A pickling additive, a pickling agent containing the additive, and its application.
By using acid pickling additives containing surfactants, complexing agents, and chelating agents in the TOPCon process, the acid pickling tank process was optimized, solving the problem of difficult dehydration of the wet oxide layer on the silicon wafer surface, and achieving effective dehydration and cost optimization of the silicon wafer.
Patent Information
- Application Number
- CN202611005076.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-07
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing TOPCon process back polishing, the wet oxide layer on the silicon wafer surface is difficult to dehydrate, leading to wafer sticking and liquid carryover. Furthermore, existing improvement measures, such as adding HF, may affect the passivation effect of the tunneling layer and poly layer or increase costs.
By using pickling additives containing surfactants, complexing agents, and chelating agents, the pickling process is optimized, partially replacing HCl, and combined with simplified water washing and slow lifting steps, effective dehydration of silicon wafers is achieved.
It effectively solves the problems of silicon wafer adhesion and liquid carryover, while maintaining the passivation effect of the tunneling layer and the poly layer, thus reducing production costs.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solar cell technology, and specifically relates to an acid pickling additive, an acid pickling agent containing the additive, and its application. Background Technology
[0002] The existing TOPCon process's back polishing step is prone to chip adhesion and liquid carryover issues. The current back polishing process mainly consists of ① pre-cleaning - ② water washing - ③ alkaline polishing - ④ water washing - ⑤ post-cleaning - ⑥ water washing - ⑦ acid washing - ⑧ water washing - ⑨ slow lifting - ⑩ drying. Among these, the acid washing tank in step ⑦ contains only HCl and water, and the silicon wafer surface has a wet oxide layer that is not easy to dehydrate. This results in a certain proportion of chip adhesion and liquid carryover still existing after the slow lifting and drying tank treatments, requiring manual extraction and rework.
[0003] Currently, some companies retain a certain concentration of HF in the pickling tank to improve its dehydration, but this also removes the wet oxide layer, leading to a decrease in the passivation effect of the subsequent tunneling layer and poly layer, which in turn reduces the battery efficiency. Other manufacturers add additives to the slow lifting tank to improve dehydration, but the new additives will bring about an increase in cost. Summary of the Invention
[0004] In view of the above-mentioned problems existing in the prior art, the present invention proposes a pickling additive, a pickling agent containing the additive, and its application.
[0005] Specifically, one aspect of the present invention provides a pickling additive, the pickling additive comprising a surfactant, a complexing agent, and a chelating agent.
[0006] In one or more embodiments, the pickling additive has a chelating agent to complexing agent mass ratio of (7-75):100.
[0007] In one or more embodiments, the pickling additive has a mass ratio of chelating agent to surfactant of (12-150):100.
[0008] In one or more embodiments, the surfactant is an alkyl glycoside.
[0009] In one or more embodiments, the degree of polymerization of the alkyl glycoside is 1.1-3.
[0010] In one or more embodiments, the complexing agent is a crown ether.
[0011] In one or more embodiments, the crown ether is selected from one or more of 15-crown ether-5, 12-crown ether-4, 18-crown ether-6, 21-crown ether-7, and 24-crown ether-8.
[0012] In one or more embodiments, the crown ether is 15-crown ether-5.
[0013] In one or more embodiments, the chelating agent comprises a carboxyl group and a hydroxyl group.
[0014] In one or more embodiments, the chelating agent is selected from one or more of glutamic acid diacetic acid, methylglycine diacetic acid, iminodisuccinic acid, ethylenediaminedisuccinic acid, citric acid, and gluconic acid.
[0015] In one or more embodiments, the chelating agent is citric acid.
[0016] Another aspect of the present invention provides a pickling agent comprising the pickling additives described in any embodiment of the present invention and water.
[0017] In one or more embodiments, the pickling agent contains a pickling additive with a mass fraction of 0.7%-2.4%.
[0018] In one or more embodiments, the pickling agent contains a surfactant with a mass fraction of 0.2%-0.8%, a complexing agent with a mass fraction of 0.4%-1.3%, and a chelating agent with a mass fraction of 0.1%-0.3%.
[0019] Another aspect of the present invention provides a pickling method for preparing silicon wafers, the pickling method comprising pickling the silicon wafers using the pickling agent described in any embodiment of the present invention.
[0020] Another aspect of the present invention provides a back polishing method for preparing silicon wafers, characterized in that the back polishing method includes the acid washing method described in any embodiment of the present invention.
[0021] In one or more embodiments, the back polishing method includes a wet processing flow, which sequentially includes pre-cleaning, water washing, alkaline polishing, water washing, post-cleaning, water washing, acid washing, and drying.
[0022] In one or more embodiments, the silicon wafer is a TOPCon battery silicon wafer.
[0023] In one or more embodiments, the silicon wafer is a monocrystalline silicon wafer.
[0024] Another aspect of the present invention provides a silicon wafer prepared by the acid pickling method or the back polishing method described in any embodiment of the present invention.
[0025] Another aspect of the present invention provides a solar cell comprising a silicon wafer as described in any embodiment of the present invention or a silicon wafer prepared by an acid washing method or a back polishing method as described in any embodiment of the present invention.
[0026] This invention optimizes and reduces costs in existing tank processes. By adding pickling agent to the pickling tank, it can replace part of the HCl used and achieve dehydration. In addition, it can directly eliminate the two tanks in the existing process (⑧ water washing and ⑨ slow lifting). The process is simple and can be directly optimized and reduced in mass production, solving the problem of liquid residue on the surface mount. Attached Figure Description
[0027] Figure 1 This is a comparison diagram of the process flow before and after optimization of the back-throwing trough machine of the present invention. Detailed Implementation
[0028] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used herein are explained and defined in general terms below. Unless otherwise specified, all technical and scientific terms used herein have the common meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.
[0029] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.
[0030] In this document, the terms “contains,” “includes,” “containing,” and similar terms encompass the meanings of “basically composed of” and “composed of.” For example, when this document discloses “A contains B and C,” “A is basically composed of B and C” and “A is composed of B and C” should be considered as having been disclosed in this document.
[0031] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values (including integers and fractions) within those ranges.
[0032] Unless otherwise specified, percentages refer to mass percentages and proportions refer to mass ratios in this article.
[0033] In this article, the sum of the percentages of all components in the composition is 100%.
[0034] In this document, when describing embodiments or examples, it should be understood that it is not intended to limit the invention to those embodiments or examples. Rather, all alternatives, modifications, and equivalents of the methods and materials described herein are covered within the scope of this invention.
[0035] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.
[0036] Pickling additives
[0037] The pickling additives of the present invention include surfactants, complexing agents, and chelating agents.
[0038] In the pickling additive of the present invention, the mass ratio of chelating agent to complexing agent is (7-75):100, for example 7:100, 8:100, 9:100, 10:100, 15:100, 20:100, 25:100, 30:100, 35:100, 40:100, 45:100, 50:100, 55:100, 60:100, 65:100, 70:100, 75:100, or any range between two values.
[0039] In the pickling additive of the present invention, the mass ratio of chelating agent to surfactant is (12-150):100, for example 12:100, 13:100, 14:100, 15:100, 20:100, 25:100, 30:100, 35:100, 40:100, 45:100, 50:100, 55:100, 60:100, 65:100, 70:1 00, 75:100, 80:100, 85:100, 90:100, 95:100, 100:100, 105:100, 110:100, 115:100, 120:100, 125:100, 130:100, 135:100, 140:100, 145:100, 150:100, or any range between two values.
[0040] In this invention, the surfactant is preferably an alkyl glycoside. Alkyl glycosides are nonionic surfactants synthesized from glucose (or starch hydrolysis products) and fatty alcohols via an acetalization reaction under an acidic catalyst, with the general formula RO(G). n Where: R represents C8-C 18The saturated or unsaturated alkyl chain (lipophilic group) is typically derived from natural oils such as coconut oil and palm kernel oil. G represents a glucose unit (hydrophilic group), derived from renewable resources such as corn starch and wheat. n represents the degree of polymerization, indicating the number of glucose units attached to the alkyl chain. The degree of polymerization (n) of the alkyl glycosides suitable for this invention can be 1.1-3, preferably 1.4-1.6, for example. It should be understood that the alkyl glycosides suitable for this invention can be various commercially available alkyl glycosides.
[0041] In this invention, the complexing agent is preferably a crown ether. Crown ethers are a class of organic compounds with a macrocyclic polyether structure, whose molecular skeleton uses oxygen atoms as heteroatoms and methylene (-CH2-) as bridging units, forming a ring-shaped cavity structure resembling a "crown". The crown ethers used in this invention include, but are not limited to, one or more selected from 15-crown ether-5, 12-crown ether-4, 18-crown ether-6, 21-crown ether-7, and 24-crown ether-8. In some preferred embodiments, the complexing agent is 15-crown ether-5.
[0042] The chelating agent of the present invention comprises a carboxyl group and a hydroxyl group. Chelating agents suitable for the present invention include, but are not limited to, one or more selected from GLDA (glutamic acid diacetic acid), MGDA (methylglycine diacetic acid), IDS (iminodisuccinic acid), EDDS (ethylenediaminedisuccinic acid), citric acid, and gluconic acid, preferably citric acid.
[0043] Pickling agent
[0044] The pickling agent of the present invention includes the pickling additives and water described in any of the embodiments herein.
[0045] In the pickling agent described in this article, the mass fraction of the pickling additive is 0.7%-2.4%, for example, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, or any range between two values.
[0046] In the pickling agent described in this article, the mass fraction of the surfactant is 0.2%-0.8%, for example, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, or any range between two values.
[0047] In the pickling agent described in this article, the mass fraction of the complexing agent is 0.4%-1.3%, for example, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.1%, 1.2%, 1.3%, or any range between two values.
[0048] In the pickling agent described in this article, the mass fraction of the chelating agent is 0.1%-0.3%, for example, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, or any range between two values.
[0049] In this invention, complexing agents and chelating agents can remove metal ions. The hydroxyl and carboxyl groups on the molecular chain of the chelating agent (e.g., citric acid) can form stable complexes with metal ions. The complexing agent (crown ether) can chelate metal cations within the ring and form stable complexes with various metal salts, ammonium salts, organic cationic compounds, etc. In water, these hydrophilic functional groups can form hydrogen bonds with water molecules, allowing the polymer molecular chains to fully extend in water, thereby achieving good dissolution.
[0050] In this invention, the surfactant has excellent dehydrating properties. When the pickling additive is used in the pickling process of back polishing, the content of its reaction products is extremely low and it is soluble in water. Under the action of the surfactant, the pickling additive and its reaction products can be separated from the silicon wafer, making the silicon wafer surface clean. At the same time, the silicon wafers prepared by it are not easy to adhere to the wafer in the basket, reducing the proportion of wafer sticking and liquid.
[0051] application
[0052] The present invention provides a pickling method for preparing silicon wafers, which includes pickling the silicon wafers using the pickling agent described in any embodiment herein.
[0053] The present invention also provides a back polishing method for preparing silicon wafers, which includes the acid washing method described in any embodiment herein.
[0054] In this invention, the back polishing method includes a wet processing flow, specifically, the wet processing flow includes pre-cleaning, water washing, alkaline polishing, water washing, post-cleaning, water washing, acid washing and drying in sequence.
[0055] In the wet processing flow of this invention, the water wash after pre-cleaning is to remove the residue of the pre-cleaning solution in the previous step.
[0056] In the wet processing flow of this invention, the water washing after alkaline polishing is to remove the residue of the alkaline polishing solution in the previous step.
[0057] In the wet processing flow of this invention, the water wash after the post-wash is to remove the residue of the post-wash solution in the previous step.
[0058] The preferred amount of pickling agent used in the application process is generally 0.1% to 0.4% of the liquid volume of the tank, for example, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, or any range between two values. Controlling the amount of pickling agent used within the above range helps to maintain a low usage amount and avoid pickling additive residues.
[0059] In some implementations, the silicon wafer is a TOPCon battery silicon wafer; in other implementations, the silicon wafer is a monocrystalline silicon wafer.
[0060] The present invention also provides silicon wafers prepared using the acid pickling method described in any of the embodiments herein.
[0061] The present invention also provides silicon wafers prepared using the back polishing method described in any embodiment herein.
[0062] The present invention also provides a solar cell comprising a silicon wafer as described in any embodiment herein or prepared by an acid washing method or back polishing method as described in any embodiment herein.
[0063] The present invention will be described below by way of specific embodiments. It should be understood that these embodiments are merely illustrative and are not intended to limit the scope of the invention. The methods, reagents, and materials used in the embodiments and comparative examples are conventional methods, reagents, and materials in the art, unless otherwise stated. The starting material compounds in the embodiments and comparative examples are all commercially available.
[0064] Example 1
[0065] This embodiment provides a method for disposing of TOPCon batteries (e.g., ...). Figure 1 (As shown in the right figure), the specific steps include: (1) Pretreatment: After the Zhonghuan silicon wafer is oxidized on both sides, it is first passed through the BSG (borosilicate glass) chain machine to remove the oxide layer on the back and sides of the silicon wafer; (2) Tank etching: The silicon wafer that has been pretreated in step (1) enters the tank etching machine, and the PN junction on the back of the silicon wafer is removed by wet etching and the back of the silicon wafer is polished. (3) Wet treatment process: ① Pre-cleaning: The silicon wafer obtained in step (2) is put into the pre-cleaning tank for pre-cleaning. The pre-cleaning solution in the pre-cleaning tank includes a sodium hydroxide solution with a volume fraction of 0.4% (sodium hydroxide mass concentration of 45%) and a hydrogen peroxide solution with a volume fraction of 1% (hydrogen peroxide solution mass concentration of 31%) (the volume ratio of alkaline solution to hydrogen peroxide is 2:5, and the remaining components are deionized water). The temperature is 65℃ and the pre-cleaning time is 90s. ② Water washing: The silicon wafer after ① pre-cleaning is put into the water tank for water washing. ③ Alkaline polishing: After being washed with water in step ②, the silicon wafers are placed in an alkaline polishing tank to react with the polishing solution. The front side of the silicon wafer is protected by an oxide layer and does not participate in the reaction. The PN junction on the back side is removed through the reaction, and the back side is polished to a surface morphology with a reflectivity of about 41~43%. The polishing solution includes a 0.5% sodium hydroxide solution (sodium hydroxide mass concentration of 45%) and a 0.1% polishing additive (Topband's BP21V62) by volume. The remaining components are deionized water. The temperature is 35-50℃ and the alkaline polishing time is 120s. ④ Water washing: After being alkaline polished in step ③, the silicon wafers are placed in a water tank for water washing. ⑤ Post-cleaning: The cleaning solution includes a 0.8% sodium hydroxide solution (sodium hydroxide mass concentration is 45%) and a 3% hydrogen peroxide solution (hydrogen peroxide mass concentration is 31%), with the remaining components being deionized water. The temperature is 65℃ and the pre-cleaning time is 90s. ⑥ Water washing: The silicon wafers after post-cleaning in step ⑤ are placed in a water bath for water washing. ⑦ Pickling: The silicon wafers washed with water in step ⑥ enter the pickling tank and are pickled with pickling agent. The pickling agent includes pickling additives and water. The pickling additives include 1-oxododecyl-α-D-glucoside (C12APG alkyl glycoside), 15-crown ether-5 and citric acid. In the pickling agent, the mass fraction of alkyl glycoside is 0.4%, the mass fraction of 15-crown ether-5 is 0.6%, and the mass fraction of citric acid is 0.2%. The pickling time is 110 seconds at room temperature. ⑩ Drying: The silicon wafers after acid washing (⑦) are placed in a drying tank and dried at high temperature to remove surface moisture, and then set aside for use.
[0066] Example 2
[0067] This embodiment uses a back polishing method similar to that of Example 1, but the difference is that in the pickling process, the mass fraction of alkyl glycoside in the pickling agent is 0.2%, the mass fraction of 15-crown ether-5 is 0.4%, and the mass fraction of citric acid is 0.3%.
[0068] Example 3
[0069] This embodiment uses a back polishing method similar to that of Example 1, but the difference is that in the pickling process, the mass fraction of alkyl glycoside in the pickling agent is 0.5%, the mass fraction of 15-crown ether-5 is 0.7%, and the mass fraction of citric acid is 0.1%.
[0070] Comparative Example 1
[0071] This embodiment uses a back polishing method similar to that of Example 1, but the difference is that in the wet processing flow, ⑦ pickling: the pickling agent is hydrochloric acid with equal mass fractions (the sum of the mass fractions of alkyl glycoside, 15-crown ether-5, and citric acid); ⑦ The process after pickling is as follows: ⑧ Water washing: The silicon wafers after acid washing (⑦) are placed in a water bath for water washing; ⑨ Slow pulling: The silicon wafer, after being washed by water in step ⑧, is placed in the slow pulling tank at 45°C and pulled for 30 seconds; ⑩ Drying: After being slowly pulled up by ⑨, the silicon wafers are placed in a drying tank and dried at high temperature to remove surface moisture, and then set aside for use.
[0072] Comparative Example 2
[0073] This embodiment uses a back polishing method similar to that of Example 1, but the difference is that in the pickling process, the alkyl glycoside has a mass fraction of 2%, the 15-crown ether-5 has a mass fraction of 5%, and the citric acid has a mass fraction of 3%.
[0074] Test case
[0075] The metal ions on the silicon wafer surface in each embodiment and comparative example were obtained by ICP-MS testing using the following steps: 1. Place the silicon wafer in a VPD chamber and expose it to HF vapor to dissolve the natural oxide or thermally oxidized SiO2 surface layer; 2. Place the extraction droplet (usually 250 μL of 2% HF / 2% H2O2) on the wafer, and then tilt it in a carefully controlled manner so that the droplet “sweeps” across the wafer surface; 3. As the extraction droplet moves across the wafer surface, it collects dissolved SiO2 and all contaminant metals; 4. Transfer the extracted droplets from the wafer surface to an ICP-MS or ICP-MS / MS system for analysis. The test results are shown in Table 1.
[0076] Table 1
[0077] Application examples
[0078] The silicon wafers used in each embodiment and comparative example were fabricated into TOPCon cells using the same process and tested under standard test conditions (STC), namely a temperature of 25°C and a light intensity of 1000 W / m². 2The spectrum was AM 1.5G. The photoelectric conversion efficiency (Eta), short-circuit current (Isc), open-circuit voltage (Uoc), fill factor (FF), series resistance (Rs), parallel resistance (Rsh), and reverse saturation current (IRev2) were output using a Maiwei tester. The test results are shown in Table 2.
[0079] Table 2
Claims
1. A pickling additive, characterized in that, The pickling additives include surfactants, complexing agents, and chelating agents.
2. The pickling additive as described in claim 1, characterized in that, In the pickling additive, the mass ratio of chelating agent to complexing agent is (7-75):100; In the pickling additive, the mass ratio of chelating agent to surfactant is (12-150):
100.
3. The pickling additive as described in claim 1, characterized in that, The surfactant is an alkyl glycoside.
4. The pickling additive as described in claim 3, characterized in that, The degree of polymerization of the alkyl glycoside is 1.1-3.
5. The pickling additive as described in claim 1, characterized in that, The complexing agent is a crown ether.
6. The pickling additive as described in claim 5, characterized in that, The crown ether is selected from one or more of 15-crown ether-5, 12-crown ether-4, 18-crown ether-6, 21-crown ether-7 and 24-crown ether-8, preferably 15-crown ether-5.
7. The pickling additive as described in claim 1, characterized in that, The chelating agent contains a carboxyl group and a hydroxyl group. Preferably, the chelating agent is selected from one or more of glutamic acid diacetic acid, methylglycine diacetic acid, iminodisuccinic acid, ethylenediaminedisuccinic acid, citric acid and gluconic acid. More preferably, the chelating agent is citric acid.
8. A pickling agent, characterized in that, The pickling agent comprises the pickling additive according to any one of claims 1-7 and water.
9. The pickling agent as described in claim 8, characterized in that, The pickling agent contains pickling additives at a mass fraction of 0.7%-2.4%.
10. The pickling agent as described in claim 8, characterized in that, In the pickling agent, the surfactant has a mass fraction of 0.2%-0.8%, the complexing agent has a mass fraction of 0.4%-1.3%, and the chelating agent has a mass fraction of 0.1%-0.3%.
11. A pickling method for preparing silicon wafers, characterized in that, The pickling method includes pickling the silicon wafer using the pickling agent according to any one of claims 8-10.
12. A back polishing method for preparing silicon wafers, characterized in that, The back polishing method includes the acid washing method as described in claim 11.
13. The back-projection method as described in claim 11, characterized in that, The back polishing method includes a wet processing flow, which sequentially includes pre-cleaning, water washing, alkaline polishing, water washing, post-cleaning, water washing, acid washing, and drying.
14. The pickling method as described in claim 11 or the back polishing method as described in claim 12 or 13, characterized in that, The silicon wafer is a TOPCon battery silicon wafer, and / or the silicon wafer is a monocrystalline silicon wafer.
15. A silicon wafer, characterized in that, The silicon wafer is prepared using the acid pickling method described in claim 11 or the back polishing method described in claim 12 or 13.
16. A solar cell, characterized in that, The solar cell comprises the silicon wafer of claim 15 or a silicon wafer prepared by the acid washing method of claim 11 or the back polishing method of claim 12 or 13.