Recycling method for tape-casting green body of silicon nitride substrate
By adjusting the processing technology and formula composition of the silicon nitride ceramic substrate, the waste green body is mixed with the new slurry to prepare high-quality casting belts, which solves the problem that waste green body cannot be recycled, reduces production costs and increases Product performance.
Patent Information
- Application Number
- CN202410988919.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The waste green body generated in the existing silicon nitride ceramic substrate casting process cannot be effectively recycled, resulting in waste of resources and increased material costs.
By adjusting the processing technology and formula composition, the discarded green body is mixed with the new slurry, and after vacuum drying, crushing, slurrying, ball milling, filtration and vacuum defoaming, a high-quality silicon nitride casting belt is prepared to achieve waste Recycling of green bodies.
It effectively reduces the production cost of silicon nitride substrates, improves product performance, reduces solid waste generation, is suitable for mass production applications, and optimizes environmental protection effects.
Smart Images

Figure CN118930282A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic preparation, and in particular relates to a method for recycling a silicon nitride substrate tape-cast green body. Background Art
[0002] In recent years, electronic power devices have developed towards high power, high frequency, high density, and integration, which has put forward higher requirements for ceramic heat dissipation substrates in devices. Silicon nitride ceramic substrates have high mechanical properties, low toughness, low ductility, high thermal conductivity, wear resistance, thermal shock resistance and other characteristics. They are recognized as ceramic substrate materials with high thermal conductivity and high reliability. They are suitable for applications with large mechanical vibration, large thermal shock, large current shock, and high reliability and stability, such as aerospace, rail transportation, electric vehicles, photovoltaic inverters, smart grids, etc.
[0003] Silicon nitride powder is the main raw material for silicon nitride ceramics and related products. It is a covalent bond compound with a nitrogen atom and silicon atom ratio of 4:3. It has a hexagonal crystal structure and has three crystal phases: α, β and γ. Among them, α and β phases are the most common forms of Si3N4 and can be prepared under normal pressure. α-Si3N4 is a low-temperature stable phase, and β-Si3N4 is a high-temperature stable phase. During the sintering process of silicon nitride ceramics, α-Si3N4 will undergo abnormal grain growth and phase deformation into columnar crystal β-Si3N4. This structure plays a bridging, bifurcation and deflection role in crack propagation, which can improve the toughness of the material and greatly improve the strength of the ceramic. Therefore, a high α phase content is an important guarantee for obtaining high-performance silicon nitride ceramics. High-quality silicon nitride powder is the initial condition for obtaining high-performance silicon nitride ceramics, which generally requires high purity, fine particle size and narrow distribution, and high α phase content. At present, the main methods for preparing silicon nitride powder include silicon powder nitridation method, imide synthesis method, carbon thermal reduction method, plasma method, etc. Different powder synthesis processes have a huge impact on the characteristics of the powder. However, whether it is domestic or foreign, high-performance silicon nitride powder has high production costs and is expensive due to its raw materials, processes, equipment, efficiency and other factors.
[0004] Existing silicon nitride ceramic substrates are mostly produced by dry pressing and tape casting. The characteristics of the tape casting process are high production efficiency, continuous operation, high level of automation, stable process, and very suitable for large-scale batch production. However, during the production of tape casting, it is inevitable that there will be green billets with poor thickness uniformity in the front and rear sections and on both sides of the tape casting, which cannot be used to produce products. According to differences in the width difference of the tape casting machine, the formula system and the process, this part accounts for about 10% to 30%. In addition, some scrap green billets and unqualified green billets will also be produced during the molding process. These green billets cannot produce products, and directly scrapping them will not only produce more solid waste, but also greatly increase the material cost of the product. However, since the edge width of this part of the green billet is narrow and the thickness is uneven, the thickness of the front and rear sections does not meet the requirements, and the molding is poor. It is difficult to recycle it with existing technology, so it can only be scrapped.
[0005] Therefore, it is urgent to develop a silicon nitride substrate tape casting green body recycling application technology so that the silicon nitride substrate tape casting waste green body can be recycled. Summary of the invention
[0006] The present invention realizes the recycling of discarded green billets of silicon nitride substrate tape casting. By adjusting the processing technology and the formulation composition, the discarded green billets and the newly prepared slurry are used together to prepare silicon nitride tape casting green tape, which not only realizes the recycling of the discarded green billets, but also significantly reduces the production cost of the tape casting green tape.
[0007] The present invention provides a method for recycling a silicon nitride substrate tape-cast green body, which comprises the following steps:
[0008] A. After vacuum drying, the recovered green body is crushed, and then the dried and crushed green body is mixed with a solvent and a dispersant for slurrying, and then a plasticizer and a defoamer are added. After ball milling, the material is filtered through a 200-800 mesh screen and a strong magnetic filter, and the particle size is detected to obtain a dispersed slurry of the recovered green body;
[0009] B. Mix the recycled green body dispersion slurry obtained in step A with the newly prepared slurry, continue ball milling, detect the particle size, filter the discharged material, and perform vacuum degassing treatment, and then age and filter through a 200-800 mesh sieve to obtain a casting slurry;
[0010] C. Perform tape casting on the tape casting slurry obtained in step B to obtain a silicon nitride tape casting green tape.
[0011] Wherein, in the above method, in step A, the solvent, dispersant and plasticizer are of the same type as those of the newly prepared slurry.
[0012] Wherein, in the above method, in step A, the amount of the solvent added is 20% to 200% of the mass of the green body after drying and crushing.
[0013] Preferably, in the above method, in step A, the amount of the solvent added is 70% to 200% of the mass of the green body after drying and crushing.
[0014] Wherein, in the above method, in step A, the solvent is a mixture of three types of alcohols, benzenes and ketones in a mass ratio of 1 to 10:1 to 10:1 to 10, or a mixture of two types of alcohols, benzenes and ketones in a mass ratio of 1 to 10:1 to 10; the alcohol is isobutyl alcohol, tert-butyl alcohol, phenylethyl alcohol, diacetone alcohol, n-butyl alcohol, ethylene glycol, isopropyl alcohol, propanol or ethanol; the benzene is toluene or xylene; the ketone is cyclohexanone, butanone, dibutyl ketone or methyl isobutyl ketone.
[0015] Wherein, in the above method, in step A, the amount of the plasticizer added is 0.5% to 5% of the mass of the green body after drying and crushing.
[0016] Preferably, in the above method, in step A, the amount of the plasticizer added is 0.5-3% of the mass of the green body after drying and crushing.
[0017] Wherein, in the above method, in step A, the plasticizer is at least one of dibutyl phthalate, dioctyl phthalate, butyl benzyl phthalate, glycerol or polyethylene glycol.
[0018] Wherein, in the above method, in step A, the amount of the dispersant added is 0.1% to 2.0% of the mass of the green body after drying and crushing.
[0019] Wherein, in the above method, in step A, the dispersant is at least one of polyvinyl pyrrolidone, fish oil, triolein, castor oil phosphate or triethyl phosphate.
[0020] Wherein, in the above method, in step A, the amount of the defoaming agent added is 0.05% to 1.0% of the mass of the green body after drying and crushing.
[0021] Wherein, in the above method, in step A, the defoaming agent is any one of n-butanol, diethylhexanol, isooctyl alcohol, isopentanol, diisobutyl carbinol or tributyl phosphate, or a mixture of two thereof.
[0022] Wherein, in the above method, in step A, the vacuum drying temperature is 15 to 60° C., the vacuum degree is 5 to 100 Pa, and the time is 4 to 96 hours.
[0023] Wherein, in the above method, in step A, the pulping operation is: stirring at 600-1200 rpm for 0.5-5 hours.
[0024] In the above method, in step A, the ball milling operation is as follows: the ball milling medium is silicon nitride balls, and the models are two to four combinations of Φ3mm, Φ5mm, Φ8mm, Φ10mm, Φ12mm, Φ15mm and Φ20mm, and the mass ratios of the two to four combinations are 1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1:1±0.1:1±0.1, the amount of ball milling medium added is 30% to 50% of the ball mill volume, the ball milling speed is 25 to 60rpm, and the ball milling time is 8 to 48h.
[0025] Wherein, in the above method, in step A, the particle size D50 of the recovered green body dispersion slurry is controlled at 0.5-1.0 μm.
[0026] Wherein, in the above method, in step B, the mixing ratio of the newly prepared slurry based on the mass of silicon nitride powder and the recycled green body dispersion slurry based on the mass of the green body after drying and crushing is 9:1 to 0:10.
[0027] Preferably, in the above method, in step B, the mixing ratio of the newly prepared slurry based on the mass of silicon nitride powder and the recycled green body dispersion slurry based on the mass of the green body after drying and crushing is 9:1 to 1:9 or 0:10.
[0028] In the above method, in step B, the ball milling operation is as follows: the ball milling medium is silicon nitride balls, and the models are two to four combinations of Φ3mm, Φ5mm, Φ8mm, Φ10mm, Φ12mm, Φ15mm and Φ20mm, and the mass ratios of the two to four combinations are 1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1:1±0.1:1±0.1, respectively. The amount of ball milling medium added is 30% to 50% of the ball mill volume, the ball milling speed is 25 to 60rpm, and the ball milling time is 8 to 48h.
[0029] Wherein, in the above method, in step B, the vacuum degree of the vacuum degassing treatment is -95KPa to -100KPa, and the degassing time is 30 to 300min.
[0030] Wherein, in the above method, in step B, the aging time is 0.5h to 12h.
[0031] Wherein, in the above method, in step B, the particle size D50 of the obtained casting slurry is controlled at 0.45 to 0.9 μm.
[0032] Wherein, in the above method, in step B, the viscosity of the obtained casting slurry is 5000-40000 cps, and the solid content is 60%-80%.
[0033] Wherein, in the above method, in step B, in step C, during the tape casting, the scraper height is 0.6-2.0 mm, the tape casting speed is 0.1-0.5 m / min, and the oven temperature is 25-100° C. in multiple steps.
[0034] Wherein, in the above method, in step B and step C, the thickness of the obtained silicon nitride tape is 0.2 to 1.0 mm.
[0035] Beneficial effects of the present invention:
[0036] The present invention can effectively recycle the discarded green billets generated in the casting and molding processes, greatly reduce the material cost of the silicon nitride substrate, and improve the product competitiveness; by adjusting the dispersion process using the recycled green billets as raw materials and optimizing the ratio of the recycled green billet dispersion slurry and the newly prepared slurry, it is possible to obtain a casting green tape with excellent performance and ensure the performance of the product after sintering; the present invention uses relatively simple equipment, processes and operating steps, has a high efficiency in recycling discarded green billets, and is suitable for mass production applications; the present invention also greatly reduces the solid waste generated by discarding silicon nitride casting and molding green billets, which is beneficial to environmental protection and environmental safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a real picture of the silicon nitride tape prepared in Example 1.
[0038] Figure 2 This is a SEM image of the surface of the silicon nitride tape prepared in Example 2.
[0039] Figure 3 This is a picture of the actual ceramic body after sintering the silicon nitride tape-cast green body prepared in Example 3.
[0040] Figure 4 This is a SEM image of the cross-section of the silicon nitride tape-cast green body prepared in Example 4 after sintering. DETAILED DESCRIPTION
[0041] Specifically, a method for recycling a silicon nitride substrate tape-cast green body comprises the following steps:
[0042] A. After the recovered green body is vacuum dried (generally in a vacuum drying oven), it is crushed, and then the dried and crushed green body is mixed with a solvent and a dispersant for pulping, and then a plasticizer and a defoamer are added, and after ball milling (generally in a ball milling tank), the material is filtered through a 200-800 mesh screen and a strong magnetic filter, and the particle size is detected to obtain a dispersed slurry of the recovered green body;
[0043] B. Mix the recycled green body dispersion slurry obtained in step A with the newly prepared slurry, continue ball milling (generally in a ball mill), detect the particle size and filter the discharged material, and perform vacuum degassing treatment (generally in a degassing tank), and then age and filter through a 200-800 mesh sieve to obtain a casting slurry;
[0044] C. The casting slurry obtained in step B is subjected to casting molding (generally cast molding on a PET release film) to obtain a silicon nitride casting green tape.
[0045] In step A of the present invention, the amount of the solvent added is 20% to 200% of the mass of the green body after drying and crushing; preferably 70% to 200%. The type of solvent used in preparing the recycled green body dispersion slurry is the same as the solvent used for the newly prepared slurry. The solvent is a mixture of three types of alcohols, benzenes and ketones in a mass ratio of 1 to 10:1 to 10:1 to 10, or a mixture of two types of alcohols, benzenes and ketones in a mass ratio of 1 to 10:1 to 10; the alcohol is isobutyl alcohol, tert-butyl alcohol, phenylethyl alcohol, diacetone alcohol, n-butyl alcohol, ethylene glycol, isopropyl alcohol, propanol or ethanol; the benzene is toluene or xylene; the ketone is cyclohexanone, butanone, dibutyl ketone or methyl isobutyl ketone.
[0046] In step A of the present invention, the amount of the plasticizer added is 0.5% to 5% of the mass of the green body after drying and crushing; preferably 0.5% to 3%. The type of plasticizer used in preparing the recycled green body dispersion slurry is the same as the plasticizer used in the newly prepared slurry. The plasticizer is at least one of dibutyl phthalate, dioctyl phthalate, butyl benzyl phthalate, glycerol or polyethylene glycol.
[0047] In step A of the present invention, the amount of the dispersant added is 0.1% to 2.0% of the mass of the green body after drying and crushing. The type of dispersant used in preparing the recycled green body dispersion slurry is the same as the dispersant used in the newly prepared slurry. The dispersant is at least one of polyvinyl pyrrolidone, fish oil, triolein, castor oil phosphate or triethyl phosphate.
[0048] In step A of the present invention, when preparing the dispersion slurry of the recycled green body, the types of the solvent, dispersant and plasticizer used need to be consistent with the types of the solvent, dispersant and plasticizer used in preparing the new slurry in step B. In addition, in the prior art, the recycled green body is also produced in the production of new material tape casting. When preparing the dispersion slurry of the recycled green body, the types of the solvent, dispersant and plasticizer used also need to be consistent with the new material; and when the method for producing silicon nitride tape using recycled green bodies provided by the present invention is used for production, recycled green bodies are inevitably produced. When the recycled green bodies are recycled, the types of solvents, dispersants and plasticizers also need to be kept consistent; keeping the types of materials consistent in each process is more conducive to ensuring the stability of product performance.
[0049] In step A of the present invention, the amount of the defoamer added is 0.05% to 1.0% of the mass of the green body after drying and crushing. The defoamer is any one of n-butanol, diethylhexanol, isooctyl alcohol, isopentanol, diisobutyl carbinol or tributyl phosphate, or a mixture of two thereof.
[0050] In step A of the present invention, the vacuum drying temperature is 15 to 60° C., the vacuum degree is 5 to 100 Pa, and the time is 4 to 96 hours.
[0051] The pulping operation of the present invention is: stirring at 600-1200 rpm for 0.5-5 hours (generally carried out in a high-speed disperser).
[0052] According to the dispersion characteristics of the recycled green body, the present invention optimizes the dispersion process, adopts a specific ball milling process, makes the slurry have good dispersibility, and makes the particle size of the recycled green body dispersion slurry meet the requirements. In step A, the operation of the ball milling is: the ball milling medium is silicon nitride balls, the model is a combination of two to four of Φ3mm, Φ5mm, Φ8mm, Φ10mm, Φ12mm, Φ15mm and Φ20mm, the mass ratio of the two to four combinations is 1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1:1±0.1, the amount of ball milling medium added is 30% to 50% of the ball milling volume, the ball milling speed is 25 to 60rpm, and the ball milling time is 8 to 48h.
[0053] There is a greater possibility of introducing impurities in each link of the recycled green body. Therefore, in step A of the present invention, the material is first filtered with a 200-800 mesh screen to initially filter impurities and dry materials. The slurry after screening is passed through a strong magnetic filter, and the slurry is passed through a pipeline strong magnetic filter inserted with several magnetic bars, and flows around the magnetic bars to further remove impurities such as iron in the recycled green body to avoid excessive impurity content, which may have an adverse effect on the appearance and performance of the product. In addition, the particle size of the recycled green body dispersion slurry cannot be significantly different from the particle size of the newly made slurry. If the particle size of the recycled green body dispersion slurry is not controlled, it is easy to cause the casting cracking and sintering performance to change significantly, thereby affecting the final product appearance and performance. Therefore, if the particle size of the recycled green body dispersion slurry is too large, it is necessary to extend the ball milling time for dispersion. If the particle size is too small, it is necessary to reduce the amount of addition in step B, or the entire batch is scrapped, and the purpose of recycling cannot be achieved. Therefore, in step A, the present invention needs to detect the particle size so that the particle size D50 of the recovered green body dispersion slurry is controlled within the range of 0.5 to 1.0 μm.
[0054] In step B of the present invention, the mixing ratio of the newly made slurry in terms of the mass of silicon nitride powder and the recycled green body dispersion slurry in terms of the mass of green body after drying and crushing is 9:1 to 0:10. In the present invention, the newly made slurry can be completely omitted, that is, all the recycled green body dispersion slurry is used to prepare the tape casting green body. Although this configuration is feasible, the potential risk is relatively large: if the newly made slurry is not added, the slurry particle size after redispersion is prone to the risk of potential particle size being too small, thereby causing related problems; in addition, although the impurity removal measures are added during the preparation of the recycled green body dispersion slurry, it cannot be guaranteed that the impurities are 100% removed, and there is also a risk of potential impurities exceeding the standard. Therefore, the use of recycled green body dispersion slurry is generally used for the treatment of certain abnormal batches that need to be recycled in batches; in terms of long-term stable production, the present invention adopts the configuration of "mixing newly made slurry and recycled green body dispersion slurry", that is, the present invention preferably controls the mixing ratio of the newly made slurry in terms of the mass of silicon nitride powder and the recycled green body dispersion slurry in terms of the mass of green body after drying and crushing to be 9:1 to 1:9 or 0:10.
[0055] In step B of the present invention, the ball milling process is also optimized. In step B, the ball milling operation is as follows: the ball milling medium is silicon nitride balls, and the models are two to four combinations of Φ3mm, Φ5mm, Φ8mm, Φ10mm, Φ12mm, Φ15mm and Φ20mm, the mass ratio of the two to four combinations is 1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1:1±0.1:1±0.1, the amount of ball milling medium added is 30% to 50% of the ball mill volume, the ball milling speed is 25 to 60rpm, and the ball milling time is 8 to 48h.
[0056] In step B of the present invention, the vacuum degree of the vacuum degassing treatment is -95KPa to -100KPa, and the degassing time is 30 to 300min.
[0057] In step B of the present invention, the aging time is 0.5h to 12h.
[0058] In step B of the present invention, there is a certain difference in the slurry particle size before and after the new slurry and the recycled green body dispersion slurry are mixed. Therefore, in step B, it is necessary to continue ball milling. The ball milling mixing process will have a certain impact on the slurry particle size. The 200-800 mesh filter screen of the slurry after ball milling and mixing filters large particle impurities. This proportion accounts for a small proportion, and the slurry particle size will not be affected before and after filtration, and the particle size D50 of the obtained tape casting slurry is finally controlled at 0.45-0.9 μm; avoid problems such as tape casting cracking or sintering performance changes caused by excessive particle size. In step A of the present invention, the slurry particle size is controlled to indicate whether the recycled green body is evenly dispersed when dispersed into the slurry and whether the powder grain morphology is destroyed (over-grinding) during the dispersion process; the slurry particle size is controlled in step B to indicate the slurry situation after the recycled material is mixed with the new material, and the particle size is strictly controlled to obtain a tape casting green belt with performance that meets the standard.
[0059] In step B of the present invention, the viscosity of the obtained casting slurry is 5000-40000 cps, and the solid content is 60%-80%.
[0060] In step C of the present invention, during the tape casting, the scraper height is 0.6-2.0 mm, the tape casting speed is 0.1-0.5 m / min, and the oven temperature is 25-100° C. in multiple steps.
[0061] In step C of the present invention, the thickness of the obtained silicon nitride tape is 0.2-1.0 mm.
[0062] In the present invention, the recycled green blanks are green blanks with poor thickness uniformity in the front and rear sections and on both sides of the casting process, leftover green blanks, unqualified green blanks, etc. In production, a small amount of green blanks may be contaminated by impurities such as oil stains. Since this part is very small, it can be recycled.
[0063] In the present invention, the newly prepared slurry is prepared by conventional operation in the existing silicon nitride substrate casting process. For example, the newly prepared slurry preparation process in CN117003567A can be adopted, and the specific preparation process is as follows:
[0064] a. The new material consists of an inorganic phase and an organic phase, wherein the inorganic phase is silicon nitride powder; the organic phase consists of a dispersant, a plasticizer, a binder and a solvent, and their contents are 0.5-3%, 4-15%, 4-15% and 60-80% of the mass of the inorganic phase powder, respectively; the particle size of the silicon nitride powder is between 300nm and 1500nm; the binder is at least one of polyvinyl butyral and polymethyl methacrylate;
[0065] b. Add the binder and plasticizer into the solvent (30-60% of the total solvent), stir and dissolve them thoroughly, and then let them stand for 12-24 hours to obtain a presol;
[0066] c. Ball-mill the dispersant and the solvent (remaining solvent) in proportion for 5 to 30 minutes to fully dissolve the dispersant, then add the silicon nitride powder and ball-mill for 0.5 to 5 hours to obtain a primary ball-milled slurry, wherein the primary ball-milling includes any one or more combinations of drum ball milling, stirring ball milling or sand milling;
[0067] d. Add the first ball-milled slurry and presol into the roller ball mill, and continue ball-milling for 12 h to 24 h to obtain a new slurry.
[0068] However, the present invention is not limited to the new slurry in CN117003567A mentioned above. The new slurry for preparing silicon nitride tape prepared by other existing processes in the field is also applicable to the method of the present invention, as long as the recovered green body is produced in the process of preparing silicon nitride tape with the corresponding new slurry.
[0069] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.
[0070] Example 1
[0071] A silicon nitride substrate tape casting green body recycling application technology, wherein the slurry is composed of recycled green body dispersion slurry and newly prepared slurry, and the amount of recycled green body dispersion slurry added is 15% of the weight of silicon nitride powder in the newly prepared slurry according to the mass of the recycled green body after drying and crushing;
[0072] The recycled green body dispersion slurry is composed of recycled green body, dispersant, solvent, plasticizer and defoamer, wherein the contents of the dispersant, solvent, plasticizer and defoamer are 0.5%, 70%, 1.2% and 0.2% of the mass of the recycled green body after drying and crushing, respectively; the types of solvent, plasticizer and dispersant used in the recycled green body dispersion slurry are consistent with those of the newly prepared slurry;
[0073] New slurry preparation process:
[0074] a. The slurry raw material is composed of an inorganic phase and an organic phase, wherein the inorganic phase is silicon nitride powder, and the organic phase is composed of a dispersant, a plasticizer, a binder and a solvent, and the contents thereof are 0.6%, 8%, 12% and 70% of the mass of the silicon nitride powder, respectively;
[0075] b. Add the binder and plasticizer into the solvent (45% of the total solvent), stir and dissolve them thoroughly, and then let them stand for 12 hours to obtain a presol;
[0076] c. The dispersant and the solvent (55% of the total solvent) are ball-milled in proportion for 5 minutes to fully dissolve the dispersant, and then silicon nitride powder is added and ball-milled for 4 hours to obtain a primary ball-milled slurry;
[0077] d. Add the first ball-milled slurry and presol into the roller ball mill, and continue ball-milling for 24 hours to obtain a newly prepared slurry;
[0078] Among them, the solvent is toluene, ethanol and cyclohexanone mixed in a mass ratio of 1:2:1; the plasticizer is a mixture of butyl benzyl phthalate and polyethylene glycol in a mass ratio of 3:1; the binder is polyvinyl butyral; the dispersant is fish oil and triolein mixed in a mass ratio of 2:1, and the defoamer is a mixture of diethylhexanol and isoamyl alcohol in a mass ratio of 1:1.
[0079] The silicon nitride substrate tape casting green body recovery application method is as follows:
[0080] (1) The recovered green body is placed in a vacuum drying oven for treatment at a temperature of 40° C., a vacuum degree of 50 Pa, and a treatment time of 24 h, and then crushed;
[0081] (2) The solvent and dispersant were stirred and mixed in a high-speed disperser for 10 minutes, and then the crushed recycled green body was added and the slurry was stirred at 800 rpm × 1 hour;
[0082] (3) pouring the mixed slurry in step 2 into a ball mill, adding a plasticizer and a defoamer, and then ball milling, the balls are Φ5mm, Φ8mm, and Φ10mm silicon nitride balls with a mass ratio of 1:1:1, and the added amount is 35% of the ball mill volume, and the ball milling is carried out at 55rpm for 12h. The material is filtered through a 200-mesh screen and a strong magnetic filter, and the particle size is detected to prepare a recycled green body dispersion slurry with a particle size D50 of 0.78μm;
[0083] (4) The newly prepared slurry and the recycled green body dispersion slurry were added and mixed in proportion, and the ball milling was continued. The balls were Φ5 mm, Φ8 mm, and Φ10 mm silicon nitride balls with a mass ratio of 1:1:1, and the amount added was 35% of the ball mill volume. The ball milling was carried out at 55 rpm for 36 hours;
[0084] (5) After the particle size is detected, the material is filtered and vacuum degassing is performed at -95 KPa for 120 minutes, then aged for 3 hours and filtered through a 200-mesh stainless steel sieve to prepare a casting slurry with a viscosity of 22000 mPa.s, a particle size D50 of 0.80 μm, and a solid content of 70%;
[0085] (6) The scraper height was set to 1.2 mm, the casting speed was set to 0.25 m / min, and the drying temperature was set according to Table 1 to prepare a silicon nitride casting tape with a thickness of 0.5 mm.
[0086] Table 1 Drying temperature
[0087] Temperature Zone 1 2 3 4 5 Temperature(℃) 40 50 60 72 95
[0088] The slurry prepared by adding the recycled green body in Example 1 has good fluidity, the cast green tape has a smooth appearance, uniform thickness, excellent toughness and strength, and the green body has uniform microscopic grain distribution. Figure 1 shown.
[0089] Example 2
[0090] A silicon nitride substrate tape casting green body recycling application technology, wherein the slurry is composed of recycled green body dispersion slurry and newly prepared slurry, and the amount of recycled green body dispersion slurry added is 50% of the weight of silicon nitride powder in the newly prepared slurry according to the mass of the recycled green body after drying and crushing;
[0091] The recycled green body dispersion slurry is composed of recycled green body, dispersant, solvent, plasticizer and defoamer, wherein the contents of the dispersant, solvent, plasticizer and defoamer are 0.6%, 100%, 1.0% and 0.4% of the mass of the recycled green body after drying and crushing, respectively;
[0092] Wherein, the solvent, dispersant and plasticizer are the same as those in Example 1;
[0093] Among them, the defoamer is a mixture of n-butanol and isoamyl alcohol in a mass ratio of 2:1;
[0094] The newly prepared slurry is the same as in Example 1.
[0095] The silicon nitride substrate tape casting green body recovery application method is as follows:
[0096] (1) The recovered green body is placed in a vacuum drying oven for treatment at a temperature of 40° C., a vacuum degree of 10 Pa, and a treatment time of 48 h, and then crushed;
[0097] (2) Stirring and mixing the solvent and dispersant in a high-speed disperser for 10 minutes, then adding the crushed recycled green body, and stirring the slurry at 1200 rpm × 2 hours;
[0098] (3) Pour the mixed slurry in step 2 into a ball mill, add a plasticizer and a defoamer, and then perform ball milling. The balls are Φ5 mm, Φ8 mm, and Φ10 mm silicon nitride balls with a mass ratio of 1:1:1, and the added amount is 35% of the ball mill volume. The ball milling is performed at 55 rpm for 18 hours. The material is filtered through a 200 mesh screen and a strong magnetic filter, and the particle size is tested by sampling to obtain a recycled green body dispersion slurry with a particle size D50 of 0.75 μm.
[0099] (4) The newly prepared slurry and the recycled green body dispersion slurry were added and mixed in proportion, and the ball milling was continued. The balls were Φ5 mm, Φ8 mm, and Φ10 mm silicon nitride balls with a mass ratio of 1:1:1, and the amount added was 35% of the ball mill volume. The ball milling was carried out at 55 rpm for 36 hours;
[0100] (5) After the particle size is detected, the material is filtered and vacuum degassing is performed at -95.7 KPa for 85 minutes, then aged for 2 hours and filtered through a 200-mesh stainless steel sieve to prepare a casting slurry with a viscosity of 8000 mPa.s, a particle size D50 of 0.74 μm, and a solid content of 68.9%;
[0101] (6) The scraper height was set to 1.0 mm, the casting speed was set to 0.3 m / min, and the drying temperature was set according to Table 1 to prepare a silicon nitride casting tape with a thickness of 0.4 mm.
[0102] Example 2 further increases the proportion of recycled silicon nitride green bodies on the basis of Example 1, and the prepared tape casting slurry has good fluidity, and the tape casting green tape has good toughness, uniform thickness, smooth surface, and no defects such as pits, bubbles, and cracks; Figure 2 It can be seen that the silicon nitride green ceramic particles are evenly distributed.
[0103] Example 3
[0104] A silicon nitride substrate tape casting green body recycling application technology, wherein the slurry is composed of recycled green body dispersion slurry and newly prepared slurry, and the amount of recycled green body dispersion slurry added is 100% of the weight of silicon nitride powder in the newly prepared slurry according to the mass of the recycled green body after drying and crushing;
[0105] The recycled green body dispersion slurry is composed of recycled green body, dispersant, solvent, plasticizer and defoamer, wherein the contents of the dispersant, solvent, plasticizer and defoamer are 0.8%, 120%, 1.2% and 0.6% of the mass of the recycled green body after drying and crushing, respectively;
[0106] Wherein, the solvent, dispersant and plasticizer are the same as those in Example 1;
[0107] The defoamer is a mixture of isoamyl alcohol and diisobutyl carbinol in a mass ratio of 1:1;
[0108] The newly prepared slurry is the same as in Example 1.
[0109] The silicon nitride substrate tape casting green body recovery application method is as follows:
[0110] (1) The recovered green body is placed in a vacuum drying oven for treatment at a temperature of 50° C., a vacuum degree of 10 Pa, and a treatment time of 24 h, and then crushed;
[0111] (2) Stirring and mixing the solvent and dispersant in a high-speed disperser for 10 minutes, then adding the crushed recycled green body, and stirring the slurry at 1200 rpm × 4 hours;
[0112] (3) Pour the mixed slurry in step 2 into a ball mill, add a plasticizer and a defoamer, and then perform ball milling. The balls are Φ5 mm, Φ8 mm, and Φ10 mm silicon nitride balls with a mass ratio of 1:1:1, and the added amount is 35% of the ball mill volume. The ball milling is performed at 55 rpm for 24 hours. The material is filtered through a 400 mesh screen and a strong magnetic filter and the particle size is detected to prepare a recycled green body dispersion slurry with a particle size D50 of 0.71 μm.
[0113] (4) The newly prepared slurry and the recycled green body dispersion slurry were added and mixed in proportion, and the ball milling was continued. The balls were Φ5 mm, Φ8 mm, and Φ10 mm silicon nitride balls with a mass ratio of 1:1:1, and the addition amount was 35% of the ball mill volume. The ball milling was carried out at 55 rpm for 30 hours;
[0114] (5) After the particle size is detected, the material is filtered and vacuum degassing is performed at -95.5 KPa for 90 minutes, then aged for 2 hours and filtered through a 200-mesh stainless steel sieve to prepare a casting slurry with a viscosity of 8000 mPa.s, a particle size D50 of 0.72 μm, and a solid content of 69.5%;
[0115] (6) The scraper height was set to 1.2 mm, the casting speed was set to 0.2 m / min, and the silicon nitride casting tape with a thickness of 0.52 mm was prepared by casting according to the drying temperature in Table 1.
[0116] Example 3 further increases the proportion of recycled silicon nitride green bodies on the basis of Examples 1 and 2. The prepared tape casting slurry has good fluidity, the surface of the tape casting green tape is flat, the thickness is uniform, and other properties are good. The green tape has good toughness and no defects such as pits and bubbles. Figure 3 It can be seen that the product quality of the green body of this embodiment is qualified after sintering, and there are no appearance defects such as impurities, foreign matter, bright spots, etc.
[0117] Example 4
[0118] A silicon nitride substrate tape casting green body recycling application technology, wherein all the slurry is recycled green body dispersion slurry;
[0119] The recycled green body dispersion slurry is composed of recycled green body, dispersant, solvent, plasticizer and defoamer, and the contents of the dispersant, solvent, plasticizer and defoamer are 1.5%, 150%, 2.0% and 1.0% of the mass of the recycled green body after drying and crushing, respectively;
[0120] Wherein, the solvent, dispersant and plasticizer are the same as those in Example 1;
[0121] The defoaming agent is a mixture of isoamyl alcohol and diisobutyl carbinol in a mass ratio of 1:2.
[0122] The silicon nitride substrate tape casting green body recovery application method is as follows:
[0123] (1) The recovered green body is placed in a vacuum drying oven for treatment at a temperature of 50° C., a vacuum degree of 10 Pa, and a treatment time of 48 h, and then crushed;
[0124] (2) Stirring and mixing the solvent and dispersant in a high-speed disperser for 20 minutes, then adding the crushed recycled green body, and stirring the slurry at 1200 rpm × 5 hours;
[0125] (3) Pour the mixed slurry in step 2 into a ball mill, add a plasticizer and a defoamer, and then ball mill. The balls are Φ5 mm, Φ8 mm, and Φ10 mm silicon nitride balls with a mass ratio of 1:1:1, and the added amount is 35% of the ball mill volume. The ball mill is milled at 55 rpm for 36 hours. The material is filtered through a 500 mesh screen and a strong magnetic filter and the particle size is detected to prepare a recycled green body dispersion slurry with a particle size D50 of 0.69 μm.
[0126] (4) After filtration, the green body dispersion slurry was recovered and subjected to vacuum degassing treatment at -95.4 KPa for 70 minutes, then aged for 2 hours and filtered through a 200-mesh stainless steel sieve to prepare a casting slurry with a viscosity of 6000 mPa.s without adding new slurry, a particle size D50 that is the particle size after the recovered slurry is dispersed, and a solid content of 68.1%;
[0127] (5) The scraper height was set to 1.1 mm, the casting speed was set to 0.25 m / min, and the silicon nitride casting tape with a thickness of 0.45 mm was prepared by casting according to the drying temperature in Table 1.
[0128] Example 4 is a tape casting slurry prepared by dispersing the fully recycled green body. The tape casting green tape has a smooth surface, uniform thickness, good toughness, and no defects such as pits and bubbles. Figure 4 It can be seen that the tape-cast green body prepared by fully recycling the green body slurry in this embodiment has uniform and dense grain growth after sintering, and the product has better mechanical properties and reliability.
[0129] The performance test of the products after sintering in the above embodiments is shown in Table 2.
[0130] Table 2 Product performance test table
[0131]
[0132]
[0133] Comparative Example 1
[0134] It is basically the same as Example 2, except that the added solvent ratio is 60% of the mass of the recovered green body, the ball milling dispersion time of the recovered green body slurry is 6 hours, the thickness of the prepared silicon nitride tape is 0.4 mm, the appearance of the tape is cracked during casting, and the black spots and bright spots are serious after sintering.
[0135] Comparative Example 2
[0136] It is basically the same as Example 1, except that no defoaming agent is added to the formula, the amount of plasticizer added is 0.4% of the mass of the recovered green body, the thickness of the prepared silicon nitride tape is 0.5 mm, the appearance of the tape is cracked during casting, the green body is hard and has poor toughness, and there are many bubbles in the appearance.
[0137] In Comparative Example 1, the reduction in the dispersion solvent increased the viscosity of the slurry, and the shortened dispersion time resulted in poor dispersion of the recovered green body, resulting in uneven dispersion. Therefore, it is necessary to reasonably control the solvent ratio and the dispersion time cannot be too short.
[0138] In Comparative Example 2, the addition of defoaming agent was cancelled and the addition ratio of plasticizer was reduced, which resulted in difficulty in defoaming the slurry, and the cast tape became hard, cracked and had bubbles. In order to obtain a cast tape with good casting appearance and moderate hardness, it is necessary to reasonably control the addition ratio of defoaming agent and plasticizer.
[0139] It should be noted that the above are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and other variations are possible. All variations directly or indirectly derived from the disclosure of the present invention by those skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A method for recycling silicon nitride substrate tape casting green body, characterized in that: The following steps are involved: A. After vacuum drying, the recovered green body is crushed, and then the dried and crushed green body is mixed with a solvent and a dispersant for slurrying, and then a plasticizer and a defoamer are added. After ball milling, the material is filtered through a 200-800 mesh screen and a strong magnetic filter, and the particle size is detected to obtain a dispersed slurry of the recovered green body; B. Mix the recycled green body dispersion slurry obtained in step A with the newly prepared slurry, continue ball milling, detect the particle size, filter the discharged material, and perform vacuum degassing treatment, and then age and filter through a 200-800 mesh sieve to obtain a casting slurry; C. Perform tape casting on the tape casting slurry obtained in step B to obtain a silicon nitride tape casting green tape.
2. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step A, at least one of the following must be met: The solvent, dispersant and plasticizer are of the same type as those of the newly prepared slurry; The amount of the solvent added is 20% to 200% of the mass of the green body after drying and crushing; preferably 70% to 200%; The solvent is a mixture of three types of alcohols, benzenes and ketones in a mass ratio of 1 to 10:1 to 10:1 to 10, or a mixture of two types of alcohols, benzenes and ketones in a mass ratio of 1 to 10:1 to 10; the alcohol is isobutyl alcohol, tert-butyl alcohol, phenylethyl alcohol, diacetone alcohol, n-butyl alcohol, ethylene glycol, isopropyl alcohol, propanol or ethanol; the benzene is toluene or xylene; the ketone is cyclohexanone, butanone, dibutyl ketone or methyl isobutyl ketone; The amount of the plasticizer added is 0.5% to 5% of the mass of the green body after drying and crushing; preferably 0.5 to 3%; The plasticizer is at least one of dibutyl phthalate, dioctyl phthalate, butyl benzyl phthalate, glycerol or polyethylene glycol; The amount of the dispersant added is 0.1% to 2.0% of the mass of the green body after drying and crushing; The dispersant is at least one of polyvinyl pyrrolidone, fish oil, triolein, castor oil phosphate or triethyl phosphate; The amount of the defoamer added is 0.05% to 1.0% of the mass of the green body after drying and crushing; The defoaming agent is any one of n-butanol, diethylhexanol, isooctyl alcohol, isopentanol, diisobutyl carbinol or tributyl phosphate or a mixture of two thereof.
3. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step A, at least one of the following must be met: The vacuum drying temperature is 15-60°C, the vacuum degree is 5-100Pa, and the time is 4-96h; The slurrying operation is: stirring at 600-1200 rpm for 0.5-5 hours.
4. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step A, the ball milling operation is as follows: the ball milling medium is silicon nitride balls, and the models are two to four combinations of Φ3mm, Φ5mm, Φ8mm, Φ10mm, Φ12mm, Φ15mm and Φ20mm, the mass ratios of the two to four combinations are 1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1:1±0.1:1±0.1, the amount of ball milling medium added is 30% to 50% of the ball mill volume, the ball milling speed is 25 to 60rpm, and the ball milling time is 8 to 48h.
5. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step A, the particle size D50 of the recovered green body dispersion slurry is controlled to be 0.5-1.0 μm.
6. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step B, the mixing ratio of the newly prepared slurry based on the mass of silicon nitride powder and the recycled green body dispersion slurry based on the mass of the green body after drying and crushing is 9:1 to 0:10, preferably 9:1 to 1:9 or 0:
10.
7. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step B, the ball milling operation is as follows: the ball milling medium is silicon nitride balls, and the models are two to four combinations of Φ3mm, Φ5mm, Φ8mm, Φ10mm, Φ12mm, Φ15mm and Φ20mm, the mass ratios of the two to four combinations are 1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1, 1±0.1:1±0.1:1±0.1:1±0.1:1±0.1, the amount of ball milling medium added is 30% to 50% of the ball mill volume, the ball milling speed is 25 to 60rpm, and the ball milling time is 8 to 48h.
8. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step B, at least one of the following is met: The vacuum degree of the vacuum degassing treatment is -95KPa to -100KPa, and the degassing time is 30 to 300min; The aging time is 0.5h to 12h; The particle size D50 of the obtained casting slurry is controlled at 0.45-0.9 μm; The viscosity of the obtained casting slurry is 5000-40000 cps, and the solid content is 60%-80%.
9. The method for recycling silicon nitride substrate tape-cast green body according to claim 1, characterized in that: In step C, during the tape casting, the scraper height is 0.6-2.0 mm, the tape casting speed is 0.1-0.5 m / min, and the oven temperature is 25-100° C. in multiple steps.
10. The method for recycling silicon nitride substrate tape-cast green body according to any one of claims 1 to 9, characterized in that: In step C, the thickness of the obtained silicon nitride tape is 0.2 to 1.0 mm.
Citation Information
Patent Citations
Method for preparing high-performance ceramic by recycling ceramic cast film waste
CN117069483A
Cited By
Preparation method of ceramic photocuring 3D printing slurry with recycled green bodies
CN119430883A
Preparation method of green body recycled ceramic photocuring 3D printing paste
CN119430883B
Silicon nitride tape-casting blank waste recycling method, tape-casting blank and application
CN119638440A
Method for recycling silicon nitride cast body waste, cast body and application
CN119638440B