A modified waterborne membrane adhesive, its preparation method and application

By using polyisoprene graft copolymerization technology, a modified aqueous membrane binder with flexible main chain crosslinking was prepared, which solved the problems of loss of adhesion, thermal shrinkage and electrolyte swelling of lithium-ion battery membranes at high temperatures, and achieved high temperature stability and environmental friendliness, making it suitable for power batteries and energy storage batteries.

CN123107590APending Publication Date: 2026-11-17HUNAN LINTE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611518700.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion battery separator adhesives are prone to loss of adhesion at high temperatures, thermal shrinkage, and poor resistance to electrolyte swelling. Furthermore, their production is not environmentally friendly enough, making it difficult to meet the high safety and long life requirements of power batteries and energy storage batteries.

Method used

Using polyisoprene as the grafted main chain, hard monomers, carboxyl monomers and amide monomers are copolymerized to form a synergistic structure of cross-linking within the flexible main chain and heat-resistant support from the hard monomers. Combined with water-based processing technology, a modified waterborne membrane adhesive is prepared.

Benefits of technology

It maintains good bonding strength and dimensional stability at high temperatures, is resistant to electrolyte swelling, and has excellent environmental performance, making it suitable for power batteries and energy storage batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention belongs to the technical field of lithium-ion battery separators and water-based binders, specifically disclosing a modified water-based separator binder, its preparation method, and its application. The binder uses polyisoprene as the grafted main chain, copolymerized with grafted hard monomers, carboxyl monomers, and amide monomers. By dry weight, its raw material composition includes 20-45 parts polyisoprene, 25-50 parts hard monomers, 10-25 parts carboxyl monomers, and 5-18 parts amide monomers. The preparation method is also disclosed. The binder is combined with boehmite to prepare a ceramic slurry, which is then coated onto the surface of a polyolefin-based membrane to obtain a heat-resistant ceramic-coated separator. The longitudinal and transverse thermal shrinkage rates at 180℃ / 1h are both ≤2%, and the peel strength is ≥110 N / m. This invention, through the synergy of flexible main chain crosslinking and the heat-resistant support of hard monomers, balances toughness, heat resistance, and adhesion performance. The entire process is water-based, exhibiting excellent environmental friendliness, and is suitable for power and energy storage battery applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery separators and aqueous binders, and particularly to a modified aqueous separator binder, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries, due to their high energy density and long cycle life, have been widely used in electric vehicles, energy storage systems, and portable electronic devices. As a key component of lithium-ion batteries, the separator's performance directly affects the battery's safety and reliability. Traditional polyolefin (PE / PP) separators experience significant thermal shrinkage above 130°C, easily leading to direct contact between the positive and negative electrodes, causing internal short circuits and ultimately thermal runaway. Therefore, coating the polyolefin base membrane with a ceramic coating containing inorganic ceramic particles (such as boehmite and alumina) effectively improves the high-temperature dimensional stability of the separator. Ceramic-coated separators have become the mainstream technology in the fields of power batteries and energy storage batteries.

[0003] The performance of ceramic-coated separators largely depends on the choice of binder. Currently, commercial ceramic binders are mainly divided into two categories: oil-based and water-based systems. Oil-based systems are dominated by PVDF, but their processing requires the use of organic solvents such as N-methylpyrrolidone (NMP), which is not only environmentally unfriendly and costly, but also suffers from significant adhesion degradation at high temperatures, easily leading to ceramic layer detachment above 180°C. Water-based systems are represented by polyacrylates and styrene-butadiene rubber (SBR). Polyacrylate binders have a low glass transition temperature, softening and losing adhesion above 130°C, resulting in ceramic layer pulverization and detachment. While SBR binders have good adhesion, they have poor resistance to electrolyte swelling, leading to a significant increase in battery impedance after long-term cycling, and insufficient high-temperature dimensional stability.

[0004] In addition, although there are waterborne binder solutions such as styrene-acrylate copolymer and acrylamide-modified acrylic acid in the existing technology, these solutions generally have the following defects: (1) lack of flexible main chain toughening design, the high proportion of hard monomers leads to coating embrittlement, and powder is easy to fall off after bending; (2) no effective internal cross-linking structure is provided in the copolymer, the molecular chain is easy to slide at high temperature, and the heat resistance is insufficient; (3) binders containing polyisoprene are mainly used in electrode systems, and are mainly random copolymers of isoprene monomers. There are no reports on the preparation of waterborne binders for membranes using polyisoprene emulsion as graft main chain and simultaneous composite hard monomer / carboxyl monomer / amide monomer.

[0005] Therefore, developing a water-based ceramic diaphragm adhesive that combines excellent high-temperature heat resistance, high bonding strength, good electrolyte resistance, and environmental friendliness has become an urgent technical problem to be solved in this field. Summary of the Invention

[0006] In view of the above-mentioned problems, the present invention provides a modified water-based membrane adhesive, its preparation method, and its application. The present invention, through a synergistic structural design of flexible main chain intra-linking and hard monomer heat-resistant support, balances coating toughness, high-temperature heat resistance, and adhesion performance. Furthermore, the entire process is water-based, exhibiting excellent environmental friendliness, and is suitable for the fields of power batteries and energy storage batteries.

[0007] To address the aforementioned problems, this invention provides a modified waterborne membrane adhesive, which is copolymerized with polyisoprene as the grafted main chain and grafted with hard monomers, carboxyl monomers and amide monomers. The raw material composition of the aqueous membrane adhesive, based on dry weight, includes: 20-45 parts of polyisoprene; 25-50 parts of hard monomer; 10-25 parts of carboxyl monomer; 5-18 parts of amide monomer; The hard monomer is styrene and / or acrylonitrile; The carboxyl monomer is a monomer containing a carboxyl group or capable of hydrolyzing to produce a carboxyl group, selected from one or more of methacrylic acid, acrylic acid, itaconic acid, and maleic anhydride, wherein the maleic anhydride can be hydrolyzed to produce a carboxyl group during the polymerization process; The amide monomer is selected from one or more of acrylamide, methacrylamide, N-hydroxymethylacrylamide, and N-isobutoxyacrylamide.

[0008] Preferably, the raw material composition, based on dry weight, includes: 25-40 parts of polyisoprene, 28-45 parts of hard monomer, 12-20 parts of carboxyl monomer, and 8-15 parts of amide monomer.

[0009] Preferably, the raw material composition further includes 0.2 to 1.2 parts of initiator, 1.5 to 4 parts of emulsifier, neutralizer, and deionized water; The initiator is selected from one of ammonium persulfate, sodium persulfate, potassium persulfate, and azobisisobutyramidine hydrochloride; The emulsifier is selected from one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and alkylphenol polyoxyethylene ether; The neutralizing agent is selected from one of ammonia, sodium hydroxide, lithium hydroxide, and triethylamine; The amount of deionized water used results in a solid content of 20% to 40% for the aqueous membrane adhesive.

[0010] Preferably, the grafting rate of the polyisoprene is 82% to 95%.

[0011] Based on the same inventive concept, the present invention also provides a method for preparing a modified aqueous membrane adhesive as described in any of the above claims, comprising the following steps: (1) Preparation of base emulsion: The first part of deionized water and the first part of emulsifier are put into the reaction vessel, and polyisoprene emulsion is added and stirred to form base emulsion; Mechanism: Polyisoprene emulsion is a commercially available water-based polyisoprene latex. Its latex particles contain highly cis-1,4-polyisoprene molecular chains with numerous unsaturated carbon-carbon double bonds (-C=C-). In the presence of an emulsifier, anionic emulsifier molecules (such as sodium dodecyl sulfate) are adsorbed onto the surface of the polyisoprene latex particles. The hydrophilic groups face the aqueous phase, while the hydrophobic segments are anchored to the latex particle surface. Through electrostatic repulsion and steric hindrance, the latex particles are stably dispersed in the aqueous phase.

[0012] (2) Preparation of pre-emulsion: The remaining deionized water, the remaining emulsifier, hard monomer, carboxyl monomer, and amide monomer are mixed evenly by stirring to obtain the pre-emulsion; Mechanism: Under stirring and shearing action, highly hydrophobic hard monomers (styrene, acrylonitrile) and highly hydrophilic carboxyl and amide monomers form mixed monomer droplets under the action of emulsifier molecules. Emulsifier molecules adsorb onto the surface of the monomer droplets, with their hydrophobic segments extending into the oil phase and their hydrophilic groups facing the aqueous phase. This reduces the interfacial tension between the oil and water, stabilizing the monomer droplets in the aqueous phase. The average particle size and size distribution of the monomer droplets directly affect the monomer mass transfer rate in subsequent polymerization reactions and the structural uniformity of the graft copolymer.

[0013] It is worth emphasizing that the process design of preparing the base emulsion and pre-emulsion in separate reactors in this invention has significant technical implications: on the one hand, separating the polyisoprene backbone from the mixed monomers avoids excessive swelling of the polyisoprene latex particles by the monomers at room temperature, effectively controlling the graft polymerization reaction to occur only inside and on the surface of the latex particles, and preventing excessive formation of homopolymers; on the other hand, separate reactor preparation ensures that the monomer droplets in the pre-emulsion achieve the most complete dispersion and stability under conditions where there is no competitive emulsifier adsorption from the polyisoprene latex particles, laying the foundation for subsequent "semi-continuous droplet addition" polymerization.

[0014] (3) Graft polymerization reaction: Nitrogen gas is introduced into the reactor to remove oxygen, and the temperature is raised to 65~85℃; the initiator and the pre-emulsion are added dropwise to the reactor simultaneously, and the reaction is maintained at the temperature after the addition is completed; Mechanism of nitrogen purging: The purpose of introducing nitrogen into the reactor is to remove dissolved oxygen from the reaction system. Oxygen is a strong inhibitor of free radical polymerization. Its inhibition mechanism is as follows: Oxygen can undergo rapid addition reactions with primary free radicals or chain-growing free radicals to form peroxy radicals (R-OO·). The activity of peroxy radicals is much lower than that of carbon-center free radicals, making it difficult to continue initiating monomer polymerization, thus leading to a significant decrease in the polymerization rate or even complete termination. By purging dissolved oxygen from the system with nitrogen, it is ensured that the primary free radicals generated by the decomposition of the initiator can efficiently initiate monomer polymerization, guaranteeing the smooth progress of the polymerization reaction.

[0015] Mechanism of initiator decomposition and primary free radical generation: The initiators selected in this invention (ammonium persulfate, sodium persulfate, potassium persulfate, and azobisisobutyramidine hydrochloride) are all water-soluble, thermally decomposable initiators, and their decomposition mechanism is as follows: Persulfates (taking ammonium persulfate as an example) undergo thermal decomposition under heating conditions: S₂O₈ 2- → 2SO4 - This decomposition reaction is a first-order reaction, and the decomposition rate depends on temperature. Each sulfate radical (SO4) - • It has strong oxidizing properties and high reactivity, and can extract electrons or hydrogen atoms from compounds containing unsaturated bonds or active hydrogen to generate corresponding free radicals.

[0016] Azo initiators (taking azobisisobutyramidine hydrochloride as an example, V-50) undergo homolytic decomposition of the CN bond under heating conditions: RN=NR→2R·+N2↑. The amidine cationic free radicals generated by their decomposition have high initiation activity and good water solubility due to their positive charge, making them suitable for aqueous polymerization systems.

[0017] The decomposition rate of initiators is closely related to temperature: the higher the temperature, the larger the decomposition rate constant, and the higher the concentration of free radicals generated per unit time. This invention controls the polymerization temperature between 65 and 85°C. Within this temperature range, the initiator has a moderate decomposition half-life, enabling it to continuously and stably generate free radicals during the 2.5–4 h dropwise addition process, thus maintaining the smooth progress of the polymerization reaction.

[0018] Chain initiation and chain growth—the mechanism of graft copolymerization: The graft copolymerization reaction of this invention occurs both inside and on the surface of polyisoprene latex particles, and its core chemical reaction includes the following two pathways: Pathway 1: Double bond addition initiation pathway. Primary free radicals generated from the decomposition of the initiator (primarily sulfate radicals SO42-) -(Taking as an example) First, the unsaturated carbon-carbon double bond (-C=C-) on the polyisoprene molecular chain is attacked, undergoing an addition reaction with one carbon atom of the double bond, causing the double bond to open and generating a new free radical active center on the other carbon atom, namely the polyisoprene macromolecular free radical. This macromolecular free radical further undergoes an addition reaction with hard monomers, carboxyl monomers, or amide monomers, with the monomer molecules inserting between the macromolecular free radical and the double bond, achieving chain growth and forming graft copolymer segments. In this process, the polyisoprene molecular chain acts as the "graft backbone," with hard monomers (styrene / acrylonitrile) grafted onto the backbone in the form of rigid segments, giving the copolymer a high glass transition temperature; carboxyl monomers are grafted in the form of carboxyl-containing segments, providing adhesive functionality; and amide monomers are grafted in the form of amide-containing segments, providing self-crosslinking active sites. The pathway is illustrated below: (1) Initiator decomposition: S2O8 2- →2SO4 - ·; (2) Activation of double bonds in the main chain: ~P~CH2-C(CH3)=CH-CH2~+ SO4 - ·→~P~CH2-C·(CH3)-CH(SO4 - )-CH2~; (3) Chain growth (taking styrene as an example): ~P~CH2-C·(CH3)-CH(SO4) - )-CH2~ +nCH2=CH(C6H5)→~P~CH2-C(CH3)-[CH2-CH(C6H5)]n-CH(SO4 - )-CH2~; (4) Chain growth (taking methacrylic acid as an example): ~P~CH2-C·(CH3)-CH(SO4) - )-CH2~+mCH2=C(CH3)-COOH→~P~CH2-C(CH3)-[CH2-C(CH3)(COOH)] m -CH(SO4 - )-CH2~; Pathway 2: α-Methylene hydrogen abstraction initiation pathway. The primary free radicals generated from the initiator decomposition can also attack the hydrogen atom on the α-methylene (-CH2-) group next to the double bond in the polyisoprene molecular chain, undergoing a hydrogen abstraction reaction to generate water molecules and a polyisoprene macromolecular free radical. The active center of this macromolecular free radical is located on the carbon atom of the main chain, and it can also initiate the graft polymerization of the monomer. The mechanism of this pathway is as follows: (1) Hydrogen abstraction of α-methylene: ~P~CH2-C(CH3)=CH-CH2~+SO4 - ·→~P~CH·-C(CH3)=CH-CH2~+HSO4 - ; (2) Graft chain growth: ~P~CH·-C(CH3)=CH-CH2~+monomer→~P~CH(monomer)-C(CH3)=CH-CH2~; Compared with Pathway 1, Pathway 2 does not consume the unsaturated double bonds on the polyisoprene backbone, but it can also form grafting active sites on the backbone to achieve graft copolymerization of hard monomers and functional monomers.

[0019] The mechanism of simultaneous internal crosslinking reaction: During graft polymerization, unsaturated double bonds on the polyisoprene molecular chain can undergo intermolecular crosslinking reactions under the action of an initiator. Specifically, the double bonds on polyisoprene molecular chain A form macromolecular free radicals under free radical initiation, which then undergo addition reactions with the double bonds on another polyisoprene molecular chain B, forming a carbon-carbon single bond crosslinking structure between the two chains and releasing new free radical active centers to continue the reaction. This crosslinking reaction connects multiple polyisoprene backbones through chemical bonds, forming an intermolecular crosslinking network.

[0020] Kinetic mechanism of simultaneous dropwise addition process: This invention adopts a "semi-continuous" feeding method in which the initiator aqueous solution and the pre-emulsion are simultaneously added dropwise to the reaction vessel, which has the following mechanism: Traditional "one-time addition" methods cause a sudden increase in monomer concentration in the reaction system, leading to excessively rapid polymerization rates, concentrated release of polymerization heat, and a tendency for "explosive polymerization," resulting in a broadened molecular weight distribution and uneven grafting structures. This invention, however, uses a slow, synchronous dropwise addition over 2.5–4 hours, allowing monomers to continuously enter the reaction system at a low, constant rate, maintaining a low steady-state monomer concentration. Under these conditions, the free radical polymerization of the monomer proceeds smoothly, and the heat of polymerization can be promptly removed through the reactor jacket, avoiding localized overheating and gelation effects. Simultaneously, the continuously and slowly added monomers preferentially undergo chain growth at the large molecular free radical active centers already formed inside and on the surface of the polyisoprene latex particles, reducing the probability of homopolymer formation and thus improving grafting efficiency.

[0021] The design of simultaneous initiator addition also plays a crucial role: if the initiator is added all at once, the free radical concentration will be too high in the early stage, intensifying the homopolymerization reaction; conversely, the free radical concentration will be too low in the later stage, leading to a decrease in the reaction rate. Simultaneous addition allows the initiator to continuously and uniformly decompose and generate active free radicals throughout the polymerization process, maintaining the continuity of the chain growth reaction and ensuring a monomer conversion rate of ≥96%.

[0022] The mechanism of the heat preservation reaction step: After the monomer is added dropwise, the core purpose of heat preservation for 2-5 hours is to allow the small amount of residual monomer in the reaction system to continue to fully polymerize, further increasing the monomer conversion rate to over 96%. During this stage, as the monomer concentration gradually decreases, the polymerization rate gradually slows down, but the chain growth reaction continues, and the residual monomer molecules continue to diffuse and add to the active chain ends, eventually being consumed. Furthermore, the heat preservation stage provides sufficient time and temperature conditions for the internal crosslinking reaction of the remaining double bonds on the polyisoprene backbone and for possible pre-crosslinking reactions between amide monomers, resulting in a more complete and uniform crosslinking network.

[0023] (4) Neutralization and post-treatment: After the reaction is completed, the temperature is lowered, a neutralizing agent is added to adjust the pH of the system to 7.0~9.0, the material is filtered out, and the polyisoprene modified waterborne membrane adhesive is obtained.

[0024] Mechanism of neutralization post-treatment: After the graft polymerization reaction, the carboxyl monomer segments in the reaction system contain a large number of carboxyl (-COOH) functional groups. These carboxyl groups can form physical crosslinks through hydrogen bonding, leading to increased viscosity and decreased stability of the emulsion system. This step adjusts the pH of the system to 7.0-9.0 by adding a neutralizing agent (ammonia, sodium hydroxide, lithium hydroxide, or triethylamine), causing the carboxyl groups to neutralize and generate the corresponding carboxylates (-COOH). - M + Carboxylate ions carry a negative charge, and their charge repulsion effectively weakens hydrogen bond association between polymer chains. Simultaneously, the strong hydrophilicity of carboxylate ions helps maintain the dispersion stability of polymer particles in the aqueous phase. Taking ammonia neutralization as an example, the reaction mechanism is: -COOH + NH3·H2O → -COO - NH 4+ +H2O. It is worth noting that the degree of neutralization directly affects the thickening behavior and coating performance of the binder. If the pH is too low, the degree of carboxyl group ionization is high, hydrogen bonding is strong, and the system viscosity is too high, which is detrimental to subsequent slurry preparation. If the pH is too high, excessive neutralizing agent may affect the interfacial interaction between the binder and boehmite. This invention controls the pH within a weakly alkaline range of 7.0 to 9.0, ensuring sufficient ionization of carboxyl groups while avoiding the adverse effects of excessive neutralization.

[0025] Preferably, in step (1), the amount of the first part of deionized water is 60% to 75% of the total water volume, and the amount of the first part of emulsifier is 70% of the total emulsifier volume; the stirring speed is 250 to 350 rpm (the purpose is to ensure that the polyisoprene emulsion is fully and evenly mixed with the deionized water and emulsifier to form a stable base emulsion, while avoiding excessively high shear rates that could cause latex particles to break or widen the particle size distribution, thus providing a seed system with good reactivity and dispersion stability for subsequent graft polymerization). In step (2), the stirring time is 30-45 minutes, the purpose of which is to ensure that each monomer component is fully and evenly dispersed in the aqueous phase to form a stable pre-emulsion.

[0026] In step (3), the initiator is prepared as a 5wt% aqueous solution and added dropwise over a period of 2.5 to 4 hours, and the reaction is kept at a constant temperature for 2 to 5 hours.

[0027] Based on the same inventive concept, the present invention also provides a heat-resistant ceramic-coated diaphragm, comprising a polyolefin base film and a ceramic coating coated on at least one side of the base film; The ceramic coating is formed by coating and drying a ceramic slurry, wherein the solid components of the ceramic slurry include: 100 portions of Boehmite; 6-12 parts of the modified aqueous membrane adhesive as described in any one of claims 1 to 4; Dispersant 0.8~1.5 parts; Wetting agent 0.2~0.8 parts; The ceramic slurry also contains deionized water, and the amount of deionized water used makes the solid content of the ceramic slurry 35%~45%. The diaphragm exhibits longitudinal and transverse thermal shrinkage rates of ≤2% after being kept at 180℃ for 1 hour, and a peel strength of ≥110N / m.

[0028] Preferably, the boehmite has a D50 of 0.5~1.5μm; the ceramic slurry has a solid content of 35%~45%; the polyolefin-based film has a thickness of 9~12μm; and the single-sided ceramic coating has a thickness of 2~4μm.

[0029] Based on the same inventive concept, the present invention also provides a method for preparing the heat-resistant ceramic-coated diaphragm described in any of the above claims, comprising the following steps: (1) Preparation of ceramic slurry: Boehmite and dispersant are added to deionized water for dispersion, wetting agent and the aqueous membrane binder are added, dispersion is continued, and after filtration and defoaming, ceramic coating slurry is obtained; (2) Coating and drying: The ceramic coating slurry is coated on one or both sides of the polyolefin base membrane and dried by segmented gradient heating to obtain the heat-resistant ceramic coated diaphragm.

[0030] Preferably, in step (1), the dispersion speed is 1500~2000 rpm and the dispersion time is 30 min; in step (2), the coating method is microgravure coating or slot coating; the segmented gradient heating and drying is carried out at 60℃, 80℃ and 100℃ respectively.

[0031] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Compared with existing water-based polyacrylate adhesives, which soften and lose adhesion above 130°C and have a heat shrinkage rate of over 12% at 180°C (e.g., MD 12.3% and TD 14.5% in Comparative Example 9), resulting in large-area powdering and peeling of the coating; traditional oil-based PVDF systems also show severe attenuation of adhesion at 180°C, with heat shrinkage rates of MD reaching 5.5% and TD reaching 6.3% (Comparative Example 8). This invention constructs a dense three-dimensional chemical crosslinking network through the triple synergistic effect of the intermolecular crosslinking reaction of unsaturated double bonds on the polyisoprene backbone under free radical initiation, the high glass transition temperature (Tg of homopolymers are 100°C and 104°C) of the grafted segments of hard monomers (styrene / acrylonitrile) significantly restricting the rotational freedom within the molecular chain, and the condensation reaction of hydroxymethyl (-CH2OH) groups of amide monomers (especially N-hydroxymethylacrylamide) during gradient drying to form ether bonds (-CH2-O-CH2-) crosslinking structures. The high-temperature dimensionally stable skeleton of boehmite inorganic heat-resistant filler is combined with the longitudinal and transverse thermal shrinkage rates of the separator after being kept at 180°C for 1 hour, which are both controlled within 2% (MD 1.2%~1.8% and TD 1.1%~1.7% in Examples 5~8). This completely solves the industry pain point of failure of the existing system under extreme high temperature and meets the stringent requirements of high safety of power batteries. (2) In contrast to existing technologies, although a high proportion of hard monomers can improve heat resistance, the coating becomes severely brittle and easily sheds powder after bending (e.g., the 7-styrene-propylene ternary system in Comparative Example 7 showed significant powder shedding after bending); while SBR-type adhesives have decent adhesion but insufficient dimensional stability at high temperatures. In this invention, polyisoprene serves as a flexible rubber-like main chain. Its molecular chain segments have high flexibility and mobility at room temperature, and can effectively dissipate external force energy through the extension, orientation, and slippage of the molecular chains; at the same time, the double bond internal crosslinking forms a network structure with a moderate crosslinking density, which not only gives the coating overall structural integrity but also retains the deformation capability of the flexible chain segments, achieving a toughening effect that combines rigidity and flexibility. More importantly, the carboxyl (-COOH) functional groups provided by the carboxyl monomer can undergo condensation or coordination reactions with the hydroxyl (-OH) groups on the surface of boehmite (AlOOH) during the drying process, forming aluminum carboxylate chemical bonds with both monocoordinate and bridged coordination structures. Simultaneously, the carbonyl oxygen and hydroxyl hydrogen of the carboxyl group can form hydrogen bonds with the hydroxyl groups on the boehmite surface and the polar groups on the polyolefin film surface. This synergistic effect of chemical bonding and hydrogen bonding enables the coating peel strength to reach over 110 N / m (112-125 N / m in Examples 5-8), and the coating does not peel off after bending or immersion in electrolyte, overcoming the defects of embrittlement and powdering while improving heat resistance. (3) Although the adhesion of the existing SBR system is acceptable, the rubber phase is prone to swelling in carbonate electrolyte. After immersion in electrolyte at 85°C, the coating swells significantly (Comparative Example 12), resulting in a significant increase in impedance during battery cycling. Ordinary polyacrylate systems also have insufficient resistance to electrolytes. This invention forms a three-dimensional network with high crosslinking density through a dual crosslinking structure of polyisoprene double bond internal crosslinking and amide group high-temperature self-crosslinking. This network connects polymer segments through chemical bonds, effectively restricting the free movement and extension of the segments in the electrolyte and inhibiting the penetration of solvent molecules and polymer swelling. At the same time, the benzene ring structure of styrene and the polar nitrile group of acrylonitrile in the hard monomer have a large interaction parameter with the Flory-Huggins of carbonate electrolytes, resulting in a high mixing free energy between polymer segments and electrolyte molecules. This thermodynamic incompatibility combined with the kinetic restriction of the crosslinking network gives the binder excellent resistance to electrolyte swelling. Experimental results show that the coating of the separator of the present invention does not shed powder or swell after being immersed in electrolyte at 85°C for 72 hours, and its impedance remains stable during long-term cycling. It is suitable for high-safety and long-life power battery and energy storage battery systems. (4) Compared with the existing oil-based PVDF system, which requires the use of organic solvents such as NMP, resulting in high VOC emissions, complex solvent recovery processes, and high production costs, the present invention uses water as the medium throughout the synthesis of the binder and the preparation of the ceramic slurry. The VOC emissions are extremely low, the slurry has good rheological properties and coating adaptability, and industrial production can be achieved without modifying existing coating production lines. The economic and social benefits are significant. (5) Unlike existing schemes that use isoprene monomers for random copolymerization and technical routes that only use polyisoprene as electrode binder, this invention uses pre-made polyisoprene emulsion as the grafting main chain, utilizes its unsaturated double bonds and α-methylene sites to simultaneously carry out graft copolymerization and internal crosslinking, and creatively realizes the synergistic combination of four components: polyisoprene (flexible toughening + internal crosslinking), hard monomer (heat resistant rigidity), carboxyl monomer (chemical bonding), and amide monomer (high temperature self-crosslinking). The comprehensive performance far exceeds that of existing technical solutions, and has outstanding substantive features and significant progress.

[0032] In summary, this invention, starting from molecular structure design, effectively solves long-standing technical problems in existing technologies through an innovative combination of multiple cross-linked networks and the synergistic effect of functional groups, achieving significant technological progress and possessing broad application prospects and industrialization value. Detailed Implementation

[0033] To make the present invention easier to understand, specific embodiments are described below to further illustrate the invention. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise defined, the technical terms used below have the same meaning as understood by those skilled in the art; unless otherwise specified, the raw materials and reagents involved herein can be purchased commercially or obtained by known methods.

[0034] To address the problems mentioned in the background section, this invention provides a modified water-based membrane adhesive, its preparation method, and its applications. This invention, through a synergistic structural design of flexible main-chain intra-linking and hard monomer heat-resistant support, balances coating toughness, high-temperature heat resistance, and adhesion performance. Furthermore, the entire process is water-based, exhibiting excellent environmental friendliness, making it suitable for power batteries and energy storage batteries.

[0035] The following examples and comparative models further illustrate this point.

[0036] In the following examples and comparative examples, all raw materials used were commercially available analytical grade products. The polyisoprene emulsion was a commercially available aqueous polyisoprene latex (solid content 50%~60%), filtered through a 200-mesh screen before use. Boehmite (D50=0.5~1.5μm) was purchased from commercial sources. The dispersant was a sodium polyacrylate dispersant, and the wetting agent was an acetylenic diol wetting agent.

[0037] In all embodiments, "parts" refers to dry basis mass parts. Polyisoprene is added in the form of a polyisoprene emulsion, and the amount added is converted to dry basis mass parts based on the emulsion solid content; hard monomers, carboxyl monomers, and amide monomers are added directly in monomer form.

[0038] The solid content of the adhesive was determined according to GB / T 2793-1995 "Determination of Non-volatile Matter Content in Adhesives"; the grafting rate was determined as follows: an appropriate amount of graft copolymer emulsion was taken, ethanol was added to break the emulsion and precipitate, the precipitate was separated by filtration, washed, and dried in a vacuum oven at 50℃ to constant weight, and the mass of the crude product W0 was weighed; the crude product was placed in a Soxhlet extractor and extracted by reflux with acetone as solvent for 24 hours to remove ungrafted homopolymer; the extracted product was dried in a vacuum oven at 50℃ to constant weight, and the mass of the pure graft copolymer W2 was weighed; the grafting rate was calculated according to the following formula: grafting rate (%) = (W2-W1) / W1×100%. Wherein, W1 is the amount of polyisoprene fed (dry basis mass).

[0039] Preparation of polyisoprene-modified waterborne membrane adhesive: Example 1 A polyisoprene-modified waterborne membrane adhesive: The raw material ratio, based on dry weight, is as follows: 30 parts polyisoprene (added in the form of polyisoprene emulsion, dry weight), 35 parts styrene, 18 parts methacrylic acid, 12 parts acrylamide; 0.6 parts initiator (ammonium persulfate), 2.5 parts emulsifier (sodium dodecyl sulfate); and ammonia water as neutralizer.

[0040] The preparation method of the above-mentioned polyisoprene modified waterborne membrane adhesive includes the following steps: (1) Preparation of base emulsion: Deionized water accounting for 70wt% of the total water volume and sodium dodecyl sulfate accounting for 70wt% of the total emulsifier volume are added to a reaction vessel with stirring and temperature control, and polyisoprene emulsion is added. Stir at 250~350rpm for 20min to form a uniform base emulsion. (2) Preparation of pre-emulsion: Mix the remaining 30% of deionized water, the remaining 30% of emulsifier with styrene, methacrylic acid and acrylamide evenly, and stir for 30~45min to obtain a stable pre-emulsion; (3) Graft polymerization reaction: Nitrogen gas was introduced into the reactor to remove oxygen for 30 minutes, and the temperature was raised to 75°C; ammonium persulfate was prepared into a 5wt% aqueous solution and added dropwise to the reactor simultaneously with the pre-emulsion obtained in step (2) for 3 hours; after the addition was completed, the reaction was kept at the temperature for 3.5 hours. The monomer conversion rate was 97.2% and the polyisoprene grafting rate was 88%. (4) Neutralization and post-treatment: After the reaction is completed, the temperature is lowered to below 40°C, and ammonia water solution is slowly added dropwise to adjust the pH of the system to 8.0; stirring is continued for 30 minutes, and the material is filtered through a 120-mesh filter to obtain polyisoprene modified waterborne membrane adhesive emulsion with a solid content of 30%.

[0041] Example 2 A polyisoprene-modified waterborne membrane adhesive: The raw material ratio, based on dry weight, is as follows: 25 parts polyisoprene (added in the form of polyisoprene emulsion, on a dry basis), 40 parts acrylonitrile, 15 parts acrylic acid, 10 parts N-hydroxymethylacrylamide; 0.7 parts initiator (azobisisobutyramidine hydrochloride), 3 parts emulsifier (alkylphenol polyoxyethylene ether); and triethylamine as neutralizer.

[0042] The preparation method of the above-mentioned polyisoprene modified waterborne membrane adhesive differs from that in Example 1 in that: The polymerization temperature in step (3) was 70℃, the monomer addition time was 2.5h, and the holding time was 4h. The monomer conversion rate was 96.5%, and the polyisoprene grafting rate was 85%. After neutralization in step (4), the pH of the system was adjusted to 7.5, and the binder emulsion solid content was 35%.

[0043] The proportions of the remaining raw materials and the preparation process are the same as in Example 1.

[0044] Example 3 A polyisoprene-modified waterborne membrane adhesive: The raw material ratio, based on dry weight, is as follows: 40 parts polyisoprene (added in the form of polyisoprene emulsion, dry weight), 28 parts styrene, 12 parts itaconic acid, 15 parts methacrylamide; 0.5 parts initiator (potassium persulfate), 2 parts emulsifier (sodium dodecylbenzenesulfonate); and sodium hydroxide as neutralizer.

[0045] The preparation method of the above-mentioned polyisoprene modified waterborne membrane adhesive differs from that in Example 1 in that: The polymerization temperature in step (3) was 80℃, the monomer addition time was 3.5h, and the holding time was 2.5h. The monomer conversion rate was 96.8%, and the polyisoprene grafting rate was 92%. After neutralization in step (4), the pH of the system is adjusted to 8.5, and the binder emulsion solid content is 25%.

[0046] The proportions of the remaining raw materials and the preparation process are the same as in Example 1.

[0047] Example 4 A polyisoprene-modified waterborne membrane adhesive: The raw material ratio, based on dry weight, is as follows: 35 parts polyisoprene (added in the form of polyisoprene emulsion, dry weight), 35 parts styrene and acrylonitrile (mass ratio 1:1), 16 parts methacrylic acid and itaconic acid (mass ratio 2:1), 14 parts N-isobutoxyacrylamide; 0.8 parts initiator (ammonium persulfate), 3 parts emulsifier (a mixture of sodium dodecyl sulfate and alkylphenol polyoxyethylene ether (mass ratio 1:1)); and lithium hydroxide as the neutralizing agent.

[0048] The preparation method of the above-mentioned polyisoprene modified waterborne membrane adhesive differs from that in Example 1 in that: The polymerization temperature in step (3) was 72℃, the monomer addition time was 3 hours, and the reaction time was 3 hours. The monomer conversion rate was 97.5%, and the polyisoprene grafting rate was 90%. After neutralization in step (4), the pH of the system was adjusted to 8.2, and the binder emulsion solid content was 28%.

[0049] The proportions of the remaining raw materials and the preparation process are the same as in Example 1.

[0050] Comparative Example 1 A polyisoprene-free styrene-acrylic ternary system aqueous membrane adhesive: The raw material ratio, based on dry weight, is as follows: 50 parts styrene, 25 parts methacrylic acid, 12 parts acrylamide; 0.6 parts initiator (ammonium persulfate), 2.5 parts emulsifier (sodium dodecyl sulfate); and ammonia water as the neutralizing agent.

[0051] The preparation process of the above-mentioned water-based membrane adhesive is the same as in Example 1. The monomer conversion rate was tested and found to be 96.5%.

[0052] Comparative Example 2 A commercially available oil-based PVDF adhesive: A commercially available battery-grade PVDF binder (Solve® 5130) was used, and an 8% solids content binder solution was prepared using NMP as a solvent for later use.

[0053] Comparative Example 3 A common commercially available water-based polyacrylate adhesive: Use commercially available water-based polyacrylate binder specifically for ceramic diaphragms (ZEON CORPORATION, Japan, brand name 900B) directly.

[0054] Comparative Example 4 The difference between this comparative example and Example 1 is that polyisoprene was replaced with an equal amount of polybutadiene (on a dry basis). The remaining raw material ratios and preparation processes are the same as in Example 1. Testing showed a monomer conversion rate of 95.8% and a polybutadiene grafting rate of 76%.

[0055] Comparative Example 5 The difference between this comparative example and Example 1 is that the polyisoprene was replaced with an equal amount of polychloroprene emulsion (on a dry basis). The remaining raw material ratios and preparation processes were the same as in Example 1. Testing showed a monomer conversion rate of 96.1% and a polychloroprene grafting rate of 79%.

[0056] Comparative Example 6 The difference between this comparative example and Example 1 is that the polyisoprene was replaced with an equal amount of commercially available membrane-grade SBR styrene-butadiene latex (on a dry basis). The remaining raw material ratios and preparation processes were the same as in Example 1. Testing showed a monomer conversion rate of 95.2% and an SBR grafting rate of 71%.

[0057] Preparation of heat-resistant ceramic-coated diaphragms: Example 5 The method for preparing a heat-resistant ceramic-coated diaphragm using the polyisoprene-modified waterborne diaphragm binder obtained in Example 1 includes the following steps: (1) Preparation of ceramic slurry: On a dry basis, 100 parts of boehmite and 1 part of sodium polyacrylate dispersant were added to deionized water and dispersed at a high speed of 1500~2000 rpm for 30 min until the powder was completely dispersed; 0.3 parts of acetylenic diol wetting agent and 8 parts of binder (pure) from Example 1 were added and dispersed for another 20 min. After filtration through a 200-mesh filter and vacuum defoaming, a uniform ceramic coating slurry was obtained. The solid content of the slurry was adjusted to 40% with deionized water.

[0058] (2) Coating and drying: The ceramic slurry is uniformly coated on one side of a PE base film with a thickness of 9μm using a micro-gravure coating method. The coating thickness on one side is 3μm. The coated wet film is then dried in three gradient ovens at 60℃, 80℃ and 100℃. The residence time in each oven is 1~3min (the actual time is adjusted according to the production line speed and coating drying status) to obtain a heat-resistant ceramic coated diaphragm.

[0059] Example 6 The method for preparing a heat-resistant ceramic-coated diaphragm using the polyisoprene-modified waterborne diaphragm binder obtained in Example 2 includes the following steps: (1) Preparation of ceramic slurry: On a dry basis, 100 parts of boehmite and 1.2 parts of sodium polyacrylate dispersant were added to deionized water and dispersed at a high speed of 1500~2000 rpm for 30 min until the powder was completely dispersed; 0.5 parts of acetylenic diol wetting agent and 10 parts of binder (pure) from Example 2 were added and dispersed for another 20 min. After filtration through a 200-mesh filter and vacuum defoaming, a uniform ceramic coating slurry was obtained. The solid content of the slurry was adjusted to 38% with deionized water.

[0060] (2) Coating and drying: The above ceramic slurry is coated on both sides of a PP base film with a thickness of 12μm using a slit coating method, and the coating thickness on one side is 2.5μm. The coated wet film is then dried in three gradient ovens at 60℃, 80℃ and 100℃. The residence time in each oven is 1~3min (the actual time is adjusted in time according to the production line speed and coating drying status) to obtain a heat-resistant ceramic coated diaphragm.

[0061] Example 7 The method for preparing a heat-resistant ceramic-coated diaphragm using the polyisoprene-modified waterborne diaphragm binder obtained in Example 3 includes the following steps: (1) Preparation of ceramic slurry: On a dry basis, 100 parts of boehmite and 0.9 parts of sodium polyacrylate dispersant were added to deionized water and dispersed at a high speed of 1500~2000 rpm for 30 min until the powder was completely dispersed; 0.2 parts of acetylenic diol wetting agent and 7 parts of binder (pure) from Example 3 were added and dispersed for another 20 min. After filtration through a 200-mesh filter and vacuum defoaming, a uniform ceramic coating slurry was obtained. The solid content of the slurry was adjusted to 42% with deionized water.

[0062] (2) Coating and drying: The ceramic slurry is coated on one side of a PE base film with a thickness of 9μm using a micro-gravure coating method. The coating thickness on one side is 3.5μm. The coated wet film is then dried in three gradient ovens at 60℃, 80℃ and 100℃. The residence time in each oven is 1~3min (the actual time is adjusted according to the production line speed and coating drying status) to obtain a heat-resistant ceramic coated diaphragm.

[0063] Example 8 The method for preparing a heat-resistant ceramic-coated diaphragm using the polyisoprene-modified waterborne diaphragm binder obtained in Example 4 includes the following steps: (1) Preparation of ceramic slurry: On a dry basis, 100 parts of boehmite and 1.5 parts of sodium polyacrylate dispersant were added to deionized water and dispersed at a high speed of 1500~2000 rpm for 30 min until the powder was completely dispersed; 0.8 parts of acetylenic diol wetting agent and 12 parts of binder (pure) from Example 4 were added and dispersed for another 20 min. After filtration through a 200-mesh filter and vacuum defoaming, a uniform ceramic coating slurry was obtained. The solid content of the slurry was adjusted to 45% with deionized water.

[0064] (2) Coating and drying: The above ceramic slurry is coated on both sides of a PP base film with a thickness of 12μm using a slit coating method, and the coating thickness on one side is 4μm. The coated wet film is then dried in three gradient ovens at 60℃, 80℃ and 100℃. The residence time in each oven is 1~3min (the actual time is adjusted according to the production line speed and coating drying status) to obtain a heat-resistant ceramic coated diaphragm.

[0065] Comparative Example 7 Using the styrene-acrylic ternary binder obtained in Comparative Example 1, a ceramic-coated diaphragm was prepared according to the same diaphragm preparation process as in Example 5.

[0066] Comparative Example 8 Using the commercially available oil-based PVDF binder from Comparative Example 2, a ceramic slurry (8 parts pure PVDF, 100 parts boehmite, and 1 part dispersant) was prepared with NMP as the solvent. The coating method was the same as in Example 5, except for the drying conditions: the coated wet film was sequentially dried in three independently controlled temperature gradient ovens at 90°C, 110°C, and 130°C, with a residence time of 2-4 minutes in each oven, resulting in the comparative ceramic-coated diaphragm.

[0067] Comparative Example 9 A ceramic-coated diaphragm was prepared using the commercially available water-based polyacrylate binder (Zeon 900B) from Comparative Example 3, following the same diaphragm preparation process as in Example 5.

[0068] Comparative Example 10 Using the polybutadiene-modified binder obtained in Comparative Example 4, a ceramic-coated diaphragm was prepared according to the same diaphragm preparation process as in Example 5.

[0069] Comparative Example 11 Using the polychloroprene modified binder obtained in Comparative Example 5, a ceramic-coated diaphragm was prepared according to the same diaphragm preparation process as in Example 5.

[0070] Comparative Example 12 Using the SBR-modified binder obtained in Comparative Example 6, a ceramic-coated diaphragm was prepared according to the same diaphragm preparation process as in Example 5.

[0071] Performance testing and results analysis: The adhesives of Examples 5-8 and Comparative Examples 7-12 were tested as follows, and the test results are shown in Table 1 below.

[0072] (1) High-temperature heat shrinkage rate test The ceramic-coated diaphragm was cut into 100mm × 100mm samples and placed in a 180℃ constant temperature oven for 1 hour. The longitudinal (MD) and transverse (TD) dimensional changes before and after the heat preservation were measured, and the thermal shrinkage rate was calculated: Thermal shrinkage rate = (Dimensions before heat preservation) × Dimensions after heat preservation ... (Dimensions after insulation) / Dimensions before insulation × 100%.

[0073] (2) Coating peel strength test Following the method in GB / T 2790—1995, the ceramic-coated diaphragm was fixed to a steel plate with the coated side facing outwards. A 20mm wide strip of 3M tape was then applied to the coated surface. A universal tensile testing machine was used to peel the diaphragm at a rate of 100mm / min along a 180° direction. The peel force was recorded, and the peel strength (N / m) was calculated. Five parallel samples were tested for each group of specimens, and the average value was taken.

[0074] (3) Electrolyte immersion test The ceramic-coated diaphragm was cut into 50mm × 50mm samples and immersed in LiPF6 / carbonate electrolyte (1 mol / L LiPF6 dissolved in EC / EMC / DEC = 1:1:1 volume ratio) for 72 hours at a constant temperature of 85℃. After removal, the surface electrolyte was blotted dry with filter paper, and the coating was visually inspected for phenomena such as powdering, swelling, or peeling.

[0075] (4) Bending test Bend the ceramic-coated diaphragm repeatedly along a 5mm diameter rod 10 times and visually inspect the coating for cracks or powdering.

[0076] Table 1:

[0077] As shown in Table 1, comparing Example 5 with Comparative Example 7, the heat shrinkage rate (MD) of Comparative Example 7 (a styrene-acrylic ternary system without a polyisoprene flexible backbone) at 180℃ reached 7.2% and 8.1%, significantly higher than the 1.8% and 1.1% of Example 5; the peel strength was only 99 N / m, lower than the 112 N / m of Example 5; and significant powdering occurred in the coating after bending. This indicates that the introduction of the polyisoprene flexible backbone, through its own double bonds participating in copolymerization to form an intermolecular cross-linking structure, significantly improves the toughness and high-temperature dimensional stability of the coating, and is the core structural unit for achieving low heat shrinkage, high adhesive strength, and bending resistance.

[0078] As can be seen from the comparison between Example 5 and Comparative Example 8 in Table 1, the water-based adhesive system of the present invention is superior to the traditional oil-based PVDF system in terms of heat shrinkage rate and peel strength at 180℃. Moreover, it does not require the use of organic solvents such as NMP, and the entire process is water-based, with low VOC emissions and low production costs, thus completely solving the environmental protection and high-temperature failure problems of oil-based systems.

[0079] As shown in Table 1, comparing Example 5 with Comparative Example 9, ordinary commercially available water-based polyacrylate adhesives have severely softened and failed at 180°C, with a heat shrinkage rate as high as 12.3% / 14.5%, and the coating powders and peels off over a large area, failing to meet the high heat resistance requirements. In contrast, this invention, through a triple crosslinking structure design of polyisoprene internal crosslinking, hard monomers to improve Tg, and amide monomer self-crosslinking, significantly improves the high-temperature rigidity and structural stability of the adhesive, achieving a leapfrog improvement in heat resistance and electrolyte resistance.

[0080] As can be seen from the comparison between Example 5 and Comparative Example 10 in Table 1, although the polybutadiene-modified system (grafting rate 76%) possesses a certain degree of flexibility, its grafting reactivity is lower than that of polyisoprene (grafting rate 88%), resulting in insufficient crosslinking density. Consequently, its 180℃ heat shrinkage rate (4.3% / 4.8%) and electrolyte resistance (slight swelling and edge powdering after immersion) are both weaker than those of the system of this invention. This indicates that the presence of methyl groups on the side of the polyisoprene molecular chain enhances its free radical grafting reactivity, enabling the formation of a denser crosslinked network.

[0081] As can be seen from the comparison between Example 5 and Comparative Example 11 in Table 1, although the heat shrinkage rate (3.9% / 4.2%) of the polychloroprene modified system (grafting rate 79%) is slightly better than that of the polybutadiene system, the material is brittle (it cracks obviously after bending), and the molecular chain contains chlorine groups, which can easily cause side reactions in the battery system, making it unsuitable for high-end power battery separator application scenarios.

[0082] As shown in Table 1, comparing Example 5 with Comparative Example 12, the traditional SBR system (grafting rate 71%) exhibits severe high-temperature thermal shrinkage (6.1% / 6.7%) and significant swelling after immersion in electrolyte at 85°C. The double bond reactivity of the butadiene segments in the SBR is lower than that of polyisoprene, resulting in a significantly reduced grafting rate and insufficient cross-linking structure, which fails to meet the performance requirements of high heat resistance and long-cycle membranes.

[0083] In summary, this invention, through a quaternary copolymer structure design using polyisoprene as the flexible grafted main chain and grafting hard monomers, carboxyl monomers, and amide monomers, fully leverages the synergistic effects of cross-linking toughening within the flexible main chain, heat-resistant support from the hard monomers, chemical bonding of carboxyl groups, and self-cross-linking stability of amide groups. This achieves a unified combination of low heat shrinkage (≤2%) at 180℃, high peel strength (≥110N / m), excellent electrolyte resistance, and good bending resistance. Furthermore, the entire process is water-based and environmentally friendly, making it suitable for the high-safety separator requirements in the fields of power batteries and energy storage batteries.

[0084] The polyisoprene-modified waterborne membrane adhesive and its heat-resistant ceramic-coated membrane provided by this invention have widely available raw materials and mature preparation processes. The entire process of adhesive synthesis and ceramic slurry preparation uses water as a medium, requires no organic solvents, and has low VOC emissions. It is compatible with existing membrane coating production lines for microgravure coating and slot coating equipment, and can achieve industrial production without modifying existing production lines, thus having significant economic and social benefits.

[0085] The binder of this invention can also be applied to other types of inorganic coated membranes (such as alumina coated membranes, silica coated membranes, etc.) and composite coated membrane systems, with a wide range of applications.

[0086] The above embodiments merely illustrate several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the inventive concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A modified waterborne membrane adhesive, characterized in that, It is copolymerized with polyisoprene as the grafted main chain, grafted with hard monomers, carboxyl monomers and amide monomers; The raw material composition of the aqueous membrane adhesive, based on dry weight, includes: 20-45 parts of polyisoprene; 25-50 parts of hard monomer; 10-25 parts of carboxyl monomer; 5-18 parts of amide monomer; The hard monomer is styrene and / or acrylonitrile; The carboxyl monomer is selected from one or more of methacrylic acid, acrylic acid, itaconic acid, and maleic anhydride; The amide monomer is selected from one or more of acrylamide, methacrylamide, N-hydroxymethylacrylamide, and N-isobutoxyacrylamide.

2. The modified waterborne membrane adhesive according to claim 1, characterized in that, The raw material composition, based on dry basis by mass, includes: 25-40 parts of polyisoprene, 28-45 parts of hard monomer, 12-20 parts of carboxyl monomer, and 8-15 parts of amide monomer.

3. The modified waterborne membrane adhesive according to claim 1, characterized in that, The raw material composition also includes 0.2-1.2 parts of initiator, 1.5-4 parts of emulsifier, neutralizer and deionized water; The initiator is selected from one of ammonium persulfate, sodium persulfate, potassium persulfate, and azobisisobutyramidine hydrochloride; The emulsifier is selected from one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and alkylphenol polyoxyethylene ether; The neutralizing agent is selected from one of ammonia, sodium hydroxide, lithium hydroxide, and triethylamine; The amount of deionized water used results in a solid content of 20% to 40% for the aqueous membrane adhesive.

4. The modified waterborne membrane adhesive according to claim 1, characterized in that, The grafting rate of the polyisoprene is 82%~95%.

5. A method for preparing a modified aqueous membrane adhesive as described in any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Preparation of base emulsion: The first part of deionized water and the first part of emulsifier are put into the reaction vessel, and polyisoprene emulsion is added and stirred to form base emulsion; (2) Preparation of pre-emulsion: The remaining deionized water, the remaining emulsifier, hard monomer, carboxyl monomer, and amide monomer are mixed evenly by stirring to obtain the pre-emulsion; (3) Graft polymerization reaction: Nitrogen gas is introduced into the reactor to remove oxygen, and the temperature is raised to 65~85℃; the initiator and the pre-emulsion are added dropwise to the reactor simultaneously, and the reaction is maintained at the temperature after the addition is completed; (4) Neutralization and post-treatment: After the reaction is completed, the temperature is lowered, a neutralizing agent is added to adjust the pH of the system to 7.0~9.0, the material is filtered out, and the polyisoprene modified waterborne membrane adhesive is obtained.

6. The preparation method according to claim 5, characterized in that, In step (1), the amount of the first part of deionized water is 60% to 75% of the total water volume, and the amount of the first part of emulsifier is 70% of the total emulsifier volume; the stirring speed is 250 to 350 rpm. In step (2), the stirring time is 30~45 min; In step (3), the initiator is prepared as a 5wt% aqueous solution and added dropwise over a period of 2.5 to 4 hours, and the reaction is kept at a constant temperature for 2 to 5 hours.

7. A heat-resistant ceramic-coated diaphragm, characterized in that, Includes a polyolefin-based film and a ceramic coating applied to at least one side of the base film; The ceramic coating is formed by coating and drying a ceramic slurry, wherein the solid components of the ceramic slurry include: 100 portions of Boehmite; 6-12 parts of the modified aqueous membrane adhesive as described in any one of claims 1 to 4; Dispersant 0.8~1.5 parts; Wetting agent 0.2~0.8 parts; The ceramic slurry also contains deionized water, and the amount of deionized water used makes the solid content of the ceramic slurry 35%~45%. The diaphragm exhibits longitudinal and transverse thermal shrinkage rates of ≤2% after being kept at 180℃ for 1 hour, and a peel strength of ≥110N / m.

8. The heat-resistant ceramic-coated diaphragm according to claim 7, characterized in that, The boehmite has a D50 of 0.5~1.5μm; the ceramic slurry has a solid content of 35%~45%; the polyolefin-based film has a thickness of 9~12μm; and the single-sided ceramic coating has a thickness of 2~4μm.

9. A method for preparing a heat-resistant ceramic-coated diaphragm as described in claim 7 or 8, characterized in that, Includes the following steps: (1) Preparation of ceramic slurry: Boehmite and dispersant are added to deionized water for dispersion, wetting agent and the aqueous membrane binder are added, dispersion is continued, and after filtration and defoaming, ceramic coating slurry is obtained; (2) Coating and drying: The ceramic coating slurry is coated on one or both sides of the polyolefin base membrane and dried by segmented gradient heating to obtain the heat-resistant ceramic coated diaphragm.

10. The preparation method according to claim 9, characterized in that, In step (1), the dispersion speed is 1500~2000 rpm and the dispersion time is 30 min; in step (2), the coating method is microgravure coating or slot coating; the segmented gradient heating and drying is carried out at 60℃, 80℃ and 100℃ respectively.