A PE foam tape resistant to battery swelling and its preparation method
By introducing a three-layer structure and specific material treatment into the PE foam tape, the peel stress and thermal aging problems caused by the expansion of silicon anode batteries are solved, and the tape achieves high peel strength and anti-expansion performance under high temperature and high humidity conditions, ensuring the structural stability of electronic devices.
Patent Information
- Application Number
- CN202611335197.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing PE foam tapes cannot effectively resist the peeling stress and thermal aging problems caused by the volume expansion of silicon anode batteries during charging and discharging, resulting in back cover lifting, frame adhesive cracking, foam delamination, and waterproof seal failure.
The PE foam tape adopts a three-layer structure, including a first adhesive layer, a foam material layer, and a second adhesive layer. It uses acrylic adhesive and crosslinking agent, and is treated by electron beam irradiation crosslinking and latent curing agent. Combined with a uniform pore structure design, it enhances the tape's heat aging resistance and anti-expansion performance.
It improves the peel strength of the tape under high temperature and high humidity conditions, enhances its resistance to battery expansion, and ensures that the tape does not crack or delaminate during the charging and discharging of silicon anode batteries, maintaining good adhesion performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of adhesive materials, specifically relating to a PE foam tape resistant to battery swelling and its preparation method. Background Technology
[0002] PE foam tape is widely used in full-screen smartphones, tablets, and automotive display modules due to its excellent compression resilience and stress dispersion capabilities. PE foam tape is die-cut into a precision U-shaped frame, serving three core functions: first, as a structural adhesive layer, firmly fixing the screen module to the mid-frame; second, constructing a physical barrier, utilizing the closed-cell structure of the foam to achieve dust and water resistance; and third, absorbing the impact energy from drops and vibrations, protecting the fragile display panel.
[0003] As smartphones, tablets, and other electronic products become increasingly thinner, lighter, and longer-lasting, silicon anode materials, due to their high theoretical specific capacity (approximately 4200 mAh / g), have become a crucial development direction for next-generation lithium-ion battery anode materials. However, silicon anodes undergo approximately 300% volume expansion during charging and discharging. This significant volume change forces the adhesive tape used to withstand continuous peeling and pushing stresses caused by the battery's floating position, easily leading to technical problems such as back cover lifting, frame adhesive cracking, poor foam delamination requiring rework, and waterproof seal failure.
[0004] In addition to expanding in size, silicon anode batteries also generate heat during charging and discharging, so the tape needs to have excellent heat aging resistance. Summary of the Invention
[0005] To overcome the shortcomings of existing technologies, the present invention aims to provide a PE foam tape resistant to battery expansion, comprising a first adhesive layer, a foaming material layer, and a second adhesive layer stacked sequentially; the first and second adhesive layers are obtained by drying an acrylic adhesive; the acrylic adhesive, by weight, comprises 100 parts of polyacrylic acid resin masterbatch, 5-20 parts of tackifying resin, 0.5-3 parts of crosslinking agent, 3-6 parts of porous material, and 0.1-0.15 parts of surface treatment agent; the foaming material layer, by weight, comprises 70-80 parts of low-density polyethylene, 15-25 parts of foaming agent, and 0.5-2 parts of nucleating agent.
[0006] Preferably, the tackifying resin includes at least one of phenolic epoxy resin, terpene and its derivative resin, and rosin and its derivative resin.
[0007] Preferably, the crosslinking agent includes at least one of modified imidazole and dicyandiamide epoxy resin.
[0008] Preferably, the porous material is a zeolite molecular sieve with a pore size of 0.8-1.2 nm.
[0009] Preferably, the melt index of the low-density polyethylene is 1.5-2.0 g / 10 min.
[0010] Preferably, the foaming agent is azodicarbonamide with a particle size of 4-6 μm.
[0011] Preferably, the nucleating agent includes at least one of talc and calcium carbonate, with a particle size of 1-15 μm.
[0012] This invention also proposes a method for preparing the aforementioned battery-resistant PE foam tape, comprising the following steps: S1. Mix and granulate the low-density polyethylene, foaming agent and nucleating agent in the formula, then extrude to make master sheet, then achieve high cross-linking degree through electron beam irradiation, and finally foam in foaming furnace to make foam material layer. S2. First, the crosslinking agent is loaded into the porous material by impregnation, and then the surface is treated with a surface treatment agent to obtain a latent curing agent; the polyacrylic resin masterbatch, tackifying resin and diluent are stirred and mixed evenly, and then the latent curing agent is added to make an acrylic adhesive to be coated. S3. Apply acrylic adhesive to a release film and dry to obtain a first adhesive layer. Transfer the first adhesive layer to one side of the foam material layer. Apply another portion of acrylic adhesive to a release film and dry to obtain a second adhesive layer. Transfer the second adhesive layer to the other side of the foam material layer. Then, dry and cure at 60°C and roll up to obtain a PE foam tape resistant to battery expansion.
[0013] The beneficial effects of this invention are as follows: The foamed material layer (PE foam) prepared by this invention has a density controlled at 80-100 kg / m³. 3 The average pore size is 70-100µm, with uniform pore size distribution (standard deviation ≤ 30% of average pore size), and a closed-cell rate ≥ 90%, preferably ≥ 95%. PE foam in this range exhibits excellent cell structure, with a fine and uniform closed-cell structure, providing a thicker solid foundation for the pore walls and resisting Z-axis compression collapse. Furthermore, the high closed-cell rate provides gas-supported counter-pressure, better dispersing the thrust force generated by battery expansion.
[0014] This invention loads a crosslinking agent into a porous material to form a latent curing agent, which is then added to an acrylic adhesive. The porosity of the latent curing agent allows it to absorb moisture under high temperature and humidity, resulting in the discharge of the curing agent from the pores. The crosslinking agent further crosslinks under high temperature and humidity, thereby improving the aging peel strength of the adhesive layer: after aging for 7 days at 65°C and 95%RH, the peel strength is increased by more than 10% compared to the peel strength at room temperature, and can be increased by up to 45%.
[0015] This invention adds tackifying resin to acrylic adhesive, resulting in excellent initial tack on the inclined surface and excellent rapid bonding performance of the tape.
[0016] This invention combines PE foam with a uniform pore size distribution with a high Tg acrylic adhesive layer, so that when the tape is applied to the simulated test of the expansion of silicon anode battery during charge and discharge, it can withstand the force of about 100% of the battery expansion without popping open or local delamination. Detailed Implementation
[0017] The present application solution will be further described below with reference to specific embodiments.
[0018] A method for preparing a PE foam tape resistant to battery swelling includes the following steps: S1. Mix and granulate the low-density polyethylene, foaming agent and nucleating agent in the formula, then extrude to make master sheet, then achieve high cross-linking degree through electron beam irradiation, and finally foam in foaming furnace to make foam material layer. S2. Soak the crosslinking agent in the porous material and stir for 1 hour. Then, perform surface treatment with a surface treatment agent (KH550) to obtain a latent curing agent. Mix the polyacrylic resin masterbatch, tackifying resin and diluent evenly, and then add the latent curing agent to prepare the acrylic adhesive to be coated. The diluent is used in appropriate amount to adjust the solid content (30-40%) of the acrylic adhesive.
[0019] S3. Apply acrylic adhesive to a release film and dry to obtain a first adhesive layer. Transfer the first adhesive layer to one side of the foam material layer. Apply another portion of acrylic adhesive to a release film and dry to obtain a second adhesive layer. Transfer the second adhesive layer to the other side of the foam material layer. Then, dry and cure at 60-120℃ and roll up to obtain a PE foam tape resistant to battery expansion.
[0020] The polyacrylic acid resin masterbatch has the following formulation: 50g isooctyl acrylate, 40g butyl acrylate, 3g acrylic acid, 1g hydroxyethyl acrylate, 10g methyl methacrylate, 4g isobornyl methacrylate, 115g ethyl acetate, and 0.5g initiator (BPO). This polyacrylic acid resin masterbatch is prepared using existing solution polymerization methods via free radical polymerization.
[0021] Each example and comparative example was prepared according to the formulation in Table 1 and the preparation method described above.
[0022] Table 1 Formulations of each embodiment and comparative example
[0023] In Table 1, the phenolic epoxy resin used was DEN438 manufactured by Dow Chemical Company; the rosin resin used was D-125 manufactured by Arakawa Chemical Company; the dicyandiamide epoxy resin used was AmicureCG-325G manufactured by Evonik Corporation; and the zeolite molecular sieve used was JLOX-5A-15 manufactured by Jianlong Micro-Nano New Materials Co., Ltd.
[0024] The PE foam tapes prepared in each embodiment and comparative example were used as samples for performance testing.
[0025] The testing method is as follows: 1. The peel force test of steel plate shall be conducted using a peel force testing machine, in accordance with GB / T 2792-2014; 2. Peel strength of aged steel plates was tested after being placed at 65℃ and 95%RH for 7 days.
[0026] 3. The battery expansion test uses a whole-machine simulation test method: (1) Following the mobile phone manufacturing process, apply the tape to the designated area (usually around the edge) of the battery back cover. Ensure that there are no bubbles or wrinkles and that the tape is applied accurately.
[0027] (2) Assemble the attached battery back cover onto the middle frame. Place the filler block, which is 0.4-0.6 mm higher than the original battery, in the battery placement area. After standing for 24 hours, place it under 65℃ and 95%RH conditions for 7 days and observe whether the tape delaminates or comes off. The test result "OK" indicates no delamination or coming off, and "NG" indicates delamination or coming off.
[0028] 4. Initial adhesion is achieved using the inclined plane rolling ball method (30° incline), refer to GB / T4852-2002.
[0029] The test results are shown in Table 2: Table 2
[0030] Test results explanation and principle explanation: By comparing the data from Examples 1, 2, and 3 and Comparative Example 1, it was found that using zeolite molecular sieves to design a latent curing agent can further crosslink the tape under conditions of 65°C and 95%RH, improve the aging peel strength, and further improve the degree of crosslinking and peel strength with increasing addition amount.
[0031] By comparing the data from Example 1, Comparative Example 1, and Comparative Example 2, it is demonstrated that the self-made PE foam with uniform pore size distribution can disperse the pushing force caused by battery expansion and can be applied to the use of silicon anode batteries.
[0032] The above preferred embodiments should be regarded as illustrative examples of the embodiments of the present application. Any technical deductions, substitutions, improvements, etc. that are similar to or based on the present application should be considered within the scope of protection of this patent.
Claims
1. A PE foam tape resistant to battery swelling, characterized in that: It includes a first adhesive layer, a foam material layer, and a second adhesive layer that are stacked sequentially; The first adhesive layer and the second adhesive layer are obtained by drying an acrylic adhesive; the acrylic adhesive, by weight, includes 100 parts of polyacrylic acid resin masterbatch, 5-20 parts of tackifying resin, 0.5-3 parts of crosslinking agent, 3-6 parts of porous material, and 0.1-0.15 parts of surface treatment agent; The foamed material layer, by weight, comprises 70-80 parts of low-density polyethylene, 15-25 parts of foaming agent, and 0.5-2 parts of nucleating agent.
2. The PE foam tape for resisting battery swelling according to claim 1, characterized in that: The tackifying resin includes at least one of phenolic epoxy resin, terpene and its derivative resin, and rosin and its derivative resin.
3. The PE foam tape for resisting battery swelling according to claim 1, characterized in that: The crosslinking agent includes at least one of modified imidazole and dicyandiamide epoxy resin.
4. The PE foam tape for resisting battery swelling according to claim 1, characterized in that: The porous material is a zeolite molecular sieve with a pore size of 0.8-1.2 nm.
5. The PE foam tape for resisting battery swelling according to claim 1, characterized in that: The melt index of the low-density polyethylene is 1.5-2.0 g / 10 min.
6. The PE foam tape for resisting battery swelling according to claim 1, characterized in that: The foaming agent is azodicarbonamide, with a particle size of 4-6 μm.
7. The PE foam tape for resisting battery swelling according to claim 1, characterized in that: The nucleating agent includes at least one of talc and calcium carbonate, with a particle size of 1-15 μm.
8. A method for preparing a battery-resistant PE foam tape according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Mix and granulate the low-density polyethylene, foaming agent and nucleating agent in the formula, then extrude to make master sheet, then achieve high cross-linking degree through electron beam irradiation, and finally foam in foaming furnace to make foam material layer. S2. First, the crosslinking agent is loaded into the porous material by impregnation, and then the surface is treated with a surface treatment agent to obtain a latent curing agent; the polyacrylic resin masterbatch, tackifying resin and diluent are stirred and mixed evenly, and then the latent curing agent is added to make an acrylic adhesive to be coated. S3. Apply acrylic adhesive to a release film and dry to obtain a first adhesive layer. Transfer the first adhesive layer to one side of the foam material layer. Apply another portion of acrylic adhesive to a release film and dry to obtain a second adhesive layer. Transfer the second adhesive layer to the other side of the foam material layer. Then, dry and cure at 60-120℃ and roll up to obtain a PE foam tape resistant to battery expansion.