A layered heterogeneous duplex stainless steel based on a short-process technology and its preparation method
By performing initial solution treatment, multi-pass cold rolling deformation, and short-time annealing on economical duplex stainless steel slabs, the problems of high risk of hot rolling cracking, long production process, and insufficient strength and plasticity in the traditional preparation of duplex stainless steel have been solved, achieving efficient material preparation and performance improvement.
Patent Information
- Application Number
- CN202611603746.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional duplex stainless steel preparation processes suffer from high risk of hot rolling cracking, long production processes, long annealing times, and insufficient strength-plasticity matching. In particular, how can we construct a layered heterogeneous structure that is conducive to improving the strength-plasticity matching while shortening the annealing time after cold rolling after omitting the hot rolling thinning process?
Using economical duplex stainless steel slabs or plates with a thickness of 4~20mm, after initial solution treatment, rapid water cooling is performed, followed by direct multi-pass cold rolling deformation treatment, combined with short-time annealing treatment, to construct a layered heterogeneous structure, avoid hot rolling thinning, shorten the production process and improve the strength-plasticity matching.
By using direct cold rolling and short-time annealing processes, the production process is significantly shortened, production costs are reduced, the strength-plasticity matching of materials is improved, a layered heterogeneous structure is formed along the rolling direction, the comprehensive mechanical properties of the materials are improved, and they have good engineering application value.
Smart Images

Figure CN123108256A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of heat treatment and rolling technology of metallic materials, and particularly relates to a layered heterogeneous duplex stainless steel based on a short-process technology and its preparation method. Background Technology
[0002] Duplex stainless steel is a stainless steel material composed of both ferrite and austenite phases. In engineering applications, it is usually required that both phases maintain an appropriate volume fraction to obtain good strength, toughness, and corrosion resistance. Among them, the cost-saving duplex stainless steel represented by 2101 duplex stainless steel, by using Mn-N elements to replace Ni elements in alloying, significantly reduces raw material costs and shows good application prospects in petrochemical, marine engineering, energy equipment, rail transportation, and structural steel fields.
[0003] Currently, the industrial production of duplex stainless steel sheets typically involves a traditional process flow including continuous casting of thick slabs, hot rolling for thinning, cold rolling, and annealing. In actual production, the thickness of traditional continuously cast slabs can typically reach 200-220 mm, making direct cold rolling difficult. Therefore, multi-pass hot rolling is necessary for thinning. However, the ferrite and austenite phases in duplex stainless steel differ significantly in chemical composition, crystal structure, stacking fault energy, deformation resistance, and high-temperature mechanical properties. This leads to uneven stress and strain distribution between the two phases during hot working, resulting in deformation incoordination.
[0004] For energy-saving duplex stainless steels, reducing Ni content typically requires increasing the content of austenite-stabilizing elements such as Mn and N. While the addition of N helps stabilize austenite, its solid solution strengthening effect also increases the deformation resistance of the austenite phase, further exacerbating the deformation incompatibility between ferrite and austenite. Under these circumstances, defects such as edge cracking are easily induced during hot rolling, significantly reducing yield and greatly increasing production costs.
[0005] On the other hand, in the traditional manufacturing process, cold-rolled duplex stainless steel usually requires a long annealing process of more than 30 minutes to eliminate cold deformation structure and restore plasticity. However, long annealing not only prolongs the production cycle, increases energy consumption, and reduces production efficiency, but also, compared with austenitic stainless steels such as 304 and 316, conventionally annealed duplex stainless steel still has certain deficiencies in plasticity, making it difficult to meet the needs of higher plasticity applications.
[0006] In recent years, with the development of thin-gauge billet preparation and supply conditions, using thin duplex stainless steel slabs or plates with relatively small thicknesses as starting materials and omitting the hot rolling thinning process in subsequent processing has become a potential way to reduce the risk of hot working cracking, shorten the production process, and reduce energy consumption. However, for energy-saving duplex stainless steel, how to fully utilize the synergistic control of cold rolling deformation and short-time annealing processes to regulate the two-phase microstructure while omitting the subsequent hot rolling thinning process and significantly shortening the annealing time after cold rolling, and thus constructing a layered heterogeneous microstructure within the material that is conducive to improving the strength-plasticity matching, remains a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] To address the problems of high risk of hot rolling cracking, long production process, long annealing time, and insufficient strength-plasticity matching in the traditional preparation process of economical duplex stainless steel, this invention proposes a layered heterogeneous duplex stainless steel based on a short process and its preparation method.
[0008] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing layered heterogeneous duplex stainless steel based on a short-process technology includes the following steps: (1) Solution treatment is performed on the thin slab or plate of economical duplex stainless steel with a thickness of 4~20mm, followed by rapid water cooling to obtain the initial state of duplex stainless steel. (2) After surface treatment of the initial state duplex stainless steel obtained in step (1), it is directly subjected to multi-pass cold rolling deformation treatment to obtain cold-rolled duplex stainless steel. (3) The cold-rolled duplex stainless steel obtained in step (2) is subjected to short-time annealing and then water quenching to obtain layered heterogeneous duplex stainless steel.
[0009] This invention uses economical duplex stainless steel slabs or plates with a thickness of 4-20 mm as the starting material. In subsequent processing, hot rolling thinning is no longer performed. Instead, a combination of initial solution treatment, direct cold rolling, and short-time annealing is used. The layered refinement of the microstructure and deformation-induced phase transformation during cold rolling are utilized, combined with recovery and recrystallization during short-time annealing, to construct a layered heterogeneous microstructure within the material. This shortens the production process, reduces production costs, and improves the strength-plasticity balance of duplex stainless steel.
[0010] Further, in step (1), the energy-saving duplex stainless steel is 2101 energy-saving duplex stainless steel.
[0011] This invention reduces raw material costs while maintaining good overall performance by increasing the content of Mn and N elements and decreasing the content of Ni element. Under the short-process technology of this invention, the lamellar morphology, deformation-induced phase transformation behavior, and the degree of recovery and recrystallization of the two-phase structure can be effectively controlled, which is beneficial for forming a layered heterogeneous structure.
[0012] Further, in step (1), the initial state duplex stainless steel has a total volume fraction of ferrite and austenite phases of 100%, wherein the volume fraction of any one phase is 40~60%, and the other phase is the balance.
[0013] The near-equilibrium ratio of the two phases mentioned above is conducive to the joint participation of the ferrite and austenite phases in cold rolling deformation. Due to the differences in crystal structure and deformation resistance between the two phases, strain distribution occurs during cold rolling, and the phases extend and refine along the rolling direction under the cumulative reduction, providing a basis for the subsequent short-time annealing to construct a layered heterogeneous structure.
[0014] Further, in step (1), the specific operation of the solution treatment is as follows: first, the high temperature furnace is heated to 1050~1150℃, and then the economical duplex stainless steel slab or plate is placed in the high temperature furnace for heat preservation treatment, and the heat preservation time is 30~120min.
[0015] The above-mentioned solid solution parameters are beneficial for adjusting the ratio of the two phases, promoting the re-dissolution of potentially harmful precipitates, and taking into account grain size control, so as to obtain an initial state duplex stainless steel with a suitable ratio of two phases and a relatively uniform microstructure, providing a good microstructure basis for subsequent cold rolling.
[0016] Further, in step (2), the surface treatment includes one or more of polishing, pickling and impurity removal.
[0017] The above surface treatment helps to remove oxide scale and attached impurities from the material surface, reduces the risk of oxide scale being pressed into the matrix and the initiation and propagation of surface cracks, thereby improving the surface quality of the material after cold rolling.
[0018] Further, in step (2), the thickness reduction of each pass in the multi-pass cold rolling deformation process is 0.1~0.3mm, or the reduction rate of each pass is 1~5% based on the initial thickness, until the total reduction rate reaches 60~90%.
[0019] This multi-pass, low-deformation cold rolling process helps avoid edge cracking, while ensuring that the two-phase microstructure achieves sufficient layered refinement and introduces enough deformation energy storage, providing a driving force for recovery and recrystallization during the subsequent short-time annealing process.
[0020] Further, in step (3), the specific operation of the short-time annealing treatment is as follows: first, heat the high-temperature furnace to 800~1050℃, and then place the cold-rolled duplex stainless steel in the high-temperature furnace and keep it warm for 30~180s.
[0021] Compared to traditional long-time annealing (≥30 min), this short-time treatment can promote recovery and recrystallization, improve plasticity, and effectively inhibit grain coarsening and weakening of layered structure. Thus, it retains the layered heterogeneous characteristics and its strengthening effect while significantly shortening the heat treatment time and reducing energy consumption.
[0022] The present invention also provides a layered heterogeneous duplex stainless steel, which is prepared by the above-described preparation method.
[0023] The product has a heterogeneous structure distributed in layers along the rolling direction, which can generate heterogeneous deformation coordination, TWIP / TRIP effect and back stress strengthening effect during deformation, thereby improving work hardening ability and strength-plasticity matching, resulting in excellent comprehensive mechanical properties.
[0024] Furthermore, in the layered heterogeneous duplex stainless steel, the ferrite phase and the austenite phase are distributed in layers along the rolling direction.
[0025] This specific layered heterogeneous morphology is a key structural feature for achieving back stress strengthening and strain distribution coordination, which helps to delay local necking and enable the material to achieve excellent elongation while maintaining high strength.
[0026] The present invention also provides an application of the above-mentioned layered heterogeneous duplex stainless steel in the fields of petrochemicals, marine engineering, energy equipment, rail transportation, or structural steel.
[0027] This material combines high strength, high plasticity, and excellent corrosion resistance, which can meet the comprehensive requirements of structural materials for safety, durability, and lightweighting under the above-mentioned harsh working conditions, and has broad prospects for engineering applications.
[0028] Compared with the prior art, the present invention has the following advantages and technical effects: 1. This invention uses economical duplex stainless steel slabs or plates with a thickness of 4~20mm as the starting material. In subsequent processing, hot rolling thinning is no longer performed, but cold rolling deformation is performed directly, which helps to reduce the risk of cracking during hot rolling, shorten the production process, and reduce production costs.
[0029] 2. This invention uses direct cold rolling with a large reduction rate of 60-90% to refine the microstructure of duplex stainless steel along the rolling direction and promote deformation-induced phase transformation of austenite, thereby providing a microstructure basis for the formation of layered heterostructure.
[0030] 3. This invention uses a short-time annealing treatment of 800~1050℃ for 30~180s to replace the traditional long-time annealing treatment of more than 30min. While achieving microstructure control, it significantly shortens the heat treatment time, reduces energy consumption, and improves production efficiency.
[0031] 4. This invention, through the synergistic control of direct cold rolling and short-time annealing, forms a layered heterogeneous structure distributed along the rolling direction in the material. This structure facilitates the coordination of heterogeneous deformation and back stress strengthening during plastic deformation, improves the material's work hardening ability, and thus improves the strength-plasticity balance of energy-saving duplex stainless steel.
[0032] 5. The process flow of this invention is simple, the range of process parameters is clear, and it can be implemented using conventional cold rolling equipment and annealing equipment, thus having good industrial adaptability and application value. Attached Figure Description
[0033] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 Equilibrium phase diagram of 2101 energy-saving duplex stainless steel calculated by JMatPro software; Figure 2 This is a schematic diagram of the process for preparing layered heterogeneous duplex stainless steel based on the short-process technology of the present invention. Figure 3 The OM diagrams are of the initial state duplex stainless steel obtained after solution treatment of duplex stainless steel in Examples 1-7 of this invention. Figure 4 These are SEM images of the duplex stainless steel cold-rolled with a 90% reduction in Examples 1-7 of this invention; Figure 5 The EBSD phase diagrams for cold rolling of duplex stainless steel with a 90% reduction in the present invention are shown in Examples 1-7 of this invention. Figure 6 The image shows the EBSD phase diagram of duplex stainless steel after cold rolling and annealing at 1030°C for 60 seconds in Example 6 of this invention. Figure 7 The image shows the EBSD phase diagram of duplex stainless steel in Comparative Example 2 of this invention after being cold-rolled and reduced by 90% and then annealed at 1030°C for 300 min. Figure 8 The figures are stress-strain curves of room temperature tensile engineering under different annealing parameters in Examples 1 to 7 of the present invention; wherein, (a) is an example with different annealing times at 800℃, and (b) is an example and a comparative example annealed at different temperatures for 60s. Figure 9 This is a comparison chart of room temperature tensile properties under different annealing parameters in Examples 1-7 (corresponding to S1-S7 in the figure) and Comparative Examples 1-2 (corresponding to D1 and D2 in the figure); Where α represents ferrite, γ represents austenite, α´ represents α´-martensite, and ε represents ε-martensite. Detailed Implementation
[0034] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0035] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0036] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0037] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0038] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0039] This invention provides a method for preparing layered heterogeneous duplex stainless steel based on a short-process technology, comprising the following steps: (1) Initial solution treatment: The thin slab or plate of economical duplex stainless steel with a thickness of 4~20mm is subjected to solution treatment and then rapidly water-cooled to obtain the initial state of duplex stainless steel. (2) Direct cold rolling treatment: After surface treatment of the initial state duplex stainless steel obtained in step (1), hot rolling thinning treatment is no longer performed. Instead, multiple cold rolling deformation treatment is performed directly to make the duplex stainless steel structure layered and refined along the rolling direction, and to promote the deformation-induced phase transformation of austenite, thus obtaining cold-rolled duplex stainless steel. (3) Short-time annealing treatment: The cold-rolled duplex stainless steel obtained in step (2) is subjected to short-time annealing treatment, followed by water quenching and cooling to obtain layered heterogeneous duplex stainless steel.
[0040] In step (1) of the following preferred embodiment of the present invention, the energy-saving duplex stainless steel is 2101 energy-saving duplex stainless steel.
[0041] In step (1) of the following preferred embodiment of the present invention, the sum of the volume fractions of ferrite phase and austenite phase in the initial state duplex stainless steel is 100%, wherein the volume fraction of ferrite phase is 40~60% and the volume fraction of austenite phase is the balance.
[0042] In step (1) of the following optional embodiments of the present invention, the specific operation of the solution treatment is as follows: first, the high temperature furnace is heated to 1050~1150℃ (e.g., 1080℃), and then the economical duplex stainless steel slab or plate is placed in the high temperature furnace for heat preservation treatment, and the heat preservation time is 30~120min (e.g., 30min).
[0043] In step (2) of the following optional embodiments of the present invention, the surface treatment includes one or more of polishing, pickling, and impurity removal. The specific operation of polishing is as follows: the surface of the plate is mechanically polished with 80#~240# alumina sandpaper to remove the surface oxide scale. The polishing direction is along the rolling direction. After polishing, the surface roughness Ra≤3.2μm. The specific operation of pickling is as follows: the plate is immersed in a pickling solution at a temperature of 40~70℃. The pickling solution is composed of 5~15% HNO3 and 1~5% HF aqueous solution by volume. The plate is soaked for 5~30 minutes until the surface oxide scale is completely dissolved and a uniform silvery-white metallic luster is presented. The specific operation of impurity removal is as follows: the plate after pickling is first rinsed with flowing deionized water until the surface pH is neutral. Then, it is ultrasonically cleaned with acetone or anhydrous ethanol for 5~15 minutes to remove residual oil and impurities on the surface. Finally, it is rinsed with deionized water and dried with cold air.
[0044] In step (2) of the following optional embodiments of the present invention, the thickness reduction of each pass of the multi-pass cold rolling deformation process is 0.1~0.3mm (e.g. 0.2mm), or the reduction rate of each pass is 1~5% based on the initial thickness, until the total reduction rate reaches 60~90% (e.g. 90%).
[0045] In step (3) of the following optional embodiments of the present invention, the specific operation of the short-time annealing treatment is as follows: first, the high-temperature furnace is heated to 800~1050℃ (such as 800℃, 850℃, 900℃, 950℃ and 1030℃), and then the cold-rolled duplex stainless steel is placed in the high-temperature furnace and kept for 30~180s (such as 30s, 60s and 180s).
[0046] Using the above preparation method, a layered heterogeneous duplex stainless steel can be prepared, in which the ferrite phase and austenite phase are distributed in layers along the rolling direction.
[0047] Layered heterostructure duplex stainless steel can be used in petrochemical, marine engineering, energy equipment, rail transportation, or structural steel applications.
[0048] The material used in the embodiments of this invention is 2101 energy-saving duplex stainless steel, the chemical composition of which is shown in Table 1. Unless otherwise specified, the following embodiments all use the same batch of 2101 energy-saving duplex stainless steel sheet as raw material.
[0049] Table 1 Chemical composition (wt.%) of 2101 energy-saving duplex stainless steel The equipment used in this embodiment of the invention includes a twin-roll mill with cold rolling function and a muffle furnace. The twin-roll mill is used only for room temperature cold rolling deformation processing and is not used for hot rolling thinning processing.
[0050] Figure 1 The equilibrium phase diagram of 2101 economical duplex stainless steel calculated by JMatPro software.
[0051] Figure 2 This is a schematic diagram of the process for preparing layered heterogeneous duplex stainless steel based on a short-process technology according to the present invention.
[0052] Unless otherwise specified, "room temperature" in this invention refers to 25±2℃.
[0053] All raw materials used in this invention were purchased from the market.
[0054] The technical solution of the present invention will be further illustrated by the following embodiments.
[0055] Examples 1-7 A method for preparing layered heterogeneous duplex stainless steel based on a short-process technology, except for differences in annealing temperature and annealing time (see Table 2), uses the same initial solution treatment and direct cold rolling steps in Examples 1-7, as detailed below: (1) Initial solution treatment A rectangular sample with dimensions of 90mm×50mm×10mm was cut from a 2101 energy-saving duplex stainless steel sheet. The muffle furnace was first heated to 1080℃, and then the sample was placed at 1080℃ and held for 30 minutes. After that, it was taken out and quickly water-cooled to room temperature to obtain the initial state of duplex stainless steel. (2) Surface treatment Use 200# sandpaper to polish the surface of the solid solution sample to remove the oxide scale and impurities. Then clean it with deionized water and alcohol and dry it with cold air. (3) Direct cold rolling The sample obtained in step (2) was subjected to room temperature multi-pass cold rolling treatment using a twin-roll mill with synchronous rotation of upper and lower rolls. The thickness reduction in each pass was about 0.2 mm until the total reduction rate reached 90%, and finally a cold-rolled duplex stainless steel with a thickness of about 1 mm was obtained. (4) Short-time annealing treatment The cold-rolled duplex stainless steel with a total reduction rate of 90% obtained in step (3) was placed in a muffle furnace preheated to a set temperature for short-term annealing. After annealing, the sample was immediately taken out and quenched in room temperature water to room temperature to obtain layered heterogeneous duplex stainless steel.
[0056] Table 2. Short-time annealing parameters and ferrite phase content of Examples 1-7 Comparative Example 1 Same as Example 1, except that step (4) is omitted.
[0057] Comparative Example 2 Same as Example 1, except that in step (4), the annealing temperature is 1030℃ and the annealing time is 300min.
[0058] OM Organizational Analysis: Depend on Figure 3 It can be seen that the 2101 duplex stainless steel after initial solution treatment is mainly composed of ferrite and austenite, with the two phases interspersed, but the microstructure is relatively large and has not yet formed an obvious fine layered structure.
[0059] SEM tissue analysis: After direct cold rolling with a 90% reduction rate, such as Figure 4 As shown, both ferrite and austenite undergo significant elongation, flattening, and refinement along the rolling direction, transforming the initial coarse blocky or strip-like structure into a continuous or semi-continuous thin-layered structure. This result indicates that direct cold rolling with a large reduction rate can effectively refine the two-phase structure and construct a layered structure arranged along the rolling direction within the material, providing a basis for the formation of a layered heterogeneous structure during subsequent short-time annealing. During large deformation cold rolling, ferrite and austenite exhibit significant differences in strain distribution due to differences in crystal structure, deformation resistance, and plastic deformation mechanism. Simultaneously, some metastable austenite undergoes deformation-induced phase transformation, resulting in the simultaneous presence of different phase structures within the cold-rolled microstructure.
[0060] EBSD tissue analysis: Depend on Figure 5 The EBSD results of the cold-rolled state show that after 90% cold rolling, the two-phase structure is significantly elongated along the rolling direction and arranged in a layered manner. At the same time, deformation-induced phase transformation characteristics can be observed.
[0061] Depend on Figure 6It can be seen that after short-time annealing at 1030℃ for 60s, the material still retains obvious two-phase layered distribution characteristics, and fine recrystallized grains have formed in local areas.
[0062] The aforementioned layered heterogeneous structure can constrain and coordinate the plastic deformation in different regions during tensile testing. The strain distribution and interface constraints between soft and hard regions help delay local strain concentration and maintain the material's work hardening ability, enabling short-time annealed specimens to achieve high elongation and strength-ductility product while maintaining a certain strength.
[0063] In contrast, by Figure 7 It can be seen that after long-term annealing at 1030℃ for 300 min, the original layered structure distributed along the rolling direction was significantly weakened, and ferrite and austenite gradually transformed into larger equiaxed grains, with a significant increase in the degree of homogenization and coarsening of the structure. The weakening of the layered heterogeneous characteristics reduced the synergistic deformation effect between different structural regions, which corresponds to the lower strength, elongation after fracture, and strength-ductility product of Comparative Example 2.
[0064] Based on the combined results of OM, SEM, EBSD and room temperature tensile testing, it can be seen that the present invention uses a combination of direct cold rolling with a large reduction rate and short-time annealing, which can promote a certain degree of recovery and recrystallization while avoiding excessive grain growth caused by long-term high-temperature annealing, and retaining the layered heterogeneous structure distributed along the rolling direction, thereby achieving a synergistic improvement in material strength and plasticity.
[0065] Room temperature tensile properties analysis: To evaluate the mechanical properties of the layered heterostructure duplex stainless steel prepared in this invention, room temperature uniaxial tensile tests were conducted on the samples obtained in Examples 1-7 and Comparative Examples 1-2. The tensile tests were performed using an INSTRON 8801 electro-hydraulic servo fatigue testing system, and the specimen dimensions conformed to GB / T 228.1-2021. Tensile specimens were cut along the rolling direction at a tensile speed of 1 mm / min. The engineering stress-strain curves of each sample were obtained through testing, and their yield strength, tensile strength, elongation after fracture, and strength-ductility product were calculated. The strength-ductility product was calculated as the product of tensile strength and elongation after fracture, with elongation after fracture expressed as a percentage. At least three parallel specimens were tested under each process condition. The room temperature tensile properties of the layered heterostructure duplex stainless steel under different short-time annealing parameters are shown in Table 3, and the results listed in Table 3 are representative test results. The engineering stress-strain curves are shown in Table 3. Figure 8 As shown, tensile properties are compared to... Figure 9 As shown.
[0066] Table 3. Room temperature tensile properties of layered heterogeneous duplex stainless steel under different short-time annealing parameters From Table 3, Figure 8 and Figure 9 It can be seen that after direct cold rolling with a 90% reduction rate, the yield strength and tensile strength of Comparative Example 1 reached 1352.8 MPa and 1473.0 MPa, respectively, but the elongation after fracture was only 3.09%, and the strength-ductility product was 4.55 GPa·%. This indicates that cold rolling with a large reduction rate can significantly improve the material strength through work hardening, but the material plasticity is severely reduced, making it difficult to meet the requirement of synergistic matching of strength and plasticity.
[0067] Compared with Comparative Example 1, after short-time annealing, the yield strength and tensile strength of Examples 1-7 decreased, while the elongation after fracture and the strength-ductility product were significantly improved. This indicates that short-time annealing can promote the recovery and recrystallization of deformed structures and improve the plastic deformation capacity of materials while retaining some of the strengthening effect of cold rolling.
[0068] When the annealing temperature remained constant at 800℃, as the annealing time increased from 30s to 60s and then to 180s, the yield strength of the material decreased from 785.9MPa to 756.1MPa and 614.9MPa, respectively, and the tensile strength decreased from 969.5MPa to 955.8MPa and 883.3MPa, respectively. Simultaneously, the elongation after fracture increased from 33.29% to 39.18% and 45.70%, respectively, and the strength-ductility product increased from 32.27 GPa·% to 37.44 GPa·% and 40.37 GPa·%. These results indicate that at lower annealing temperatures, appropriately extending the annealing time is beneficial for improving the overall strength and ductility properties; however, excessively long annealing times further weaken the work hardening effect, leading to a decrease in strength.
[0069] With the annealing time remaining constant at 60 s, as the annealing temperature increased from 800℃ to 900℃, the yield strength of the material decreased from 756.1 MPa to 596.0 MPa, the tensile strength decreased from 955.8 MPa to 846.0 MPa, while the elongation after fracture increased from 39.18% to 56.79%, and the strength-ductility product increased from 37.44 GPa·% to 48.04 GPa·%. This indicates that increasing the annealing temperature can accelerate the recovery and recrystallization processes, thereby improving the material's plasticity.
[0070] When the annealing temperature was further increased to 950℃ and 1030℃, the material still maintained high plasticity. Specifically, the elongation after fracture in Examples 6 and 7 were 53.91% and 55.86%, respectively, and the strength-ductility product was 44.04 GPa·% and 44.05 GPa·%, respectively. The yield strength of Example 7 was higher than that of Example 6, while the tensile strength continued to decrease, indicating that the yielding behavior under high-temperature short-time annealing conditions does not simply change monotonically with temperature, but is influenced by a combination of factors such as the two-phase ratio, the degree of recovery and recrystallization, and the grain structure.
[0071] Specifically, Example 7 and Comparative Example 2 used the same annealing temperature of 1030℃, but the holding time in Example 7 was only 60s, while the holding time in Comparative Example 2 was 300min. The yield strength, tensile strength, elongation after fracture, and strength-ductility product of Example 7 were 655.3MPa, 788.5MPa, 55.86%, and 44.05GPa·%, respectively, all higher than those of Comparative Example 2 (448.1MPa, 699.2MPa, 42.98%, and 30.05GPa·%). Compared with Comparative Example 2, the yield strength of Example 7 increased by approximately 46.2%, the tensile strength increased by approximately 12.8%, the elongation after fracture increased by approximately 30.0%, and the strength-ductility product increased by approximately 46.6%, while the annealing holding time was shortened to 1 / 300 of that of Comparative Example 2. The above results indicate that prolonged annealing weakens the layered structure and coarsens the grains, which not only reduces the material strength but also makes it difficult to maintain a high work hardening capacity. Short-time annealing, on the other hand, can suppress the coarsening of the structure and obtain better comprehensive mechanical properties while significantly shortening the heat treatment time.
[0072] In summary, this invention allows for effective control of material strength and plasticity over a wide range by adjusting the annealing temperature and time. Lower annealing temperatures or shorter annealing times help retain the strengthening effect of cold rolling, maintaining higher material strength; appropriately increasing the annealing temperature or extending the annealing time promotes microstructure recovery and recrystallization, improving material plasticity. Among these, the 900℃×60s short-time annealing regime exhibits the best overall strength and plasticity performance.
[0073] Conclusion: This invention proposes a method for preparing layered heterogeneous duplex stainless steel based on a short-process technology. This method uses economical duplex stainless steel slabs or plates with a thickness of 4-20 mm as starting material. An initial solution treatment is performed to obtain a ferrite-austenite duplex microstructure. Subsequently, the hot rolling thinning process is omitted, and the steel undergoes 60-90% multi-pass cold rolling deformation, combined with short-time annealing at 800-1050℃ for 30-180s and water quenching, to prepare heterogeneous duplex stainless steel with a layered distribution along the rolling direction.
[0074] Direct cold rolling can refine ferrite and austenite into layers and introduce higher deformation energy storage; short-time annealing can promote microstructure recovery and recrystallization, while retaining some of the strengthening effect of cold rolling and the characteristics of layered microstructure, thereby improving the strength-plasticity matching of the material.
[0075] The yield strength of Examples 1-7 ranged from 475.0 to 785.9 MPa, the tensile strength from 788.5 to 969.5 MPa, the elongation after fracture from 33.29% to 56.79%, and the strength-ductility product from 32.27 to 48.04 GPa·%. Among them, the specimen annealed at 900℃ for 60s had the highest strength-ductility product and the best overall performance.
[0076] Compared with traditional long-time annealing, the short-time annealing of this invention can suppress grain coarsening and layered structure weakening, and significantly shorten the heat treatment time while maintaining good mechanical properties. It has the advantages of reducing energy consumption, improving production efficiency and reducing the risk of hot rolling cracking, and has good engineering application value.
[0077] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for preparing layered heterogeneous duplex stainless steel based on a short-process technology, characterized in that, Includes the following steps: (1) Solution treatment is performed on the thin slab or plate of economical duplex stainless steel with a thickness of 4~20mm, followed by rapid water cooling to obtain the initial state of duplex stainless steel. (2) After surface treatment of the initial state duplex stainless steel, it is directly subjected to multi-pass cold rolling deformation treatment to obtain cold-rolled duplex stainless steel. (3) The cold-rolled duplex stainless steel is subjected to short-time annealing treatment, followed by water quenching to obtain layered heterogeneous duplex stainless steel; the temperature of the short-time annealing treatment is 800~1050℃ and the time is 30~180s.
2. The preparation method according to claim 1, characterized in that, In step (1), the energy-saving duplex stainless steel is 2101 energy-saving duplex stainless steel.
3. The preparation method according to claim 1, characterized in that, In step (1), the initial state duplex stainless steel has a total volume fraction of ferrite and austenite phases of 100%, with one phase having a volume fraction of 40-60% and the other phase being the balance.
4. The preparation method according to claim 1, characterized in that, In step (1), the specific operation of the solution treatment is as follows: first, heat the high temperature furnace to 1050~1150℃, and then place the economical duplex stainless steel slab or plate in the high temperature furnace for heat preservation treatment for 30~120min.
5. The preparation method according to claim 1, characterized in that, In step (2), the surface treatment includes one or more of polishing, pickling and impurity removal.
6. The preparation method according to claim 1, characterized in that, In step (2), the thickness reduction of each pass in the multi-pass cold rolling deformation process is 0.1~0.3mm, or the reduction rate of each pass is 1~5% based on the initial thickness, until the total reduction rate reaches 60~90%.
7. The preparation method according to claim 1, characterized in that, In step (3), the temperature of the short-time annealing treatment is 850℃~950℃ and the time is 60s.
8. A layered heterogeneous duplex stainless steel, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 7.
9. The layered heterogeneous duplex stainless steel according to claim 8, characterized in that, In the layered heterogeneous duplex stainless steel, the ferrite and austenite phases are distributed in layers along the rolling direction.
10. The application of the layered heterogeneous duplex stainless steel as described in claim 8 or 9 in the fields of petrochemicals, marine engineering, energy equipment, rail transportation, or structural steel.