A method and system for staged cryogenic treatment of a low-temperature austenitic ductile iron cylinder
By employing segmented cryogenic treatment and controlled reheating, the problem of residual austenite stability in low-temperature austenitic ductile iron cylinders under extreme low-temperature environments was solved, thereby improving the dimensional stability and mechanical properties of the cylinders and meeting the requirements for long-term reliable operation of BOG compressors.
Patent Information
- Application Number
- CN202512007661.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot effectively solve the problem of the stability and dimensional changes of residual austenite in low-temperature austenitic ductile iron cylinders under extreme low-temperature environments, leading to seal failure, wear and cracking, and failing to meet the long-term reliable service requirements of BOG compressors.
A segmented cryogenic treatment method is adopted, including pretreatment, segmented cryogenic treatment, controlled reheating and two low-temperature tempering, combined with intelligent control and safety protection. Through precise control of multi-stage cooling and heating rates, the residual austenite content is reduced and the material stability is improved.
It achieves a 150% improvement in the dimensional stability of the cylinder under extreme conditions of -162℃, reduces the residual austenite content to 4.2%, and improves the low-temperature tensile strength and fatigue strength, meeting the long-term reliable service requirements of BOG compressors.
Smart Images

Figure CN123108248A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cryogenic BOG compressor technology, specifically to a segmented cryogenic treatment method and system for a cryogenic austenitic ductile iron cylinder. Background Technology
[0002] Cryogenic BOG (flash vapor) compressors are core equipment in LNG (liquefied natural gas) receiving terminals and liquefaction plants' BOG recondensation and recovery systems, requiring long-term stable operation in extreme low-temperature environments ranging from -162℃ to -90℃. The cylinder, as a core component directly bearing pressure and in contact with the cryogenic medium, is generally made of cryogenic austenitic ductile iron with excellent low-temperature toughness. However, after casting and initial heat treatment, a certain amount of austenite remains in the matrix of this material. Under long-term extreme low-temperature service conditions, the retained austenite undergoes a metastable phase transformation to martensite, accompanied by volume expansion. This leads to irreversible changes in critical cylinder dimensions, a sharp increase in internal stress, and consequently, seal failure, abnormal wear, and even cracking, seriously threatening the compressor's operational safety and lifespan. Cryogenic treatment is an effective means to promote the transformation of retained austenite to martensite and improve the material's low-temperature stability.
[0003] In existing technologies, such as patent document CN112251579B, a method for reducing retained austenite in pearlitic gray cast iron during quenching is disclosed. This method optimizes the pre-quenching microstructure of pearlitic gray cast iron through a specific heating regime of "medium-temperature holding + low-speed heating," thereby controlling retained austenite to a low level after conventional quenching. The improvement of this technology lies in providing a quenching method that reduces retained austenite by optimizing the heating path without relying on cryogenic treatment. However, it targets pearlitic gray cast iron, which differs fundamentally from austenitic ductile iron in terms of matrix structure, graphite morphology, and alloy system, and its process principle is not directly applicable to the latter. More importantly, this existing technology does not involve cryogenic treatment at all, and cannot solve the problem of re-stabilizing or undergoing phase transformation of retained austenite in subsequent extreme low-temperature operating environments.
[0004] Patent document CN119776622A discloses a cold water treatment process and apparatus for reducing residual austenite in bearing steel balls, which employs a two-step cooling method of "oil quenching + cold water (≤10℃)". The improvement of this technology lies in the continuous combination of quenching media (oil and water) and the integrated device design, allowing for immediate low-temperature treatment after quenching to further promote austenite transformation. However, the low-temperature treatment temperature of this process is only around 0℃ to -10℃, falling under the category of "cold treatment" rather than cryogenic treatment, and therefore cannot achieve sufficient transformation of residual austenite under cryogenic conditions.
[0005] Patent document CN117683981A discloses a cryogenic treatment process based on martensitic transformation theory, targeting ferrous materials (such as GCr15 steel). Its core improvement lies in revealing the laws of continuous cooling transformation and isothermal transformation during the cryogenic process, and accordingly proposing an innovative process route of "segmented cooling (fast-slow-fast) to ultra-low temperature, followed by heating to a specific intermediate temperature (-70°C to -90°C) for long-term holding", aiming to improve the cryogenic treatment efficiency. However, it focuses on general process principles and laboratory-scale parameter research, does not involve industrial control means and safety protection measures supporting the process, nor provides a specific process chain coordinated with preceding and subsequent heat treatments (such as tempering).
[0006] Patent document CN119710164A discloses a cyclic heat treatment process of "two cryogenic treatments + two low-temperature tempering" for carburized parts (12CrNi3A steel). The improvement of this technology is that through two "cryogenic treatment-tempering" cycles, the content of retained austenite in the carburized layer is significantly reduced, solving the industry difficult problem that high surface hardness and extremely low retained austenite are difficult to achieve at the same time. This proves the effectiveness of multiple cyclic treatments in specific material systems. However, the basis of this process is carburizing treatment, and its core mechanism is to precipitate carbides in the carburized layer through high-temperature tempering, so as to reduce the content of carbon and alloying elements in austenite during subsequent quenching. Contents of the Invention
[0007] The purpose of the present invention is to provide a segmented cryogenic treatment method and system for a low-temperature austenitic ductile iron cylinder, so as to solve the key technical problems in the prior art that the cylinder has high retained austenite content after cryogenic treatment, poor low-temperature dimensional stability, and insufficient improvement of mechanical properties, which cannot meet the long-term reliable service requirements under extreme low-temperature working conditions.
[0008] A first object of the present invention is to provide a segmented cryogenic treatment method for a low-temperature austenitic ductile iron cylinder, comprising the following steps: S1. Pretreatment: subjecting the cast low-temperature austenitic ductile iron cylinder to preceding quenching treatment and pre-low-temperature tempering treatment; S2. First segmented cryogenic treatment: placing the cylinder treated in step S1 in a sealed cold box, introducing vaporized liquid nitrogen into the cold box as a cooling medium, and performing the first segmented cryogenic treatment according to a preset multi-stage cooling curve; The multi-stage cooling curve at least includes a first stage of cooling from room temperature to a first target temperature, a second stage of cooling from the first target temperature to a second target temperature, and a third stage of cooling from the second target temperature to a third target temperature, and the cooling rate of each stage is independently controlled; S3. First Controllable Reheating and Low-Temperature Tempering: After completing the cryogenic treatment in step S2, the liquid nitrogen supply is turned off, and the electric heater installed in the cold box is started to heat the cylinder to room temperature in the cold box according to the preset heating rate, thus completing the controllable reheating; then the cylinder is removed from the cold box and the first low-temperature tempering treatment is performed. S4. Second stage deep cryogenic treatment: The cylinder after step S3 is placed back into the cold box, and the stage deep cryogenic treatment process of step S2 is repeated. S5. Second controlled reheating and low-temperature tempering: Repeat the controlled reheating process of step S3, followed by a second low-temperature tempering treatment.
[0009] A further technical solution is that, in steps S2 and S4, the multi-stage cooling curve is specifically as follows: First stage: Cool from room temperature to -80℃, with the cooling rate controlled at 3-5℃ / min, and keep warm for 1-2 hours after reaching -80℃; The second stage: cooling from -80℃ to -150℃ at a rate of 2-3℃ / min, and holding at -150℃ for 1.5-2.5 hours. The third stage: cooling from -150℃ to -196℃ at a rate of 1-2℃ / min, and holding at -196℃ for 2-4 hours.
[0010] A further technical solution is that, in steps S3 and S5, the controllable reheating specifically includes: First stage: Raise the temperature from the final cryogenic temperature to -100℃, with the heating rate controlled at 1-2℃ / min; Second stage: Raise the temperature from -100℃ to room temperature, with the heating rate controlled at 2-3℃ / min.
[0011] A further technical solution is that, in step S1, the parameters of the pre-quenching treatment are: heating temperature 930-950℃, holding time 2.5-3h, and cooling to room temperature by oil cooling. The parameters for the pre-low temperature tempering treatment are: heating temperature 220-240℃, holding time 3-3.5h, and air cooling to room temperature.
[0012] A further technical solution is that, in step S3, the parameters for the first low-temperature tempering treatment are: heating temperature 230-250℃, holding time 3.5-4h, and cooling to room temperature by air cooling. In step S5, the parameters for the second low-temperature tempering treatment are: heating temperature 210-230℃, holding time 3-3.5h, and cooling to room temperature using a stepped cooling method.
[0013] A further technical solution is that, during the cryogenic treatment in steps S2 and S4, a temperature transmitter installed on the cold box monitors the temperature inside the box in real time and transmits the temperature signal to the electrical control cabinet; the PID adjustment module built into the electrical control cabinet outputs a control signal to the diaphragm regulating valve connected to the liquid nitrogen pipeline according to the deviation between the preset cooling curve and the measured temperature, so as to dynamically adjust the liquid nitrogen flow rate and realize closed-loop precise control of the cooling rate.
[0014] A further technical solution is that, during the controllable reheating process in steps S3 and S5, the power of the electric heater inside the cold box is adjusted by the electrical control cabinet to achieve closed-loop precise control of the heating rate.
[0015] A further technical solution is that the internal volume of the cold box is 1.3 to 1.5 times the volume of the cylinder, and at least two sets of electric heaters are evenly arranged on the inner wall of the cold box.
[0016] A further technical solution is to install a safety system in the area where cryogenic treatment is carried out. The safety system includes at least: an oxygen concentration monitor for monitoring the ambient oxygen concentration, a forced ventilation system, an emergency exhaust system, and an audible and visual alarm device; when the oxygen concentration is lower than a preset threshold, an alarm is triggered and the emergency exhaust system is automatically activated.
[0017] Another object of the present invention is to provide a system for a segmented deep cryogenic treatment method for a low-temperature austenitic ductile iron cylinder, comprising: Liquid nitrogen supply unit, including liquid nitrogen storage tank and connecting pipelines; The processing unit includes at least one sealed cold box for housing the cylinder; the cold box is equipped with an electric heater and a temperature sensor; The control unit includes an electrical control cabinet electrically connected to the temperature sensor, the diaphragm regulating valve on the liquid nitrogen supply line, and the electric heater; the electrical control cabinet is configured to execute control logic as described above. The safety unit includes an oxygen concentration monitor and a ventilation device; both the oxygen concentration monitor and the ventilation device are communicatively connected to the control unit.
[0018] Compared with the prior art, the beneficial effects of the present invention are: This invention addresses the shortcomings of existing technologies that focus solely on cryogenic theory while neglecting reheat control and suffer from fragmented process chains by constructing a complete process chain of "intelligent segmented cryogenic treatment—controllable reheating within the cold box—dual synergistic tempering." Compared to traditional room temperature reheating methods, the "controllable reheating" of this invention improves the stability of key cylinder dimensions by 150% (deviation ≤0.02mm). Through the synergistic effect of two cycles of cryogenic treatment and tempering, the residual austenite content is reduced to 4.2%, while simultaneously increasing the low-temperature tensile strength to 820MPa and the fatigue strength to 410MPa. Ultimately, it achieves synergistic enhancement of dimensional stability and mechanical properties of low-temperature austenitic ductile iron cylinders under extreme conditions of -162℃, meeting the stringent requirements for long-term reliable service of BOG compressors. Attached Figure Description
[0019] To make the objectives, technical solutions, and beneficial effects of this invention clearer, the following figures are provided for illustration: Figure 1 This is a diagram showing the temperature and time variation in a process, which is a comparative example of the present invention.
[0020] Figure 2 This is a graph showing the temperature and time variation during the process in Comparative Example 2 of this invention.
[0021] Figure 3 This is a graph showing the temperature and time variation of process three in the comparative example of this invention.
[0022] Figure 4 This is a graph showing the temperature variation over time in an embodiment of the present invention.
[0023] Figure 5 This is a microscopic component diagram of the process used in Comparative Example 1 of the present invention.
[0024] Figure 6 This is a microscopic component diagram of the process used in Comparative Example 2 of the present invention.
[0025] Figure 7 This is a microscopic component diagram of the comparative example three after process treatment according to the present invention.
[0026] Figure 8 This is a microscopic component diagram after the process of an embodiment of the present invention. Detailed Implementation
[0027] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0028] Example: like Figures 1-8As shown, this invention provides a segmented cryogenic treatment method and system for a low-temperature austenitic ductile iron cylinder, comprising the following steps: Step 1: Preprocessing stage After visually and dimensionally inspecting the cylinder to be processed and confirming that there are no surface defects, proceed with the preliminary heat treatment: 1. Quenching treatment: Place the cylinder in a bogie-type heating furnace and heat it to 940°C at a rate of approximately 15°C / min. Hold it at this temperature for 2.8 hours to fully austenitize the microstructure. Subsequently, quickly remove the workpiece and immerse it in a quenching oil bath to cool to room temperature, with the cooling rate controlled at 15-20°C / min.
[0029] 2. Pre-low temperature tempering treatment: The quenched cylinder is put back into the furnace and heated to 230°C at a rate of about 9°C / min, and held for 3.2 hours to eliminate some of the quenching stress and stabilize the microstructure. After the holding period, it is removed from the furnace and cooled to room temperature in air.
[0030] Step Two: Cryogenic Treatment System Setup and Debugging 1. Loading the workpiece into the furnace: The pre-treated cylinder is hoisted into a dedicated cryogenic treatment cold box. This cold box is made of 316L stainless steel, with an external polyurethane foam insulation layer. Its internal effective volume is designed to be 1.5 m³ (1.3 times the cylinder volume), providing space for liquid nitrogen vaporization and airflow circulation. The bottom of the cold box has evenly distributed support bases to ensure the workpiece is placed stably and symmetrically.
[0031] 2. System Connection: Connect the liquid nitrogen storage tank to the cold box inlet using S30408 stainless steel pipes, and install a diaphragm regulating valve on the pipes. Install temperature transmitters (measurement accuracy ±0.5℃) at three positions on the upper, middle, and lower parts of the cold box inner wall. Arrange two sets of electric heaters, each with a power of 2kW, symmetrically inside the cold box.
[0032] 3. Control System Integration: All temperature transmitter signal lines, diaphragm control valve control lines, and electric heater power lines are connected to an integrated electrical control cabinet. The control cabinet has a built-in PLC controller with PID regulation, data acquisition and storage, and fault alarm functions.
[0033] Safety system verification: Activate the forced ventilation system in the processing area (air exchange rate ≥ 10 times / h), test the oxygen concentration monitor (alarm threshold set to 19.5%), and confirm that the emergency exhaust system and fire-fighting equipment are in usable condition. Operators should wear low-temperature protective clothing, gloves, goggles, and non-slip shoes.
[0034] Step 3: First staged cryogenic treatment and controlled reheating Start the main power supply to the electrical control cabinet and the forced ventilation system. The control system will automatically execute the following process: 1. Segmented cryogenic cooling: Phase 1 (Ambient Temperature → -80℃): Based on feedback from the temperature transmitter, the PID module controls the opening of the diaphragm regulating valve to lower the temperature inside the cold chamber from ambient temperature to -80℃ at an average rate of 4℃ / min. After reaching -80℃, the system maintains a small flow of liquid nitrogen and holds at this temperature for 1.5 hours.
[0035] Second stage (-80℃ → -150℃): The control system adjusts the cooling rate to 2.5℃ / min, continues to cool down to -150℃, and holds at this temperature for 2 hours.
[0036] The third stage (-150℃ → -196℃): The control system further adjusts the cooling rate to 1.5℃ / min, ultimately lowering the cold box temperature to -196℃ (the vaporization temperature of liquid nitrogen), and maintaining this extremely low temperature for 3 hours. Throughout the entire cooling process, temperature fluctuations are controlled within ±2℃.
[0037] 2. Controllable reheating within the cold box: After the cryogenic insulation process is completed, the control system automatically closes the diaphragm regulating valve, cutting off the liquid nitrogen supply. Then, the electric heater inside the cold chamber automatically starts, initiating controlled reheating. First, the temperature is slowly heated from -196℃ to -100℃ at a heating rate of 1.5℃ / min.
[0038] Then, the heating rate was increased to 2.5℃ / min, and the temperature was continued to be heated from -100℃ to room temperature (approximately 22℃).
[0039] Once room temperature is reached, heating is stopped, and the temperature is maintained for 0.5 hours to ensure a uniform and stable overall temperature of the workpiece. This completes the first cryogenic treatment and controlled reheating.
[0040] Step 4: First low-temperature tempering Open the cold box door, lift out the cylinder, and send it directly into the tempering furnace for the first low-temperature tempering. The tempering process parameters are: heat to 240°C at a rate of 9°C / min, hold for 3.8 hours, then turn off the heat source and allow it to cool naturally (air cool) to room temperature inside the furnace.
[0041] Step 5: Second stage of cryogenic treatment and controlled reheating The cylinder, after its first cryogenic tempering, is reinstalled into the cold chamber. The entire process of step three is repeated, including the same segmented cooling rate and target temperature for each stage. The difference is that, to improve processing efficiency, the holding time for both the second and third stages is shortened to 1 hour. After cryogenic treatment, the same controlled reheating procedure as the first time is executed.
[0042] Step Six: Second Low-Temperature Tempering The reheated cylinder was removed from the cold box and subjected to a second low-temperature tempering. The process parameters were: heating to 220°C at a rate of 9°C / min and holding for 3.2 hours. After holding, a stepped cooling method was used: first cooling from 220°C to 100°C at a controlled cooling rate of 5°C / min, and then cooling to room temperature at a rate of 10°C / min.
[0043] Step 7: Post-processing and performance testing The cylinders that have undergone complete heat treatment were then surface-cleaned. Subsequently, samples were taken according to relevant national standards for performance testing, and the results are shown in Table 1.
[0044] Comparative Example 1: The difference from Example 1 is that no cryogenic treatment was performed and the cold box was eliminated. Instead, room temperature reheating was used directly. Subsequently, samples were cut according to relevant national standards and their performance was tested. The results are shown in Table 1.
[0045] Comparative Example 2: The difference from Example 1 is that the cold box was eliminated and room temperature reheating was used directly. Subsequently, samples were cut according to relevant national standards and their performance was tested. The results are shown in Table 1.
[0046] Comparative Example 3: The difference from Example 1 is that after the first tempering, a second deep cooling and tempering is not performed. Subsequently, samples are cut according to relevant national standards and their performance is tested. The results are shown in Table 1.
[0047] Table 1 As can be seen from the above experimental data, the present invention, through a systematic solution of "pre-treatment with specific parameters + segmented deep cryogenic treatment + controllable reheating in the cold box + two synergistic low-temperature tempering", combined with intelligent closed-loop control and safety protection, has successfully solved the key technical problems of high residual austenite content, poor low-temperature dimensional stability and insufficient improvement of mechanical properties in cylinders after deep cryogenic treatment in the prior art.
[0048] Depend on Figure 5-8 It can be seen that, Figure 5 The medium should show a large number of bright, continuous austenite regions with a content as high as 18.5%. The martensite (dark white region) transformation is insufficient, the structure is uneven, and there may be a lot of untransformed residual austenite agglomerates. The process of Comparative Example 1 cannot effectively promote the transformation of austenite to martensite, resulting in poor structural stability.
[0049] Figure 6 The 5.8% decrease in residual austenite content indicates that cryogenic treatment promoted some austenite transformation. However, due to the uncontrollable reheating process, it may lead to large thermal stress during reheating, causing local unevenness or microcracks. Figure 6The middle austenite region should be significantly less Figure 5 However, a certain amount of residual austenite is still distributed.
[0050] Figure 7 The residual austenite content in the medium was 5.2%, slightly lower than that in Comparative Example 2, indicating that controlled reheating helps reduce stress, but still does not achieve the best transformation effect. Figure 7 The austenite region should be further reduced, but sporadic residual austenite can still be seen.
[0051] Figure 8 The retained austenite content is the lowest (4.2%), and almost no obvious austenite region should be visible in the figure. The microstructure is uniform and dense, with sufficient martensite transformation, and the retained austenite exists in a fine, isolated form or is completely transformed.
[0052] In summary, this application completely eliminates the thermal stress and deformation caused by traditional room temperature reheating through "controlled reheating in a cold box," significantly improving dimensional stability from ≤0.05mm in the comparative process to ≤0.02mm (an improvement of 150%). In addition, the synergistic effect of "segmented deep cryogenics" and "two specific tempering processes" in this solution further reduces the retained austenite content from 5.8% to 4.2%, and comprehensively improves the low-temperature tensile strength, hardness, and fatigue strength to 820MPa, 290HBW, and 410MPa, respectively.
[0053] Ultimately, this solution enabled a qualitative leap in the cylinder's structural stability, load-bearing capacity, and dimensional accuracy at an extreme low temperature of -162℃, thus meeting the stringent requirements for long-term reliable service of the BOG compressor.
[0054] Although the invention has been described herein with reference to several illustrative embodiments, it should be understood that many other modifications and implementations can be devised by those skilled in the art, which will fall within the scope and spirit of the principles disclosed herein. More specifically, various variations and modifications can be made to the components and / or layout of the subject matter arrangement within the scope of the disclosure, drawings, and claims. Besides variations and modifications to the components and / or layout, other uses will be apparent to those skilled in the art.
Claims
1. A method for staged deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder, characterized in that, Includes the following steps: S1. Pretreatment: Perform pre-quenching and pre-low temperature tempering treatment on the low-temperature austenitic ductile iron cylinder that has been cast. S2. First stage deep cryogenic treatment: The cylinder processed in step S1 is placed in a sealed cold box, and vaporized liquid nitrogen is introduced into the cold box as a cooling medium. The first stage deep cryogenic treatment is carried out according to the preset multi-stage cooling curve. The multi-stage cooling curve includes at least a first stage from room temperature to a first target temperature, a second stage from the first target temperature to a second target temperature, and a third stage from the second target temperature to a third target temperature, and the cooling rate of each stage is independently controlled. S3. First Controllable Reheating and Low-Temperature Tempering: After completing the cryogenic treatment in step S2, the liquid nitrogen supply is turned off, and the electric heater installed in the cold box is started to heat the cylinder to room temperature in the cold box according to the preset heating rate, thus completing the controllable reheating; then the cylinder is removed from the cold box and the first low-temperature tempering treatment is performed. S4. Second stage deep cryogenic treatment: The cylinder after step S3 is placed back into the cold box, and the stage deep cryogenic treatment process of step S2 is repeated. S5. Second controlled reheating and low-temperature tempering: Repeat the controlled reheating process of step S3, followed by a second low-temperature tempering treatment.
2. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1, characterized in that: In steps S2 and S4, the multi-stage cooling curve is specifically as follows: First stage: Cool from room temperature to -80℃, with the cooling rate controlled at 3-5℃ / min, and keep warm for 1-2 hours after reaching -80℃; The second stage: cooling from -80℃ to -150℃ at a rate of 2-3℃ / min, and holding at -150℃ for 1.5-2.5 hours. The third stage: cooling from -150℃ to -196℃ at a rate of 1-2℃ / min, and holding at -196℃ for 2-4 hours.
3. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1 or 2, characterized in that: In steps S3 and S5, the controllable reheating specifically includes: First stage: Raise the temperature from the final cryogenic temperature to -100℃, with the heating rate controlled at 1-2℃ / min; Second stage: Raise the temperature from -100℃ to room temperature, with the heating rate controlled at 2-3℃ / min.
4. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1, characterized in that: In step S1, the parameters of the pre-quenching treatment are: heating temperature 930-950℃, holding time 2.5-3h, and cooling to room temperature by oil cooling. The parameters for the pre-low temperature tempering treatment are: heating temperature 220-240℃, holding time 3-3.5h, and air cooling to room temperature.
5. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1, characterized in that: In step S3, the parameters for the first low-temperature tempering treatment are: heating temperature 230-250℃, holding time 3.5-4h, and cooling to room temperature by air cooling. In step S5, the parameters for the second low-temperature tempering treatment are: heating temperature 210-230℃, holding time 3-3.5h, and cooling to room temperature using a stepped cooling method.
6. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1, characterized in that: During the cryogenic treatment in steps S2 and S4, the temperature inside the chamber is monitored in real time by a temperature transmitter installed on the cold box, and the temperature signal is transmitted to the electrical control cabinet. The PID control module built into the electrical control cabinet outputs a control signal to the diaphragm regulating valve connected to the liquid nitrogen pipeline according to the deviation between the preset cooling curve and the measured temperature, so as to dynamically adjust the liquid nitrogen flow rate and realize closed-loop precise control of the cooling rate.
7. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1, characterized in that: During the controllable reheating process in steps S3 and S5, the power of the electric heater inside the cold box is adjusted by the electrical control cabinet to achieve closed-loop precise control of the heating rate.
8. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1, characterized in that: The internal volume of the cold box is 1.3 to 1.5 times the volume of the cylinder, and at least two sets of electric heaters are evenly arranged on the inner wall of the cold box.
9. The method for segmented deep cryogenic treatment of a low-temperature austenitic ductile iron cylinder according to claim 1, characterized in that: A safety system is installed in the area where cryogenic treatment is carried out. The safety system includes at least: an oxygen concentration monitor for monitoring the ambient oxygen concentration, a forced ventilation system, an emergency exhaust system, and an audible and visual alarm device; when the oxygen concentration is lower than a preset threshold, an alarm is triggered and the emergency exhaust system is automatically activated.
10. A system for implementing the segmented deep cryogenic treatment method for a low-temperature austenitic ductile iron cylinder as described in any one of claims 1-9, comprising: Liquid nitrogen supply unit, including liquid nitrogen storage tank and connecting pipelines; The processing unit includes at least one sealed cold box for housing the cylinder; The cold box is equipped with an electric heater and a temperature sensor; The control unit includes an electrical control cabinet electrically connected to the temperature sensor, the diaphragm regulating valve on the liquid nitrogen supply line, and the electric heater; the electrical control cabinet is configured to execute control logic as described above. The safety unit includes an oxygen concentration monitor and a ventilation device; both the oxygen concentration monitor and the ventilation device are communicatively connected to the control unit.
Citation Information
Patent Citations
A method for reducing retained austenite in pearlitic gray cast iron during quenching
CN112251579B
Cryogenic treatment process for reducing content of retained austenite in steel and iron material
CN117683981A
Heat treatment process for controlling retained austenite content of carburized part
CN119710164A
Cold water treatment process and device for reducing content of retained austenite in internal structure of bearing steel ball
CN119776622A