40 minutes, filter and discharge to obtain the environmentally friendly low-temperature curing PVC anti-stone chip primer.

[0016] In this invention, the stirring speed in step (1) is 500 to 1500 rpm; the filler in step (2) is added in 2 to 3 batches, with an interval of 5 to 10 minutes between adjacent batches.

[0017] In this invention, the bio-based plasticizer in step (1) is a compound of epoxidized soybean oil and acetylated tributyl citrate. The epoxidized soybean oil, acetylated tributyl citrate and the heat stabilizer are mixed evenly at 40-60°C before being added to the dispersion tank.

[0018] In this invention, the PVC paste resin and chloroacetic acid copolymer resin mentioned in step (1) are added as follows: first, add 1 / 2 of the formula amount of PVC paste resin, stir for 5 to 10 minutes, then add all of the chloroacetic acid copolymer resin, stir for 5 to 10 minutes, and then add the remaining 1 / 2 of the PVC paste resin.

[0019] In this invention, after step (3), the process further includes filling the filtered coating material into a sealed container under vacuum conditions, filling it with nitrogen for protection, and storing it at 0-10°C.

[0020] This application designs segmented temperature zones to address the heat sensitivity of different components: a high-temperature zone (80–95°C) promotes plasticizer penetration into resin particles; a medium-temperature zone (50–70°C) ensures uniform dispersion of fillers; and a low-temperature zone (25–45°C) ensures that cashew nut shell blocked isocyanate does not prematurely deblock. This three-zone gradient cooling design optimizes process conditions for the heat sensitivity and dispersion requirements of different components, ensuring both sufficient resin swelling and uniform filler dispersion, while preventing premature deblocking of the cashew nut shell blocked isocyanate during preparation. This ensures the effectiveness of the cashew nut shell blocked isocyanate and the storage stability of the coating.

[0021] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention provides an environmentally friendly low-temperature curing PVC anti-stone-impact primer. By precisely matching the degree of polymerization of PVC paste resin with the vinyl acetate content in the chlorovinyl acetate copolymer resin and synergistically adjusting their mass ratio, combined with a compound plasticizer of epoxidized soybean oil and tributyl acetyl citrate, cashew phenol blocked isocyanate, and nano / micron-sized calcium carbonate graded filler, the coating can be fully cured and formed by baking at a low temperature of 120℃. The coating has both excellent mechanical properties and anti-stone-impact properties, while achieving environmental protection of bio-based plasticizers and improving storage stability. It effectively solves the technical problems of existing PVC anti-stone-impact coatings, such as high curing temperature, plasticizer migration, and insufficient adhesion.

[0022] 2. This invention also provides a method for preparing the coating, which employs a three-stage temperature gradient cooling process involving high-temperature resin dispersion at 80-95℃, medium-temperature filler dispersion at 50-70℃, and low-temperature addition of cashew phenol-blocked isocyanate at 25-45℃. Combined with batch addition of filler and segmented feeding of PVC paste resin, this method avoids filler agglomeration and premature desealing and failure of cashew phenol-blocked isocyanate during preparation. Furthermore, the post-treatment process of vacuum filling, nitrogen protection, and low-temperature storage at 0-10℃ effectively extends the coating's shelf life to more than 6 months, ensuring product storage stability. Detailed Implementation

[0023] To enable those skilled in the art to understand the features and effects of the present invention, the following description and definitions are only general descriptions of the terms and expressions mentioned in the specification. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0024] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0025] In this document, when describing embodiments or examples, it should be understood that it is not intended to limit the invention to those embodiments or examples.

[0026] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0027] This invention provides an environmentally friendly low-temperature curing PVC anti-stone chip primer, comprising the following components in parts by weight: 20-40 parts PVC paste resin; 5-10 parts vinyl acetate copolymer resin; 25-45 parts bio-based plasticizer; 1-8 parts cashew phenol blocked isocyanate; 0.5-5 parts heat stabilizer; 0.5-3 parts thixotropic agent; 15-40 parts filler; and 1-5 parts hygroscopic agent. The PVC paste resin has an average degree of polymerization of 1200-1800; the vinyl acetate content in the vinyl acetate copolymer resin is 14-18 wt%; and the mass ratio of the PVC paste resin to the vinyl acetate copolymer resin is (3-5):1.

[0028] In some embodiments, the bio-based plasticizer is a mixture of epoxidized soybean oil and tributyl acetyl citrate in a mass ratio of (1-3):(1-1.5).

[0029] In some embodiments, the filler is a mixture of nano-calcium carbonate and heavy calcium carbonate in a mass ratio of (0.2~1.5):1; the average particle size of the nano-calcium carbonate is 20~100nm, and the average particle size of the heavy calcium carbonate is 1~10μm.

[0030] In some embodiments, the isocyanate blocking rate of the cashew phenol blocked isocyanate is 90-95% based on the initial molar number of isocyanate groups, and the cashew phenol blocked isocyanate is deblocked and releases isocyanate groups at 120°C.

[0031] In some embodiments, the heat stabilizer is a calcium-zinc composite heat stabilizer; the thixotropic agent is organobentonite; and the hygroscopic agent is calcium oxide.

[0032] The present invention also provides a method for preparing an environmentally friendly low-temperature curing PVC anti-stone chip primer according to any one of the above claims, comprising the following steps: (1) Add the formulated amount of bio-based plasticizer and heat stabilizer to the dispersion vessel, heat to 80-95℃, add PVC paste resin and chlorinated vinyl acetate copolymer resin under stirring conditions, disperse evenly, and obtain resin premix; (2) Cool the resin premix to 50-70°C, and add thixotropic agent, filler and hygroscopic agent to it, and stir and disperse at 1000-2000 rpm for 30-60 minutes to obtain a mixture; (3) Cool the mixture to 25-45°C, add cashew phenol blocked isocyanate, stir at 500-1000 rpm for 10-30 minutes, then degas under vacuum for 15-40 minutes, filter and discharge to obtain the environmentally friendly low-temperature curing PVC anti-stone chip primer.

[0033] In some embodiments, the stirring speed in step (1) is 500 to 1500 rpm; the filler in step (2) is added in 2 to 3 batches, with an interval of 5 to 10 minutes between adjacent batches.

[0034] In some embodiments, the bio-based plasticizer in step (1) is a compound of epoxidized soybean oil and acetylated tributyl citrate, wherein the epoxidized soybean oil, acetylated tributyl citrate and the heat stabilizer are mixed evenly at 40-60°C before being added to the dispersion tank.

[0035] In some embodiments, the PVC paste resin and chloroacetic acid copolymer resin in step (1) are added as follows: first, add 1 / 2 of the PVC paste resin according to the formula, stir for 5 to 10 minutes, then add all of the chloroacetic acid copolymer resin, stir for 5 to 10 minutes, and then add the remaining 1 / 2 of the PVC paste resin.

[0036] In some embodiments, step (3) is followed by filling the filtered coating into a sealed container under vacuum conditions, filling it with nitrogen for protection, and storing it at 0 to 10°C.

[0037] The present invention will be described in detail below through embodiments. It should be understood that the following embodiments are only used to further explain and illustrate the content of the present invention by way of example, and are not intended to limit the present invention.

[0038] Example 1 is the best embodiment.

[0039] The chemical additives used in the embodiments and comparative examples of this invention are all commercially available, and the specific information is as follows: PVC paste resin: purchased from Henan Fengbai Industrial Co., Ltd.; Chloride-vinyl acetate copolymer resin: purchased from Kunshan Tongfuxin New Material Technology Co., Ltd.; Cashew phenol: purchased from Shandong Longhui Chemical Co., Ltd.; TDI: purchased from Wanhua Chemical; Calcium-zinc composite heat stabilizer: purchased from Jiangsu Pangrui New Material Co., Ltd.; Organic bentonite: purchased from Zhejiang Hongyu New Material Co., Ltd.; Epoxidized soybean oil: purchased from Zibo Jinghe Biotechnology Co., Ltd.; Ethyl acetate, DBTDL catalyst, Stannous octoate, Tributyl acetylacetic acid: purchased from Aladdin Reagent Co., Ltd.; Nano calcium carbonate, Heavy calcium carbonate: purchased from Zhejiang Tianshi Nanotechnology Co., Ltd.

[0040] Preparation Example 1 Under nitrogen protection, 50.0 g of cashew nut phenol and 32 mL of ethyl acetate were added to a three-necked reactor equipped with a mechanical stirrer, thermometer, and reflux condenser. The mixture was stirred until the cashew nut phenol was completely dissolved. The temperature was raised to 60°C, and 0.012 g of DBTDL catalyst was added. 12.20 g of TDI was slowly added dropwise over 30 minutes through a dropping funnel. After the addition was complete, the mixture was kept at 60°C under reflux for the reaction. During the reaction, samples were taken every hour, and the residual -NCO content in the system was determined by di-n-butylamine titration. The initial -NCO molar number was calculated based on the TDI feed amount. When the titration results showed that the residual -NCO molar number dropped to 10% of the initial value, the reaction system was immediately cooled to room temperature to terminate the reaction. Ethyl acetate was removed by distillation at 48°C under reduced pressure, and free TDI was removed by thin-film evaporation at 80°C under high vacuum. After cooling to room temperature, a yellow viscous liquid was obtained, namely cashew phenol blocked isocyanate A. The reaction endpoint blocking rate was 90%, and the free TDI content in the final product was ≤0.1 wt%.

[0041] Preparation Example 2 Under nitrogen protection, 50.0 g of cashew phenol and 32 mL of ethyl acetate were added to the reaction vessel and stirred until the cashew phenol was completely dissolved. The temperature was raised to 65°C, and 0.012 g of stannous octoate catalyst was added. 11.52 g of TDI was slowly added dropwise over 40 minutes through a dropping funnel. After the addition was completed, the reaction was maintained at 60°C under reflux. Samples were taken every hour during the reaction, and the residual -NCO content was determined by di-n-butylamine titration. The initial -NCO molar number was calculated based on the TDI feed amount. When the titration results showed that the residual -NCO molar number dropped to 5% of the initial value, the reaction system was cooled to room temperature to terminate the reaction. Ethyl acetate was removed by distillation at 48°C under reduced pressure, and free TDI was removed by thin-film evaporation at 60°C under high vacuum. After cooling to room temperature, a yellow viscous liquid was obtained, namely cashew phenol blocked isocyanate B. The reaction endpoint blocking rate was 95%, and the free TDI content in the final product was ≤0.1 wt%.

[0042] Preparation Example 3 Under nitrogen protection, 50.0 g of cashew nut phenol and 32 mL of ethyl acetate were added to a three-necked reactor equipped with a mechanical stirrer, thermometer, and reflux condenser. The mixture was stirred until the cashew nut phenol was completely dissolved. The temperature was raised to 60°C, and 0.012 g of DBTDL catalyst was added. 12.20 g of TDI was slowly added dropwise over 30 minutes through a dropping funnel. After the addition was complete, the mixture was kept at 60°C under reflux for the reaction. During the reaction, samples were taken every hour, and the residual -NCO content in the system was determined by di-n-butylamine titration. The initial -NCO molar number was calculated based on the TDI feed amount. When the titration results showed that the residual -NCO molar number dropped to 15% of the initial value, the reaction system was immediately cooled to room temperature to terminate the reaction. Ethyl acetate was removed by distillation at 48°C under reduced pressure, and free TDI was removed by thin-film evaporation at 60°C under high vacuum. After cooling to room temperature, a yellow viscous liquid was obtained, namely cashew phenol blocked isocyanate C. The blocking rate at the reaction endpoint was 85%, and the free TDI content in the final product was ≤0.1 wt%.

[0043] Example 1 This embodiment describes an environmentally friendly low-temperature curing PVC anti-stone chip primer, comprising the following components by weight: 20 parts PVC paste resin (average degree of polymerization 1500); 5 parts vinyl chloride-vinyl acetate copolymer resin (vinyl acetate content 16wt%); 30 parts bio-based plasticizer; 4 parts cashew phenol blocked isocyanate B; 2.5 parts calcium-zinc composite heat stabilizer; 1.5 parts organic bentonite; 30 parts filler; and 3 parts calcium oxide. The bio-based plasticizer is a mixture of epoxidized soybean oil and tributyl acetylacetonate in a mass ratio of 3:1.5. The filler is nano-calcium carbonate (average particle size 50nm) and heavy calcium carbonate (average particle size 5μm) in a mass ratio of 3:2. The preparation method of the environmentally friendly low-temperature curing PVC anti-stone chip primer described in this embodiment includes the following steps: (1) Mix 20 parts of epoxidized soybean oil with 10 parts of acetylated tributyl citrate and 2.5 parts of calcium-zinc composite heat stabilizer at 50°C for 15 minutes until uniform, add to a dispersion vessel, heat to 85°C, add 10 parts of PVC paste resin under stirring at 1000 rpm, stir for 8 minutes, add 5 parts of chloroacetic acid copolymer resin, stir for 8 minutes, add the remaining 10 parts of PVC paste resin, continue stirring and dispersing for 20 minutes after the addition is complete to obtain resin premix; (2) Cool the resin premix to 60°C, add 1.5 parts of organic bentonite, 3 parts of calcium oxide, and 18 parts of nano calcium carbonate and 12 parts of heavy calcium carbonate added in 3 batches (with an 8-minute interval between adjacent batches), and stir and disperse at 1500 rpm for 45 minutes to obtain the mixture. (3) Cool the mixture to 35°C, add 4 parts of cashew phenol blocked isocyanate B, stir at 800 rpm for 20 minutes, then degas at -0.09 MPa vacuum for 30 minutes, filter out the material, and obtain the environmentally friendly low-temperature curing PVC anti-stone chip primer coating. (4) Fill the filtered coating material into a sealed container under vacuum conditions, fill it with nitrogen for protection, and store it at 5°C.

[0044] Example 2 This embodiment provides an environmentally friendly low-temperature curing PVC anti-stone chip primer, comprising the following components by weight: 30 parts PVC paste resin (average degree of polymerization 1200); 10 parts vinyl chloride-vinyl acetate copolymer resin (vinyl acetate content 14wt%); 25 parts bio-based plasticizer; 1 part cashew phenol blocked isocyanate A; 0.5 parts calcium-zinc composite heat stabilizer; 0.5 parts organic bentonite; 15 parts filler; and 1 part calcium oxide. The bio-based plasticizer is a mixture of epoxidized soybean oil and acetylated tributyl citrate in a 1:1 mass ratio, i.e., 12.5 parts epoxidized soybean oil and 12.5 parts acetylated tributyl citrate. The filler is nano-calcium carbonate (average particle size 20nm) and heavy calcium carbonate (average particle size 1μm) in a 0.2:1 mass ratio, i.e., 2.5 parts nano-calcium carbonate and 12.5 parts heavy calcium carbonate. The preparation method of the environmentally friendly low-temperature curing PVC anti-stone chip primer described in this embodiment includes the following steps: (1) 12.5 parts of epoxidized soybean oil, 12.5 parts of acetylated tributyl citrate and 0.5 parts of calcium-zinc composite heat stabilizer were stirred and mixed at 40°C for 15 minutes until uniform. The mixture was added to a dispersion vessel and heated to 80°C. 15 parts of PVC paste resin were added first under stirring at 500 rpm. After stirring for 5 minutes, 10 parts of chloroacetic acid copolymer resin were added. After stirring for 5 minutes, the remaining 15 parts of PVC paste resin were added. After the addition was completed, stirring and dispersing continued for 20 minutes to obtain the resin premix. (2) Cool the resin premix to 50°C, add 0.5 parts of organic bentonite, 1 part of calcium oxide, and 2.5 parts of nano calcium carbonate and 12.5 parts of heavy calcium carbonate added in two batches (with an interval of 5 minutes between adjacent batches), and stir and disperse at 1000 rpm for 30 minutes to obtain the mixture. (3) Cool the mixture to 25°C, add 1 part of cashew phenol blocked isocyanate A, stir for 10 minutes at 500 rpm, then degas for 15 minutes under a vacuum of -0.08 MPa, filter out the material, and you will get an environmentally friendly low-temperature curing PVC anti-stone chip primer. (4) Fill the filtered coating into a sealed container under vacuum, fill it with nitrogen for protection, and store it at 0°C.

[0045] Example 3 This embodiment describes an environmentally friendly low-temperature curing PVC anti-stone chip primer, comprising the following components by weight: 40 parts PVC paste resin (average degree of polymerization 1800); 8 parts vinyl chloride-vinyl acetate copolymer resin (vinyl acetate content 18wt%); 45 parts bio-based plasticizer; 8 parts cashew phenol blocked isocyanate B; 5 parts calcium-zinc composite heat stabilizer; 3 parts organic bentonite; 40 parts filler; and 5 parts calcium oxide. The bio-based plasticizer is a mixture of epoxidized soybean oil and acetylated tributyl citrate in a mass ratio of 3:1, i.e., 33.75 parts epoxidized soybean oil and 11.25 parts acetylated tributyl citrate. The filler is nano-calcium carbonate (average particle size 100nm) and heavy calcium carbonate (average particle size 10μm) in a mass ratio of 17:23, i.e., 17 parts nano-calcium carbonate and 23 parts heavy calcium carbonate. The preparation method of the environmentally friendly low-temperature curing PVC anti-stone chip primer described in this embodiment includes the following steps: (1) Mix 33.75 parts of epoxidized soybean oil with 11.25 parts of acetylated tributyl citrate and 5 parts of calcium-zinc composite heat stabilizer at 60°C for 15 minutes until uniform, add to a dispersion vessel, heat to 95°C, add 20 parts of PVC paste resin under stirring at 1500 rpm, stir for 10 minutes, add 8 parts of chloroacetic acid copolymer resin, stir for 10 minutes, add the remaining 20 parts of PVC paste resin, continue stirring and dispersing for 20 minutes after the addition is complete to obtain resin premix; (2) Cool the resin premix to 70°C, add 3 parts organic bentonite, 5 parts calcium oxide, and 17 parts nano calcium carbonate and 23 parts heavy calcium carbonate added in 3 batches (with an interval of 10 minutes between adjacent batches), stir and disperse at 2000 rpm for 60 minutes to obtain the mixture. (3) Cool the mixture to 45°C, add 8 parts of cashew phenol blocked isocyanate B, stir at 1000 rpm for 30 minutes, then degas at -0.1 MPa vacuum for 40 minutes, filter out the material, and obtain the environmentally friendly low-temperature curing PVC anti-stone chip primer coating. (4) Fill the filtered coating into a sealed container under vacuum, fill it with nitrogen for protection, and store it at 10°C.

[0046] Comparative Example 1 The environmentally friendly low-temperature curing PVC anti-stone-impact primer described in this comparative example is exactly the same as that in Example 1, except that the average degree of polymerization of the PVC paste resin is 2000.

[0047] Comparative Example 2 The environmentally friendly low-temperature curing PVC anti-stone chip primer described in this comparative example is exactly the same as that in Example 1, except that the vinyl acetate content in the chlorovinyl acetate copolymer resin is 12wt%.

[0048] Comparative Example 3 The environmentally friendly low-temperature curing PVC anti-stone chip primer described in this comparative example is exactly the same as that in Example 1, except that the vinyl acetate content in the chlorovinyl acetate copolymer resin is 20wt%.

[0049] Comparative Example 4 The environmentally friendly low-temperature curing PVC anti-stone-impact primer described in this comparative example is exactly the same as that in Example 1, except that the mass ratio of PVC paste resin to chloroacetic acid copolymer resin is 6:1, that is, 30 parts of PVC paste resin and 5 parts of chloroacetic acid copolymer resin.

[0050] Comparative Example 5 The environmentally friendly low-temperature curing PVC anti-stone chip primer described in this comparative example is exactly the same as that in Example 1, except that the mass ratio of PVC paste resin to chloroacetic acid copolymer resin is 2:1, that is, 20 parts of PVC paste resin and 10 parts of chloroacetic acid copolymer resin.

[0051] Comparative Example 6 The method for an environmentally friendly low-temperature curing PVC anti-stone chip primer described in this comparative example differs only in that ordinary epoxy resin blocked isocyanate is used instead of cashew phenol blocked isocyanate B.

[0052] Comparative Example 7 The method for producing an environmentally friendly low-temperature curing PVC anti-stone chip primer described in this comparative example differs only in that cashew phenol-blocked isocyanate C with a blocking rate of 85% is used instead of cashew phenol-blocked isocyanate B.

[0053] Performance testing The environmentally friendly low-temperature curing PVC anti-stone chip primers obtained in the examples and comparative examples were tested for performance using the following methods, and the specific results are shown in Table 1.

[0054] Tensile strength and elongation at break: determined according to GB / T 528-2009. The coating was baked at 120℃ for 30 minutes to prepare dumbbell-shaped specimens with a thickness of 2 mm. The specimens were tested using a universal testing machine at a tensile rate of 200 mm / min, and the tensile strength and elongation at break of the specimens were recorded.

[0055] Adhesion: The adhesion was determined according to GB / T 5210-2006 "Paints and Varnishes - Pull-off Adhesion Test". The coating was sprayed onto a phosphated aluminum plate and cured by baking at 120°C for 30 minutes. The adhesion was then measured using a pull-off adhesion tester, and the force (MPa) required to pull the coating off the substrate was recorded.

[0056] Stone impact resistance: Tested according to SAE J400 standard. The coating was sprayed onto a standard test panel and cured by baking at 120°C for 30 minutes. The sample was then pretreated for 48 hours at (23±2)°C and (50±5)% relative humidity. Using a stone impact tester, 500g of angular steel shot (Type I) was sprayed onto the coating surface at approximately 100 mph under 480 kPa pressure. After testing, loose coating was removed with tape and graded according to SAE J400 standard (1–10, with 10 being the best, indicating no breakage; 6 and above are acceptable).

[0057] Applicability: The prepared coating is sealed and stored at 0-10℃. Periodically, a sample is taken from one container and individually packaged. After being warmed to a constant temperature of 23±2℃ for 2 hours, the viscosity is measured using a rotational viscometer with a suitable rotor at 23±2℃ and 20 r / min. The reading is taken 1 minute after stabilization. The initial viscosity is the viscosity measured after 24 hours at 23±2℃. The longest storage time during which the coating viscosity increase does not exceed 20% of the initial viscosity is defined as the pot life.

[0058] Plasticizer migration rate: determined according to ISO 176 standard (Plastics - Determination of loss of plasticizers - Activated carbon method). The coating was baked at 120°C for 30 minutes to prepare circular samples with a diameter of 50 mm and a thickness of 2 mm, and the initial mass (m0) was recorded. The sample was then completely covered with granular activated carbon and placed at 70°C for 24 hours. After removal and cooling to room temperature, the surface activated carbon particles were brushed off, and the final mass (m1) was recorded.

[0059] Plasticizer migration rate is calculated using the following formula: Mobility (%) = (m0 - m1) / m0 × 100%; The lower the migration rate, the better the plasticizer migration resistance of the coating.

[0060] Table 1 Performance data of Examples 1-3 and Comparative Examples 1-7 .

[0061] As shown in Table 1, the coatings of Examples 1-3 of this invention exhibit excellent tensile strength, elongation at break, adhesion, and stone impact resistance under low-temperature curing conditions of 120℃×30min, along with a long pot life and low plasticizer migration rate. This indicates that the present invention, through precise matching of the degree of polymerization of PVC paste resin and the content of vinyl acetate in chloroacetic acid copolymer resin and the synergistic effect of their mass ratio, combined with a bio-based plasticizer compound system and cashew phenol blocked isocyanate, can achieve complete curing at a low temperature of 120℃. This results in coatings with excellent mechanical strength, flexibility, adhesion, and stone impact resistance, while also achieving environmental friendliness and improved storage stability. It effectively solves the technical problems of existing PVC anti-stone impact coatings, such as excessively high curing temperature, plasticizer migration, and insufficient adhesion.

[0062] A comparison of Example 1 and Comparative Example 1 shows that the only difference between Comparative Example 1 and Example 1 is that the degree of polymerization of the PVC paste resin is 2000. After curing at 120℃ for 30 minutes, the coating's tensile strength, elongation at break, adhesion, and stone chip resistance decreased, while the plasticizer migration rate increased. This indicates that excessive polymerization leads to excessively long molecular chains, making chain segment movement difficult and plasticization incomplete at the low temperature of 120℃. The resulting coating is brittle, hard, and prone to cracking, with significantly deteriorated mechanical properties and stone chip resistance.

[0063] A comparison of Example 1 and Comparative Example 2 shows that the only difference between Comparative Example 2 and Example 1 is that the vinyl acetate content in the vinyl chloride-vinyl acetate copolymer resin is 12 wt%. After curing at 120℃ for 30 min, the coating's tensile strength, elongation at break, adhesion, and stone impact resistance decreased. This indicates that the low vinyl acetate content leads to insufficient internal plasticizing, inadequate plasticization of the system at 120℃, and a significant decrease in the coating's flexibility and stone impact resistance.

[0064] A comparison of Example 1 and Comparative Example 3 shows that the only difference between Comparative Example 3 and Example 1 is that the vinyl acetate content in the chlorovinyl acetate copolymer resin is 20 wt%. After curing at 120℃ for 30 min, the elongation at break increased, but the tensile strength and adhesion were severely deteriorated, and the plasticizer migration rate increased significantly. This indicates that although a high vinyl acetate content can improve flexibility, it disrupts the physical entanglement network of PVC molecular chains, leading to a significant decrease in the cohesive strength and interfacial bonding of the coating.

[0065] A comparison of Example 1 and Comparative Example 4 shows that the only difference between Comparative Example 4 and Example 1 is that the mass ratio of PVC paste resin to chloroacetic acid copolymer resin is 6:1. After curing at 120℃ for 30 minutes, the excessively high mass ratio resulted in insufficient internal plasticizing. Some plasticizers failed to fully swell and enter the resin network, remaining in a free state, leading to increased migration rate, decreased tensile strength, decreased elongation at break, and decreased stone chip resistance.

[0066] A comparison of Example 1 and Comparative Example 5 shows that the only difference between Comparative Example 5 and Example 1 is the mass ratio of PVC paste resin to chloroacetic acid copolymer resin, which is 2:1. After curing at 120℃ for 30 minutes, the elongation at break increased, while the tensile strength, adhesion, and stone chip resistance of the coating decreased, and the plasticizer migration rate increased. This indicates that an excessively high proportion of chloroacetic acid copolymer resin leads to an excessively large proportion of the chloroacetic acid resin component in the system. Its relatively low molecular weight disrupts the mechanical network formed by the long chains of PVC paste resin. Although the glass transition temperature of the system decreases, the network integrity is damaged, resulting in insufficient strength in the coating macroscopically, with a significant decrease in tensile strength and stone chip resistance, and an increased plasticizer migration rate.

[0067] A comparison of Example 1 and Comparative Example 6 shows that the only difference between Comparative Example 6 and Example 1 is the use of ordinary epoxy resin blocked isocyanate instead of cashew phenol blocked isocyanate. After curing at 120℃ for 30 min, the coating exhibited low tensile strength and elongation at break, poor adhesion, poor stone chip resistance, short pot life, and high plasticizer migration. This indicates that ordinary epoxy resin blocked isocyanate has low reactivity at the low temperature of 120℃, failing to form sufficient chemical bonds with the substrate, resulting in a significant decrease in adhesion. Simultaneously, the poor compatibility between epoxy resin and plasticizer disrupts the compatibility balance between the plasticizer and PVC resin, making the plasticizer more prone to migration and precipitation, thus shortening the pot life. This demonstrates that cashew phenol blocked isocyanate has a significantly better adhesion-promoting effect than ordinary epoxy resin blocked isocyanate under low-temperature curing conditions.

[0068] A comparison of Example 1 and Comparative Example 7 shows that the only difference between Comparative Example 7 and Example 1 is the use of cashew phenol-blocked isocyanate C with a blocking rate of 85%. The pot life is shortened, and tensile strength, elongation at break, adhesion, and stone chip resistance decrease, while migration increases. This is because the blocking rate is too low, resulting in excessive residual unblocked -NCO, which easily reacts with trace amounts of moisture during storage, leading to a shortened pot life; during curing, the unblocking and crosslinking are mismatched, resulting in uneven crosslinking and decreased coating cohesive strength and interfacial adhesion.

[0069] Therefore, this invention creatively provides an environmentally friendly low-temperature curing PVC anti-stone-impact primer. By precisely matching the degree of polymerization of PVC paste resin with the vinyl acetate content in the chlorovinyl acetate copolymer resin and synergistically adjusting their mass ratio, combined with a compound plasticizer of epoxidized soybean oil and tributyl acetyl citrate, cashew phenol blocked isocyanate, and nano / micron-sized calcium carbonate graded filler, the coating can be completely cured and formed by baking at a low temperature of 120℃. The coating has both excellent mechanical properties and anti-stone-impact properties, while achieving environmental protection of bio-based plasticizers and improving storage stability. It effectively solves the technical problems of existing PVC anti-stone-impact coatings, such as high curing temperature, plasticizer migration, and insufficient adhesion.

[0070] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. For those skilled in the art, other variations or modifications can be made based on the above description. It is impossible to exhaustively list all the implementation methods here. All obvious variations or modifications derived from the technical solutions of the present invention are still within the protection scope of the present invention.

Claims

1. An environmentally friendly low-temperature curing PVC anti-stone chip primer coating, characterized in that, The product comprises the following components in parts by weight: 20-40 parts PVC paste resin; 5-10 parts chlorovinyl acetate copolymer resin; 25-45 parts bio-based plasticizer; 1-8 parts cashew nut shell blocked isocyanate; 0.5-5 parts heat stabilizer; 0.5-3 parts thixotropic agent; 15-40 parts filler; and 1-5 parts hygroscopic agent. The PVC paste resin has an average degree of polymerization of 1200-1800; the chlorovinyl acetate copolymer resin contains 14-18 wt% vinyl acetate; and the mass ratio of the PVC paste resin to the chlorovinyl acetate copolymer resin is (3-5):

1.

2. The environmentally friendly low-temperature curing PVC anti-stone-impact primer coating according to claim 1, characterized in that, The bio-based plasticizer is a mixture of epoxidized soybean oil and tributyl acetylglucosamine in a mass ratio of (1-3):(1-1.5).

3. The environmentally friendly low-temperature curing PVC anti-stone-impact primer coating according to claim 1, characterized in that, The filler is composed of nano-calcium carbonate and heavy calcium carbonate in a mass ratio of (0.2~1.5):1; the average particle size of the nano-calcium carbonate is 20~100nm, and the average particle size of the heavy calcium carbonate is 1~10μm.

4. The environmentally friendly low-temperature curing PVC anti-stone-impact primer coating according to claim 1, characterized in that: In the cashew phenol blocked isocyanate, the isocyanate group blocking rate is 90-95% based on the initial molar number of isocyanate groups, and the cashew phenol blocked isocyanate releases isocyanate groups at 120°C.

5. The environmentally friendly low-temperature curing PVC anti-stone-impact primer coating according to claim 1, characterized in that, The heat stabilizer is a calcium-zinc composite heat stabilizer; the thixotropic agent is organic bentonite; and the hygroscopic agent is calcium oxide.

6. A method for preparing an environmentally friendly low-temperature curing PVC anti-stone chip primer according to any one of claims 1 to 5, characterized in that, Includes the following steps: (1) Add the formulated amount of bio-based plasticizer and heat stabilizer to the dispersion vessel, heat to 80-95℃, add PVC paste resin and chlorinated vinyl acetate copolymer resin under stirring conditions, disperse evenly, and obtain resin premix; (2) Cool the resin premix to 50-70°C, add thixotropic agent, filler and hygroscopic agent to it, and stir and disperse at 1000-2000 rpm for 30-60 minutes to obtain a mixture; (3) Cool the mixture to 25-45°C, add cashew phenol blocked isocyanate, stir at 500-1000 rpm for 10-30 minutes, then degas under vacuum for 15-40 minutes, filter and discharge to obtain the environmentally friendly low-temperature curing PVC anti-stone chip primer.

7. The preparation method of the environmentally friendly low-temperature curing PVC anti-stone-impact primer according to claim 6, characterized in that, The stirring speed in step (1) is 500 to 1500 rpm; the filler in step (2) is added in 2 to 3 batches, with an interval of 5 to 10 minutes between adjacent batches.

8. The preparation method of the environmentally friendly low-temperature curing PVC anti-stone chip primer according to claim 6, characterized in that, The bio-based plasticizer mentioned in step (1) is a compound of epoxidized soybean oil and acetylated tributyl citrate. The epoxidized soybean oil, acetylated tributyl citrate and the heat stabilizer are mixed evenly at 40-60°C before being added to the dispersion tank.

9. The preparation method of the environmentally friendly low-temperature curing PVC anti-stone chip primer according to claim 6, characterized in that, The method of adding PVC paste resin and chloroacetic acid copolymer resin in step (1) is as follows: first add 1 / 2 of the formula amount of PVC paste resin, stir for 5 to 10 minutes, then add all of the chloroacetic acid copolymer resin, stir for 5 to 10 minutes, and then add the remaining 1 / 2 of the PVC paste resin.

10. The preparation method of the environmentally friendly low-temperature curing PVC anti-stone chip primer according to claim 6, characterized in that, Step (3) is followed by filling the filtered coating material into a sealed container under vacuum conditions, filling it with nitrogen for protection, and storing it at 0-10°C.

Citation Information

Patent Citations

  • A low-density anti-stone chip coating for aluminum car bodies, its preparation method and application

    CN115851047B