Method for improving continuous casting and rolling production efficiency of thin slab
Through cross casting and automatic deviation correction technology, combined with thick-specification auxiliary steel grades, the problems of low production efficiency and low spot rate of continuous casting and rolling of thin slabs in the CSP process are solved, achieving efficient production and cost reduction.
Patent Information
- Application Number
- CN202411304081.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-19
AI Technical Summary
In the CSP process, the production efficiency of thin slab continuous casting and rolling is low, resulting in high production costs and low spot rates, and the lack of flexible production organization and transition material matching problems.
The cross-casting production mode is adopted to form a slab by cross-casting pickled steel and auxiliary steel grades, and thick-specification auxiliary steel grades are used for hot rolling transition rolling in the finishing mill, combining automatic deviation correction and pinch roll pressure control. , ensure the fast and smooth transition of the centerline of the slab.
It significantly improves production organization flexibility and production efficiency, reduces costs, reduces the spot rate from 16% to less than 5%, reduces the generation of transition materials, and extends the service life of pinch rollers.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for improving the production efficiency of thin slab continuous casting and rolling. Background Art
[0002] Under the background of green manufacturing in the steel industry, the production of thin-gauge pickled steel using the thin-slab continuous casting and rolling process represented by the CSP process has become an industry development trend, but the production potential has not yet been fully tapped. The limiting link is that the thin-slab continuous casting has not fully achieved efficient production. CSP continuous casting cannot achieve quick change of the tundish. Generally, the same steel grade batch is adopted, and the width of the single-casting slab is set once. There is no large vertical roller and fixed-width press in front of the finishing mill, so there is little room for adjusting the width of the finished product. The integration of casting and rolling makes the production organization of the thin-slab continuous casting and rolling process less flexible than the conventional process. The contract volume of certain specific varieties and specifications is small, and there are problems of high production cost and low production efficiency. For specific varieties and specifications of the CSP process, it is necessary to systematically optimize the process and equipment in combination with the characteristics of the production line to achieve efficient continuous casting of thin slabs.
[0003] In addition, there are only thin-gauge contracts for pickled steel, and no hot-roll transition materials. After each roll change of the finishing mill, a certain amount of thick-gauge transition materials need to be rolled to meet the needs of hot-rolling. In addition, due to the difference in the centering of the two-stream caster slabs in the CSP process, the transition needs to be split, which will produce a large amount of transition materials without the corresponding thickness order matching, resulting in a pickled steel spot rate of up to 16%, which seriously reduces the profitability of pickled steel. Similar production lines in the industry also have similar problems, and there is no mature solution. Summary of the invention
[0004] The purpose of the present invention is to provide a method for improving the production efficiency of thin slab continuous casting and rolling, which can significantly improve the flexibility of process production organization and the production efficiency of thin slab continuous casting and rolling, and reduce production costs while ensuring stable production and quality.
[0005] The technical solution adopted by the present invention is: A method for improving the production efficiency of thin slab continuous casting and rolling, comprising the following steps: S1, smelting molten steel according to the requirements of pickled steel and auxiliary steel grades; S2, pickled steel and auxiliary steel grades are cross-cast to form their respective slabs; S3, according to the detection data of the offset of the cast slab out of the soaking furnace, the slab is adjusted to ensure that the slab is transported to the seven-stand finishing mill along the rolling center line; S4, in the seven-stand finishing mill stage, after the working rolls are replaced in the finishing rolling, thick auxiliary steel grades are used for hot roll transition rolling, and then thin pickled steel is directly rolled; this can solve the problem that there is no contract for thick pickled steel, resulting in a large amount of hot roll transition materials without corresponding orders, resulting in a high spot rate; S5, during the coiling stage, the pinch roller pressure is controlled in sections.
[0006] Preferably, the casting machine pulling speed during casting of pickled steel and auxiliary steel types is set according to the principle that the thinner the slab thickness, the narrower the slab width, and the lower the superheat of the molten steel, the faster the casting machine pulling speed.
[0007] Preferably, the slab thickness is controlled at 60-85 mm, the slab width is controlled at 1050-1550 mm, and the casting machine pulling speed is controlled at 4.1-5.5 m / min. Preferably, when the width of the pickled steel and the auxiliary steel slabs are inconsistent, the crystallizer is quickly adjusted in width for a smooth transition during cross-casting. During rapid width adjustment, the casting machine pulling speed is controlled according to the auxiliary steel pulling speed. The rapid width adjustment rate is 40-50mm / s, the single width adjustment amount is ≤100mm, the interval time for each adjustment is t1, the total width adjustment amount in one casting is ≤500mm, and the taper is adjusted synchronously during rapid width adjustment. Preferably, the interval time t1 is 2 minutes.
[0008] Preferably, the pickled steel and the auxiliary steel are produced by cross-casting in the same strand casting machine, and each strand casting machine is equipped with a soaking furnace for heating. In step S2, the two strand casting machines produce synchronously and are heated in two soaking furnaces respectively.
[0009] Preferably, in said step S3, during the slab centering adjustment process, the deviation between the slab center line of the two-strand casting machine and the rolling center line is controlled to be ≤8mm, and the deviation of the slab center line of the two-strand casting machine is controlled to be ≤5mm.
[0010] Preferably, in the step S3, the control sequence is to start the automatic deviation correction function while the vertical roll bites the steel, and end it before the working rolls of the frame F1 of the finishing mill bite the steel, control the vertical roll pressure to 300~500KN, and the slab running speed in front of the frame F1 of the finishing mill is 0.2~0.5m / s.
[0011] Preferably, the chemical composition of the pickled steel, measured by mass percentage, includes: C: 0.04-0.07%, Si: 0.02-0.10%, Mn: 0.35-0.85%, P≤0.015%, S≤0.008%, Cr: 0.20-0.40%, Ti: 0.02-0.08%, Nb: 0.02-0.04%, Als: 0.02-0.05%, N≤0.007%, and the balance is Fe and unavoidable impurities.
[0012] Preferably, the auxiliary steel grade is ordinary C-Mn steel.
[0013] Preferably, in S5, the pressure of the pinch roller at the strip head is controlled to be 50~120KN; when the strip head enters the coiler, the reel load is connected and delayed for a period of time t2, the pinch roller light pressure mode is started, and the pinch roller pressure is reduced to 10~20KN; when the steel throwing signal of the frame F3 of the finishing mill is connected, the pinch roller light pressure mode is released, and the pinch roller pressure is controlled at 60~144KN.
[0014] t2 is 10 seconds.
[0015] The seven-stand finishing mill group includes seven stands, which are marked as F1, F2, F3, F4, F5, F6 and F7 respectively.
[0016] The beneficial effects of the present invention are: The present invention uses thin slab continuous casting rapid width adjustment technology, thin slab continuous casting adopts cross casting production mode, and the finishing rolling unit simultaneously adopts thick auxiliary steel grades for hot roller transition rolling. Under the premise of ensuring stable production and quality, the flexibility of process production organization and the production efficiency of thin slab continuous casting and rolling are significantly improved, and the difference in the centering of the two-stream casting machine slab can be eliminated through automatic deviation correction, which is conducive to the rapid and smooth transition rolling after the finishing rolling work roll is replaced. Thick auxiliary steel grades are used for hot roller transition rolling, and then thin pickled steel is directly rolled, which can solve the problem that there is no thick specification contract for pickled steel, a large number of hot roller transition materials are generated without corresponding order matching, resulting in a high spot rate, and the process cost is reduced by more than 50 yuan / ton, and the spot rate of pickled steel is reduced from 16% to less than 5%. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Schematic diagram of the operation of the crystallizer in the embodiment of the present invention.
[0018] Figure 2 It is a cross-sectional view of a crystallizer locking device according to an embodiment of the present invention.
[0019] In the figure: 1- measuring instrument; 2- crystallizer; 3- ingot; 4- adjusting pad; 5- disc spring; 6- oil cylinder. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0021] In the description of the present invention, it should be understood that if the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like are involved, the orientation or position relationship indicated is based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0022] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection. It can be a mechanical connection or an electrical connection. It can be directly connected or indirectly connected through an intermediate medium. It can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0023] Example 1 A method for improving the production efficiency of thin slab continuous casting and rolling, comprising the following steps: S1, smelting molten steel according to the requirements of pickled steel and auxiliary steel grades; S2, pickled steel and auxiliary steel grades are cross-cast to form their respective slabs; S3, according to the slab offset detection data out of the soaking furnace, the slab is centered and adjusted to ensure that the slab is transported to the seven-stand finishing mill along the rolling center line; S4, in the seven-stand finishing mill stage, after the working rolls are replaced for finishing rolling, thick auxiliary steel grades are used for hot roll transition rolling, and then thin pickled steel is directly rolled; this can solve the problem that there is no thick specification contract for pickled steel, resulting in a large amount of hot roll transition materials without corresponding orders to match, resulting in a high spot rate.
[0024] S5, during the coiling stage, the pinch roller pressure is controlled in sections.
[0025] Furthermore, when casting the pickled steel and the auxiliary steel, the casting machine pulling speed is set according to the principle that the thinner the slab thickness, the narrower the slab width, and the lower the superheat of the molten steel, the faster the casting machine pulling speed.
[0026] Furthermore, the slab thickness is controlled at 60-85 mm, the slab width is controlled at 1050-1550 mm, and the casting machine pulling speed is controlled at 4.1-5.5 m / min. Furthermore, when the width of the pickled steel and the auxiliary steel slabs are inconsistent, the crystallizer is quickly adjusted in width for a smooth transition during cross-casting. During rapid width adjustment, the casting machine pulling speed is controlled according to the auxiliary steel pulling speed. The rapid width adjustment rate is 40~50mm / s, the single width adjustment amount is ≤100mm, the interval time for each adjustment is t1, the total width adjustment amount in one casting is ≤500mm, and the taper is adjusted synchronously during rapid width adjustment. Furthermore, the interval time t1 is 2 minutes.
[0027] Furthermore, the pickled steel and the auxiliary steel are cross-casted in the same strand casting machine, and each strand casting machine is equipped with a soaking furnace for heating. In step S2, the two strand casting machines produce synchronously and are heated in two soaking furnaces respectively.
[0028] Furthermore, in the step S3, during the slab centering adjustment process, the deviation between the slab center line of the two-strand casting machine and the rolling center line is controlled to be ≤8mm, and the deviation of the slab center line of the two-strand casting machine is controlled to be ≤5mm.
[0029] Furthermore, in the step S3, during the slab centering adjustment process, the control sequence is to start the automatic deviation correction function while the vertical roll bites the steel, and end it before the working rolls of the frame F1 of the finishing mill bite the steel, and the vertical roll pressure is controlled to be 300~500KN, and the slab running speed in front of the frame F1 of the finishing mill is 0.2~0.5m / s.
[0030] Example 2 On the basis of Example 1, the parameters of the pickled steel and the auxiliary steel types are further limited, and the performance of Example 2 after the limitation is better.
[0031] The chemical composition of the pickled steel, measured by mass percentage, includes: C: 0.04-0.07%, Si: 0.02-0.10%, Mn: 0.35-0.85%, P≤0.015%, S≤0.008%, Cr: 0.20-0.40%, Ti: 0.02-0.08%, Nb: 0.02-0.04%, Als: 0.02-0.05%, N≤0.007%, and the balance is Fe and unavoidable impurities.
[0032] Furthermore, the auxiliary steel grade is ordinary C-Mn steel.
[0033] Furthermore, in S5, the pressure of the pinch roller at the head of the strip is controlled to be 50~120KN; when the head of the strip enters the coiler, the reel load is connected and delayed for a period of time t2, the pinch roller light pressure mode is started, and the pinch roller pressure is reduced to 10~20KN; when the steel throwing signal of the frame F3 of the finishing mill is connected, the pinch roller light pressure mode is released, and the pinch roller pressure is controlled at 60~144KN.
[0034] t2 is 10 seconds.
[0035] The seven-stand finishing mill group includes seven stands, which are marked as F1, F2, F3, F4, F5, F6 and F7 respectively.
[0036] Working principle of the present invention: A method for manufacturing pickled steel in a thin slab continuous casting and rolling process mainly comprises the following steps: molten steel smelting → two-stream thin slab continuous casting → two soaking furnaces heating → thin slab automatic deviation correction → vertical roll rolling → seven-stand finishing rolling → laminar cooling → coiling, thereby obtaining a pickled steel hot-rolled raw material coil, and then obtaining a final pickled steel coil through pickling.
[0037] (1) During the smelting stage, molten steel is smelted according to the composition requirements of pickled steel and auxiliary steel grades.
[0038] (2) In the two-strand thin slab continuous casting stage, the pickling steel and auxiliary steel grades are cross-casting production modes, that is, 1 furnace of auxiliary steel grade → 3 furnaces of pickling steel → 1 furnace of auxiliary steel grade → 3 furnaces of pickling steel, and so on. The slab thickness is controlled at 60~85mm, the slab width is 1050~1550mm, and the casting machine pulling speed is 4.1~5.5m / min. The slab thickness, width, and casting machine pulling speed are adjusted while cross-casting. When casting pickling steel and auxiliary steel grades, the casting machine pulling speed is set according to the principle that the thinner the slab thickness, the narrower the slab width, the lower the superheat of the molten steel, and the faster the casting machine pulling speed. See the table below for details:
[0039] When the width of the pickled steel and auxiliary steel slabs are inconsistent, the rapid width adjustment technology is used to achieve a smooth width transition during cross-casting. During rapid width adjustment, the casting machine pulling speed is controlled according to the auxiliary steel pulling speed. The rapid width adjustment rate is 40~50mm / s, the single width adjustment amount is ≤100mm, the interval between each adjustment is 2min, the total width adjustment amount in one casting is ≤500mm, and the taper is adjusted synchronously during rapid width adjustment.
[0040] The locking force requirements of the crystallizer locking device are: when the width is adjusted quickly, the locking pressure is 45-75 bar at the top and 88-138 bar at the bottom.
[0041] In order to meet the above requirements for rapid width adjustment, the mold locking device needs to provide sufficient locking force, otherwise it will cause polarization of the continuous caster.
[0042] The crystallizer locking principle: the oil cylinder is pressed upward, the piston rod moves upward, compresses the butterfly spring, and the locking rod moves upward, which loosens the crystallizer; after the oil cylinder is depressurized, the elastic force of the butterfly spring makes the locking rod move downward, thereby locking the crystallizer. The crystallizer is locked by the elastic force generated by the compression of the butterfly springs, and the compression of the butterfly spring can be adjusted by adjusting the gasket, thereby changing the size of the locking force.
[0043] The crystallizer vibration moves in a sinusoidal curve. At zero position, the speed is the maximum and the kinetic energy is the maximum; at the highest position, the crystallizer speed is zero. According to the law of conservation of energy: 1 / 2mVc=Fh m--mold mass (kg), Vc--pulling speed (m / min), h--amplitude (m), F--mold locking force (N) The crystallizer mass m = 21 tons = 21 * 103 kg, the pulling speed Vc = 5 m / min, the amplitude h = 3 * 10-3 m, substituting into the above formula, we get: F=1 / 2*21*103*(5 / 60)2 / 3*10-3=22400N=22.4KN There are 4 crystallizer locking devices, so the total required locking force is 22.4*4=89.6KN. The locking force F of the original design crystallizer is 70KN<89.6KN, so the locking force is not enough. According to the performance curve of the butterfly spring: when F is 70KN, the compression of the butterfly spring is 12.78mm. According to the linear relationship, it can be calculated that when F is 89.6KN, the compression of the butterfly spring is: 89.6*12.78 / 70=16.358mm. It can be calculated that the compression amount of the butterfly spring needs to be increased by 16.358-12.78=3.578≈3.6mm. Therefore, we increase the thickness of the adjustment pad by 3.6mm to make the locking force meet the requirements and solve this problem.
[0044] When the width and taper of the crystallizer are adjusted, the basic automation system first automatically reduces the setting value of the proportional valve on the wide side from 15.5 MPa to 13.0 MPa at the top and from 17.5 MPa to 15.0 MPa at the bottom. This is an empirical value obtained through multiple tests, which can ensure that the adjustment action of the narrow side during casting will not cause steel leakage. At the same time, the servo motor overcomes the smaller friction between the copper plates and adjusts the position of the narrow copper plate quickly and smoothly. Then, according to the new crystallizer width and taper setting values, the basic automation system compares the actual width and taper values continuously converted from the servo motor resolver signal with the set value, continuously calculates the rotation direction and speed setting value of each servo motor, and transmits it to the corresponding inverter unit through the field bus. Each inverter unit monitors the actual speed converted from the resolver signal according to the rotation direction and speed setting value, optimizes the speed regulation process, quickly and smoothly follows the speed setting value, and accurately positions the actual narrow copper plate. The entire control system is a double closed-loop structure with the servo motor speed control as the inner loop and the narrow copper plate position control as the outer loop. The upper width and left and right tapers of the narrow copper plate are manually set on the HMI screen monitored in the main control room.
[0045] Optimization of adjustment speed: The adjustment speed is proportional to the casting speed of the casting machine. For casting safety considerations, the adjustment speed coefficient in the width increasing direction is smaller than the adjustment speed coefficient in the width decreasing direction. To prevent over-adjustment, when the distance is within 2mm from the set position, the adjustment speed is reduced by the ratio of the relative distance difference to 2mm. Calculated at an average casting speed of 4m / min, the adjustment speed in the width increasing direction is 6mm / min, and the adjustment speed in the width decreasing direction is 10mm / min. At the same time, the lower limit value of the speed is set to 2.5mm / min to prevent the adjustment from being too slow when approaching the end point. When the lower mouth width is in place and only the upper side is adjusted, the adjustment speed is a constant 5mm / min. Optimization of adjustment speed can minimize the length of the slab in the width transition zone.
[0046] (3) During the automatic deviation correction stage of thin slabs, the slab centering adjustment is carried out according to the slab offset detection data of the soaking furnace to ensure that the slab is transported to the seven-stand finishing mill along the rolling center line. The deviation between the slab center line of the two-strand casting machine and the rolling center line is controlled to be ≤8mm, and the deviation of the slab center line of the two-strand casting machine is ≤5mm. The control sequence is to start the automatic deviation correction function at the same time as the vertical roller bites the steel and end before F1 bites the steel. The vertical roller pressure is controlled to be 300~500KN, and the slab running speed before F1 is 0.2~0.5m / s.
[0047] Table 2 Main process parameters of automatic deviation correction of thin slabs in Examples 1 to 6
[0048] Automatic deviation correction can eliminate the difference in the centering of the two-strand casting machine slab, which is beneficial to the fast and smooth transition rolling after the working rolls are replaced in the finishing rolling, and can effectively reduce the transition material.
[0049] (4) In the seven-stand finishing rolling stage, after the working rolls are replaced in the finishing rolling, thick auxiliary steel grades are used for hot roll transition rolling, and then thin pickled steel is directly rolled. This can solve the problem that there is no contract for thick pickled steel, resulting in a large number of hot roll transition materials without corresponding orders, resulting in a high spot rate.
[0050] Example 5: When the width of the auxiliary steel slab is 1250 mm, the width of the pickled steel slab is 1150 mm and the contract thickness is 1.2 mm, the rolling plan within one roll change unit is as follows:
[0051] Example 6: When the width of the auxiliary steel slab is 1500 mm, the width of the pickled steel slab is 1500 mm and the contract thickness is 1.4 mm, the rolling plan within one roll change unit is as follows:
[0052] The working rolls of the finishing rolling F1~4 stands are made of high-speed steel rolls preformed with oxide film. A uniform and dense Fe3O4 oxide film is preformed on the roll surface offline. Under the action of high temperature during the rolling process on the machine, Fe3O4 is further continuously generated. The oxide film has good retention and regeneration properties.
[0053] The oxide film generated on the surface of the roller by the traditional hot roller method has a three-layer structure, with the bottom layer being FeO, the middle layer being Fe3O4, and the surface layer being Fe2O3. The bottom layer FeO has a loose structure and is easy to fall off, so the oxide film generated by the conventional hot roller method is difficult to maintain and regenerate for a long time. Among the three iron oxides, Fe3O4 has high hardness, certain toughness at high temperatures, and high thermal stability. It can withstand high temperature and high pressure, and is not easy to crack and fall off during the rolling process. The present invention prefabricates a uniform and dense Fe3O4 oxide film on the surface of the high-speed steel roller, and further continuously generates Fe3O4 under the action of high temperature during the rolling process on the machine. The oxide film has good retention and regeneration properties.
[0054] (5) During the coiling stage, the pinch roller pressure is controlled in sections. The pinch roller pressure at the head of the strip is controlled to be 50~120KN; when the head of the strip enters the coiler, the roll load is connected and delayed for 10 seconds, the pinch roller light pressure mode is started, and the pinch roller pressure is reduced to 10~20KN; when the finishing rolling F3 steel throwing signal is connected, the pinch roller light pressure mode is released, and the pinch roller pressure is controlled to be 60~144KN.
[0055] Table 3 Process parameters of the segmented control of the pressure of the winding and pinching rollers in Examples 1 to 6
[0056] After the head of the strip enters the coiler, tension is established between the coiler and the finishing mill and enters a steady state. At this time, the function of the coiling pinch roller basically disappears. If the original pinch roller pressure is still maintained, uneven wear of the pinch roller will be caused, which will not only cause defects such as bright strips of the strip, but also affect the service life of the pinch roller. The present invention controls the pressure of the coiling pinch roller in sections, which can avoid the generation of bright strip defects of thin-gauge pickled steel, reduce the wear of the pinch roller by more than 60%, and increase the service life by 2 to 3 times.
[0057] (6) The chemical composition of the pickled steel, measured by mass percentage, includes: C: 0.04-0.07%, Si: 0.02-0.10%, Mn: 0.35-0.85%, P≤0.015%, S≤0.008%, Cr: 0.20-0.40%, Ti: 0.02-0.08%, Nb: 0.02-0.04%, Als: 0.02-0.05%, N≤0.007%, and the balance is Fe and unavoidable impurities.
[0058] (7) The auxiliary steel grade is ordinary C-Mn steel.
[0059] Table 1 Main process parameters of thin slab continuous casting in Examples 1 to 6
[0060] In summary, 1. The present invention develops a rapid width adjustment technology for thin slab continuous casting, and the single adjustment amount of the slab reaches 100mm, and the total width adjustment amount in one casting reaches 500mm. The thin slab continuous casting adopts a cross-casting production mode, and the finishing rolling unit simultaneously adopts thick auxiliary steel grades for hot roller transition rolling. On the premise of ensuring stable production and quality, the flexibility of CSP process production organization and the production efficiency of thin slab continuous casting and rolling are significantly improved. 2. The present invention can eliminate the difference in the centering of the two-strand casting machine slab through automatic deviation correction, which is conducive to the rapid and smooth transition rolling after the finishing rolling replaces the working rolls. And thick auxiliary steel grades are used for hot roller transition rolling, and then thin pickled steel is directly rolled, which can solve the problem that there is no thick specification contract for pickled steel, and a large number of hot roller transition materials are generated without corresponding orders, resulting in a high spot rate. The process cost is reduced by more than 50 yuan / ton, and the spot rate of pickled steel is reduced from 16% to less than 5%. 3. The present invention uses oxide film prefabricated high-speed steel rolls in the F1~4 stands at the front of the finishing rolling, which can effectively prevent the roll system iron scale defects caused by the shedding of the roll oxide film, so as to improve the surface quality of pickled steel, extend the roll replacement cycle, reduce the hot roll transition material, and thus reduce the spot rate of pickled steel. In addition, the oxide film prefabricated high-speed steel rolls can be used cyclically on the machine, significantly reducing roll consumption and relieving the tension of spare rolls.
[0061] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0062] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A method for improving the production efficiency of thin slab continuous casting and rolling, characterized in that: The following steps are involved: Molten steel is smelted according to the requirements of pickled steel and auxiliary steel grades; Cross-casting production of pickled steel and auxiliary steel grades; According to the offset detection data of the cast slab out of the soaking furnace, the slab is adjusted to ensure that the slab is transported to the finishing mill along the rolling center line; In the finishing mill stage, after the working rolls are replaced, thick auxiliary steel grades are used for hot roll transition rolling, and then thin pickled steel is directly rolled.
2. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: When casting pickled steel and auxiliary steel, the casting machine pulling speed is set according to the principle that the thinner the slab thickness, the narrower the slab width, and the lower the superheat of the molten steel, the faster the casting machine pulling speed.
3. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 2, characterized in that: Control the slab thickness at 60~85mm, the slab width at 1050~1550mm, and the casting machine speed at 4.1~5.5m / min.
4. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: When the width of the pickled steel and the auxiliary steel slabs are inconsistent, the crystallizer is quickly adjusted in width for a smooth transition during cross casting. During rapid width adjustment, the casting machine pulling speed is controlled according to the auxiliary steel pulling speed. The rapid width adjustment rate is 40~50mm / s, the single width adjustment amount is ≤100mm, the interval time for each adjustment is t1, the total width adjustment amount in one casting is ≤500mm, and the taper is adjusted synchronously during rapid width adjustment.
5. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: The pickled steel and auxiliary steel grades are cross-casted on the same strand casting machine. Each strand casting machine is equipped with a soaking furnace for heating. The two strand casting machines produce synchronously and are heated in two soaking furnaces respectively.
6. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: During the slab centering adjustment process, the deviation between the slab center line of the two-strand casting machine and the rolling center line is controlled to be ≤8mm, and the deviation of the slab center line of the two-strand casting machine is controlled to be ≤5mm.
7. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: During the slab centering adjustment process, the control sequence is to start the automatic correction function while the vertical roll bites the steel, and end it before the working roll of the frame F1 of the finishing mill bites the steel. The vertical roll pressure is controlled to 300~500KN, and the slab running speed in front of the frame F1 of the finishing mill is 0.2~0.5m / s.
8. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: The chemical composition of the pickled steel, measured by mass percentage, includes: C: 0.04-0.07%, Si: 0.02-0.10%, Mn: 0.35-0.85%, P≤0.015%, S≤0.008%, Cr: 0.20-0.40%, Ti: 0.02-0.08%, Nb: 0.02-0.04%, Als: 0.02-0.05%, N≤0.007%, and the balance is Fe and unavoidable impurities.
9. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: The auxiliary steel grade is ordinary C-Mn steel.
10. The method for improving the production efficiency of thin slab continuous casting and rolling according to claim 1, characterized in that: After the slab passes through the finishing mill, the pinch roll pressure is controlled in sections during the coiling stage; The pinch roller pressure at the strip head is controlled to be 50~120KN; when the strip head enters the coiler, the reel load is connected and delayed for a period of time t2, the pinch roller light pressure mode is started, and the pinch roller pressure is reduced to 10~20KN; when the frame F3 throwing signal of the finishing mill is connected, the pinch roller light pressure mode is released, and the pinch roller pressure is controlled at 60~144KN.
Citation Information
Patent Citations
Casting-rolling combined plant
AT519277A1
Online adjusting method for extensively reducing width of continuous casting mold
CN102240783A
700 MPa grade thin specification hot-rolled automobile structural steel produced adopting short procedure and method
CN109023109A
Slab different steel grade continuous casting method
CN113020558A
Production process of SPCC-MC steel grade for containing TDI chemical barrel cold-rolled sheet
CN117483423A
Cited By
Coiling machine coil locking pressure control method
CN120961634A