A residue-free, easy-peel adhesive film for textiles and its preparation method

By subjecting PET film to low-temperature plasma treatment and chemical modification, long carbon chains are introduced to enhance the interfacial bonding force between PET film and polyethylene hot melt adhesive, solving the problems of easy residue and insufficient adhesion of traditional adhesives, and realizing easy-to-peel and stable film application.

CN123107566APending Publication Date: 2026-11-17HUIZHOU YIDU STATIONERY SUPPLIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611478586.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional adhesives have problems in textile processing, such as strong adhesion, difficulty in peeling, and easy residue. Polyethylene hot melt adhesive has low adhesion to PET base film, resulting in poor stability.

Method used

By introducing alkenyl and hydroxyl groups into PET film through low-temperature plasma treatment, and by introducing long carbon chains into the PET film surface through the reaction of thiol compounds and chlorosilane compounds, combined with polyethylene hot melt adhesive coating, the interfacial compatibility is enhanced.

Benefits of technology

It significantly improves the adhesion and peel strength between polyethylene hot melt adhesive and PET base film. The hot melt adhesive is easy to peel off without residue, has high stability, and has moderate adhesion to textiles, making it less likely to leave residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of PET film technology and discloses a residue-free, easy-to-peel adhesive film for textiles and its preparation method. The invention involves mixing low-density polyethylene and high-density polyethylene in a mixer, then melt-blending them in a twin-screw extruder. The hot melt adhesive is extruded through a slit die and coated onto one side of a surface-modified PET film. After cooling with a cooling roller, a residue-free, easy-to-peel adhesive film is obtained. The polyethylene hot melt adhesive exhibits excellent adhesion and peel strength to the PET base film, making it difficult to peel off and demonstrating high stability. The polyethylene-based hot melt adhesive does not contain polar functional groups, resulting in low interaction forces with fabrics such as cotton and relatively low peel strength. This low peel strength helps to fix the fabric and prevent shifting. Furthermore, the hot melt adhesive is easily peeled off after adhering to the fabric, leaving no residue on the fabric surface, and the fabric fibers do not adhere to the hot melt adhesive surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of PET film technology, specifically to a residue-free, easy-to-peel adhesive film for textiles and its preparation method. Background Technology

[0002] During the cutting, sewing, and lamination processes of textile fabrics, slippage and misalignment can easily occur, causing problems such as dimensional deviations and distorted patterns. Therefore, it is necessary to quickly and temporarily fix the fabric to limit displacement, and then peel it off after processing. Adhesive films containing adhesives are typically used to bond and fix the fabric. However, traditional adhesives have strong adhesion, making it difficult to peel off the fabric surface after processing, easily leaving adhesive residue, and fibers may also remain on the adhesive film surface.

[0003] Polyethylene hot melt adhesives contain no organic solvents and no polar groups, resulting in low adhesion to textile fabrics. While offering advantages such as easy peeling and no residue, they are typically coated with polyethylene terephthalate (PET) as the base film. However, the adhesion between the PET hot melt adhesive and the PET base film is also low, leading to easy separation and affecting the film's stability. Even introducing polar oxygen-containing functional groups onto the PET film surface through corona treatment or plasma treatment fails to effectively improve its adhesion to non-polar PET hot melt adhesives. Introducing active groups such as maleic anhydride into the PET hot melt adhesive can improve the adhesion between the adhesive and the base film; however, this also increases the adhesion between the hot melt adhesive and the textile fabric, making peeling difficult and leaving residue. Summary of the Invention

[0004] This invention solves the problems of low adhesion between hot melt adhesive and PET base film and high adhesion between hot melt adhesive and fabric textiles.

[0005] This invention first provides a method for preparing a residue-free, easily peelable adhesive film, comprising: (1) Place the cleaned polyethylene terephthalate film in the chamber of the low-temperature vacuum plasma treatment instrument, evacuate, introduce argon gas, perform low-temperature plasma treatment, turn off the power, introduce air, and obtain the pretreated PET film.

[0006] (2) Add a pretreated PET membrane, a thiol compound in a mass ratio of 100:(5-7), and benzoin dimethyl ether to tetrahydrofuran. React under ultraviolet light, remove the membrane, wash with tetrahydrofuran and water, and dry to obtain the modified PET membrane precursor.

[0007] (3) Add the modified PET film precursor to n-hexane, add water dropwise, add chlorosilane compound, react, take out the film, wash the film with n-hexane and water, and dry to obtain the surface modified PET film.

[0008] (4) Mix 60-70 parts by weight of low-density polyethylene (as the matrix of hot melt adhesive), 15-33 parts by weight of high-density polyethylene (to improve melt strength during processing), 7-15 parts by weight of polypropylene (to enhance the rigidity of hot melt adhesive), 15-23 parts by weight of tackifier, and 0.2-0.3 parts by weight of antioxidant in a mixer, then melt-blend in a twin-screw extruder, and extrude the hot melt adhesive through a slit die onto one side of the surface-modified PET film, and cool it with a cooling roller to obtain a residue-free and easy-to-peel adhesive film.

[0009] Preferably, in (1), the pressure of the argon gas-controlled chamber is 10-40 Pa, the discharge power of the low-temperature vacuum plasma treatment instrument is 50-120 W, and the low-temperature plasma treatment time is 20-90 s.

[0010] Preferably, the thiol compound in (2) is dodecanethiol, tetradecanethiol, hexadecethiol or octadecethiol.

[0011] Preferably, the reaction time in (2) is 30-60 min.

[0012] Preferably, the chlorosilane compound in (3) is dodecyltrichlorosilane, tetradecyltrichlorosilane, hexadecyltrichlorosilane, or octadecyltrichlorosilane.

[0013] Preferably, the reaction time in (3) is 3-5 hours.

[0014] Preferably, the tackifier includes hydrogenated C5 petroleum resin and hydrogenated C5 / C9 copolymer petroleum resin.

[0015] Preferably, the antioxidants include antioxidant 1010, antioxidant 1076, antioxidant 1330, and antioxidant 168.

[0016] Preferably, the amount of hot melt adhesive applied is 10-120 g / m². 2 .

[0017] Preferably, the temperature of each zone of the twin-screw extruder is 150-290℃, and the temperature of the slit die is 210-270℃.

[0018] Preferably, the residue-free, easy-to-peel adhesive film is used in textiles.

[0019] The beneficial technical effects of this invention are as follows: Ar low-temperature plasma treatment is applied to the surface of the PET film, causing dehydrogenation of the C=C bonds in the PET to generate carbon free radicals and C=C double bonds. These carbon free radicals react with moisture in the air to generate hydroxyl groups, thereby introducing alkenyl and hydroxyl groups onto the PET film surface. Thiol compounds undergo addition reactions with the alkenyl groups, and chlorosilane compounds react with the hydroxyl groups, resulting in the introduction of numerous long carbon chains onto the PET film surface, thus obtaining a surface-modified PET film. Finally, polyethylene-based hot melt adhesive is extruded and coated onto one side of the surface-modified PET film. The modified PET film introduces numerous long carbon chains onto its surface. During the slit extrusion process, the molten hot melt adhesive and the modified PET film surface exhibit strong interfacial compatibility. The long carbon chains on the PET film surface are embedded in the molten polyethylene molecular chains. After cooling, the interfacial bonding force is enhanced, significantly improving the adhesion and peel strength between the polyethylene hot melt adhesive and the PET base film. The hot melt adhesive is not easily peeled off from the base film, exhibiting high stability.

[0020] The polyethylene-based hot melt adhesive of the present invention does not contain polar functional groups, has low interaction force with fabrics such as cotton fabrics, and has low peel strength. The low peel strength can fix the fabric and prevent it from shifting. At the same time, the hot melt adhesive is easy to peel off after adhering to the fabric, leaving no residue on the fabric surface, and the fabric fibers will not adhere to the hot melt adhesive surface. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the following embodiments. It should be noted that this invention is not limited to the following embodiments.

[0022] The following products are manufactured by Dongguan Zhongxuan Special Plastics Chemical Co., Ltd.: Low-density polyethylene (LDPE), model LD608 (Sinopec); High-density polyethylene (HDPE), model HD55110 (Sinopec Refining & Chemical); Polypropylene, model C180 (Sinopec); and PET film (0.35mm thickness). Example 1

[0023] (1) Place the cleaned polyethylene terephthalate film in the chamber of the low-temperature vacuum plasma treatment instrument, evacuate, introduce argon gas to control the pressure of the chamber to 20Pa, set the discharge power to 100W, perform low-temperature plasma treatment for 60s, turn off the power, introduce air, and obtain the pretreated PET film.

[0024] (2) Add 100 parts by weight of pretreated PET membrane, 5 parts by weight of dodecyl mercaptan, and 0.3 parts by weight of benzoin dimethyl ether to 800 parts by weight of tetrahydrofuran. Irradiate the mixture under ultraviolet light for 30 min. Remove the membrane, wash it with tetrahydrofuran and water, and dry it to obtain the modified PET membrane precursor.

[0025] (3) Add 100 parts by weight of modified PET film precursor to 800 parts by weight of n-hexane, add 3 parts by weight of water, add 8 parts by weight of octadecyltrichlorosilane, react for 4 hours, take out the film, wash the film with n-hexane and water, and dry to obtain surface modified PET film.

[0026] (4) Mix 65 parts by weight of low-density polyethylene, 25 parts by weight of high-density polyethylene, 10 parts by weight of polypropylene, 18 parts by weight of hydrogenated C5 petroleum resin, 0.2 parts by weight of antioxidant 1076, and 0.1 parts by weight of antioxidant 168 in a mixer, and then melt-blend them in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. Extrude the hot melt adhesive through a slit die (die temperature 210°C) onto one side of the surface-modified PET film, controlling the coating amount to be 40 g / m. 2 After being cooled by cooling rollers, a residue-free, easily peelable adhesive film is obtained. Example 2

[0027] (1) Place the cleaned polyethylene terephthalate film in the chamber of the low-temperature vacuum plasma treatment instrument, evacuate, introduce argon gas to control the pressure of the chamber to 40 Pa, set the discharge power to 50 W, perform low-temperature plasma treatment for 90 s, turn off the power, introduce air, and obtain the pretreated PET film.

[0028] (2) Add 100 parts by weight of pretreated PET membrane, 3 parts by weight of dodecyl mercaptan, and 0.15 parts by weight of benzoin dimethyl ether to 800 parts by weight of tetrahydrofuran. Irradiate the mixture under ultraviolet light for 40 min. Remove the membrane, wash it with tetrahydrofuran and water, and dry it to obtain the modified PET membrane precursor.

[0029] (3) Add 100 parts by weight of modified PET film precursor to 800 parts by weight of n-hexane, add 2 parts by weight of water, add 5 parts by weight of octadecyltrichlorosilane, react for 3 hours, take out the film, wash the film with n-hexane and water, and dry to obtain surface modified PET film.

[0030] (4) Mix 70 parts by weight of low-density polyethylene, 20 parts by weight of high-density polyethylene, 10 parts by weight of polypropylene, 23 parts by weight of hydrogenated C5 / C9 copolymer petroleum resin, 0.1 parts by weight of antioxidant 1010, and 0.1 parts by weight of antioxidant 168 in a mixer, and then melt-blend them in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. Extrude the hot melt adhesive through a slit die (die temperature 210°C) onto one side of the surface-modified PET film, controlling the coating amount to be 40 g / m. 2 After being cooled by cooling rollers, a residue-free, easily peelable adhesive film is obtained. Example 3

[0031] (1) Place the cleaned polyethylene terephthalate film in the chamber of the low-temperature vacuum plasma treatment instrument, evacuate, introduce argon gas to control the pressure of the chamber to 40 Pa, set the discharge power to 120 W, perform low-temperature plasma treatment for 20 s, turn off the power, introduce air, and obtain the pretreated PET film.

[0032] (2) Add 100 parts by weight of pretreated PET membrane, 8 parts by weight of octadecyl mercaptan, and 0.56 parts by weight of benzoin dimethyl ether to 900 parts by weight of tetrahydrofuran. Irradiate the mixture under ultraviolet light for 60 min. Remove the membrane, wash it with tetrahydrofuran and water, and dry it to obtain the modified PET membrane precursor.

[0033] (3) Add 100 parts by weight of modified PET film precursor to 900 parts by weight of n-hexane, add 5 parts by weight of water, add 12 parts by weight of dodecyltrichlorosilane, react for 5 hours, take out the film, wash the film with n-hexane and water, and dry to obtain surface modified PET film.

[0034] (4) Mix 70 parts by weight of low-density polyethylene, 15 parts by weight of high-density polyethylene, 15 parts by weight of polypropylene, 15 parts by weight of hydrogenated C5 / C9 copolymer petroleum resin, 0.2 parts by weight of antioxidant 1330, and 0.1 parts by weight of antioxidant 168 in a mixer, and then melt-blend them in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. Extrude the hot melt adhesive through a slit die (die temperature 210°C) onto one side of the surface-modified PET film, controlling the coating amount to be 40 g / m. 2 After being cooled by cooling rollers, a residue-free, easily peelable adhesive film is obtained. Example 4

[0035] (1) Place the cleaned polyethylene terephthalate film in the chamber of the low-temperature vacuum plasma treatment instrument, evacuate, introduce argon gas to control the pressure of the chamber to 10 Pa, set the discharge power to 100 W, perform low-temperature plasma treatment for 60 s, turn off the power, introduce air, and obtain the pretreated PET film.

[0036] (2) Add 100 parts by weight of pretreated PET membrane, 6.5 parts by weight of octadecyl mercaptan, and 0.4 parts by weight of benzoin dimethyl ether to 900 parts by weight of tetrahydrofuran. Irradiate the mixture under ultraviolet light for 60 min. Remove the membrane, wash it with tetrahydrofuran and water, and dry it to obtain the modified PET membrane precursor.

[0037] (3) Add 100 parts by weight of modified PET film precursor to 800 parts by weight of n-hexane, add 4 parts by weight of water, add 10 parts by weight of dodecyltrichlorosilane, react for 5 hours, take out the film, wash the film with n-hexane and water, and dry to obtain surface modified PET film.

[0038] (4) Mix 60 parts by weight of low-density polyethylene, 33 parts by weight of high-density polyethylene, 7 parts by weight of polypropylene, 20 parts by weight of hydrogenated C5 petroleum resin, 0.1 parts by weight of antioxidant 1076, and 0.1 parts by weight of antioxidant 168 in a mixer, and then melt-blend them in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. Extrude the hot melt adhesive through a slit die (die temperature 210°C) onto one side of the surface-modified PET film, controlling the coating amount to be 40 g / m. 2 After being cooled by cooling rollers, a residue-free, easily peelable adhesive film is obtained.

[0039] Comparative Example 1 differs from Example 1 in that a pretreated PET film is used instead of a surface-modified PET film.

[0040] (1) Mix 65 parts by weight of low-density polyethylene, 25 parts by weight of high-density polyethylene, 10 parts by weight of polypropylene, 18 parts by weight of hydrogenated C5 petroleum resin, 0.2 parts by weight of antioxidant 1076, and 0.1 parts by weight of antioxidant 168 in a mixer, and then melt-blend them in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. Extrude the hot melt adhesive through a slit die (die temperature 210°C) onto one side of the pretreated PET film, controlling the coating amount to be 40 g / m. 2 After being cooled by cooling rollers, an adhesive film is obtained.

[0041] Comparative Example 2 differs from Example 1 in that a modified PET film precursor is used instead of a surface-modified PET film.

[0042] (1) 65 parts by weight of low-density polyethylene, 25 parts by weight of high-density polyethylene, 10 parts by weight of polypropylene, 18 parts by weight of hydrogenated C5 petroleum resin, 0.2 parts by weight of antioxidant 1076, and 0.1 parts by weight of antioxidant 168 were mixed in a mixer, and then melt-blended in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. The hot melt adhesive was then extruded and coated onto one side of the modified PET film precursor through a slit die (die temperature 210°C), with the coating amount controlled at 40 g / m. 2 After being cooled by cooling rollers, an adhesive film is obtained.

[0043] Comparative Example 3 differs from Example 1 in that it does not use octadecyl mercaptan for modification.

[0044] (1) Add 100 parts by weight of pretreated PET film to 800 parts by weight of n-hexane, add 3 parts by weight of water, add 8 parts by weight of octadecyltrichlorosilane, react for 4 hours, take out the film, wash the film with n-hexane and water, and dry to obtain surface modified PET film.

[0045] (2) Mix 65 parts by weight of low-density polyethylene, 25 parts by weight of high-density polyethylene, 10 parts by weight of polypropylene, 18 parts by weight of hydrogenated C5 petroleum resin, 0.2 parts by weight of antioxidant 1076, and 0.1 parts by weight of antioxidant 168 in a mixer, and then melt-blend them in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. Extrude the hot melt adhesive through a slit die (die temperature 210°C) onto one side of the surface-modified PET film, controlling the coating amount to be 40 g / m. 2 After being cooled by cooling rollers, an adhesive film is obtained.

[0046] Comparative Example 4 differs from Example 1 in that a polyethylene terephthalate film is used instead of the pretreated PET film.

[0047] (1) Add 100 parts by weight of cleaned polyethylene terephthalate membrane, 5 parts by weight of dodecyl mercaptan, and 0.3 parts by weight of benzoin dimethyl ether to 800 parts by weight of tetrahydrofuran. Irradiate the mixture under ultraviolet light for 30 min. Remove the membrane, wash it with tetrahydrofuran and water, and dry it to obtain a PET membrane. (3) Add 100 parts by weight of PET membrane to 800 parts by weight of n-hexane, add 3 parts by weight of water, add 8 parts by weight of octadecyltrichlorosilane, react for 4 hours, take out the membrane, wash the membrane with n-hexane and water, and dry to obtain PET membrane.

[0048] (4) Mix 65 parts by weight of low-density polyethylene, 25 parts by weight of high-density polyethylene, 10 parts by weight of polypropylene, 18 parts by weight of hydrogenated C5 petroleum resin, 0.2 parts by weight of antioxidant 1076, and 0.1 parts by weight of antioxidant 168 in a mixer, and then melt-blend them in a twin-screw extruder at temperatures of 150°C, 170°C, 185°C, 195°C, and 200°C. Extrude the hot melt adhesive onto one side of the PET film through a slit die (die temperature 210°C), controlling the coating amount to 40 g / m². 2 After being cooled by cooling rollers, an adhesive film is obtained.

[0049] The 180° peel strength between the hot melt adhesive and its own PET film was tested according to the method of GB / T 2792-2014.

[0050] Heat the adhesive film to 120°C, adhere the hot melt adhesive layer of the film to the polyester fabric, cool to room temperature, and test the 180° peel strength between the hot melt adhesive and the fabric according to GB / T 2792-2014 method.

[0051] Table 1 Performance Tests

[0052] In each embodiment, modified PET is used as the base film and polyethylene as the hot melt adhesive layer. The modified PET film incorporates a large number of long carbon chains on its surface. During the slit extrusion process, the molten hot melt adhesive and the modified PET film surface exhibit strong interfacial compatibility. The long carbon chains on the PET film surface intercalate into the molten polyethylene molecular chains. After cooling, the interfacial bonding force is enhanced, significantly improving the adhesion and peel strength between the polyethylene hot melt adhesive and the PET base film. The hot melt adhesive is not easily peeled off from the base film, exhibiting high stability. The polyethylene-based hot melt adhesive does not contain polar functional groups, resulting in weak interaction forces with fabrics such as cotton and relatively low peel strength. This low peel strength helps to fix the fabric and prevent displacement. Furthermore, after adhering to the fabric, the hot melt adhesive is easily peeled off, leaving no residue on the fabric surface, and the fabric fibers do not adhere to the hot melt adhesive surface.

[0053] The modified PET film precursor of Comparative Example 2 and the surface-modified PET film of Comparative Example 3 both have fewer long carbon chains on their surface, resulting in weaker interfacial bonding with the polyethylene hot melt adhesive and thus lower peel strength.

[0054] Comparative Example 4: The polyethylene terephthalate film was not treated with low-temperature plasma and its surface does not contain active functional groups such as alkenyl and hydroxyl groups. It cannot react with dodecyl mercaptan and octadecyltrichlorosilane, making it difficult to introduce long carbon chains on the surface. The interfacial bonding between the PET film and the polyethylene hot melt adhesive is very weak, resulting in very low peel strength.

[0055] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

Claims

1. A method for preparing a residue-free easy peel adhesive film, characterized by, The preparation method includes: mixing 60-70 parts by weight of low-density polyethylene, 15-33 parts by weight of high-density polyethylene, 7-15 parts by weight of polypropylene, 15-23 parts by weight of tackifier, and 0.2-0.3 parts by weight of antioxidant in a mixer, then melt-blending in a twin-screw extruder, and extruding the hot melt adhesive through a slit die to coat one side of the surface-modified PET film, and cooling it with a cooling roller to obtain a residue-free, easy-to-peel adhesive film.

2. The method for preparing a residue-free, easily peelable adhesive film according to claim 1, characterized in that, The tackifier is hydrogenated C5 petroleum resin or hydrogenated C5 / C9 copolymer petroleum resin; the antioxidant includes any one or more of antioxidant 1010, antioxidant 1076, antioxidant 1330, and antioxidant 168.

3. The method for preparing a residue-free, easily peelable adhesive film according to claim 1, characterized in that, The amount of hot melt adhesive coating is 10-120 g / m 2 .

4. The method for preparing a residue-free, easily peelable adhesive film according to claim 1, characterized in that, The temperature of each zone of the twin-screw extruder is 150-290℃, and the temperature of the slit die is 210-270℃.

5. The method for preparing a residue-free, easily peelable adhesive film according to claim 1, characterized in that, The preparation method of the surface-modified PET film is as follows: (1) Place the cleaned polyethylene terephthalate film in the chamber of the low-temperature vacuum plasma treatment instrument, evacuate, introduce argon gas, perform low-temperature plasma treatment, turn off the power, introduce air, and obtain the pretreated PET film. (2) Add pretreated PET membrane, thiol compound and benzoin dimethyl ether in a mass ratio of 100:(5-7) to tetrahydrofuran, irradiate under ultraviolet light for 30-60 min, remove the membrane, wash and dry to obtain modified PET membrane precursor. (3) Add the modified PET film precursor to n-hexane, add water dropwise, add chlorosilane compound, react for 3-5 hours, take out the film, wash, dry, and obtain the surface modified PET film.

6. The method for preparing a residue-free, easily peelable adhesive film according to claim 5, characterized in that, In (1), the pressure of the argon gas-controlled chamber is 10-40 Pa, the discharge power of the low-temperature vacuum plasma treatment instrument is 50-120 W, and the low-temperature plasma treatment time is 20-90 s.

7. The method for preparing a residue-free, easily peelable adhesive film according to claim 5, characterized in that, The thiol compound in (2) is dodecanethiol, tetradecanethiol, hexadecethiol or octadecethiol.

8. The method for preparing a residue-free, easily peelable adhesive film according to claim 5, characterized in that, The chlorosilane compound in (3) is dodecyltrichlorosilane, tetradecyltrichlorosilane, hexadecyltrichlorosilane, or octadecyltrichlorosilane.

9. A residue-free, easily peelable adhesive film obtained by the preparation method according to any one of claims 1-8.