Non-oriented silicon steel and its production method

By optimizing the surface morphology and activation treatment of the work rolls on the cold rolling mill end stand, combined with the adjustment of the target crown in finishing rolling and the compensation for roll wear, the problem of uneven thickness of the insulating coating on non-oriented silicon steel was solved, achieving uniform coating and stable adhesion of the insulating coating and improving product performance.

CN123108260APending Publication Date: 2026-11-17JIANGSU SHAGANG STEEL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611628539.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the production process of non-oriented silicon steel, the thickness of the insulating coating is uneven in the width direction of the strip, which leads to unstable product performance and affects the consistency of electromagnetic properties between sheets and the stability of use.

Method used

By controlling the morphology and activation treatment of the work rolls on the cold rolling mill stand, combined with the adjustment of the crown of the finishing mill target and the compensation for roll wear, the coating process of the insulating coating is optimized to ensure the coating thickness and uniformity of distribution.

Benefits of technology

It improves the thickness and adhesion stability of the insulating coating, reduces coating thickness deviation, and enhances the consistency of inter-laminar electromagnetic properties and the stability of use of non-oriented silicon steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This application discloses a non-oriented silicon steel and its production method. The production method includes hot rolling, normalizing, cold rolling, annealing, activation treatment, and coating processes. In the cold rolling process, the surface of the work rolls of the final cold rolling mill meets the following requirements: Rpc value > 200 pieces / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005. In the activation treatment process, the cold-rolled strip steel obtained in the cold rolling process is activated using a treatment solution for 10-30 s. The chemical composition of the treatment solution, by mass percentage, includes: citric acid 4-5%, phosphate buffer 0.1-0.5%, and surface tension adjusting component 0.02-0.1%, and the pH of the treatment solution is 5.7-6.2. In the coating process, an insulating coating is applied to the surface of the strip steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of steel material preparation technology, specifically relating to a non-oriented silicon steel and its production method. Background Technology

[0002] Non-oriented silicon steel is a key material for manufacturing the cores of power equipment such as high-efficiency motors and large generator sets. During the production process of non-oriented silicon steel, an insulating coating is typically applied to its surface to prevent short circuits between the core laminations, which would increase eddy current losses.

[0003] However, the thickness and uniformity of the insulating coating have a crucial impact on product performance. If the coating is too thick, it will lead to deterioration of magnetic properties, while if the coating is too thin, it will reduce the insulation between the core laminations. Poor uniformity of coating thickness distribution in the strip width direction will cause fluctuations in the lamination factor and inconsistent insulation performance between laminations, thereby affecting the consistency of electromagnetic properties between laminations and the stability of use of non-oriented silicon steel products.

[0004] Currently, in actual production processes, there is often a problem of significant deviations in the thickness of the insulating coating in the width direction of the entire strip steel coil, which seriously affects product performance. Summary of the Invention

[0005] The purpose of this application is to provide a non-oriented silicon steel and a method for producing the same.

[0006] To achieve one of the above-mentioned objectives, one embodiment of this application provides a method for producing non-oriented silicon steel, the method comprising hot rolling, normalizing, cold rolling, annealing, activation treatment, and coating processes; In the cold rolling process, the surface of the work rolls on the final stand of the cold rolling mill meets the following requirements: Rpc value > 200 rolls / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005; In the activation process, a treatment solution is used to activate the cold-rolled strip steel obtained in the cold rolling process. The treatment time is 10-30 seconds. The chemical composition of the treatment solution includes, by mass percentage: 4-5% citric acid, 0.1-0.5% phosphate buffer, and 0.02-0.1% surface tension regulating component. The pH of the treatment solution is 5.7-6.2. In the coating process, an insulating coating is applied to the surface of the steel strip.

[0007] As a further improvement of one embodiment of this application, the phosphate buffer is selected from at least one of sodium dihydrogen phosphate and disodium hydrogen phosphate.

[0008] As a further improvement of one embodiment of this application, the surface tension regulating component is selected from nonionic surfactants; The nonionic surfactant is selected from at least one of fatty alcohol polyoxyethylene ether, secondary alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene-polyoxypropylene ether, and ethoxylated acetylenic diol.

[0009] As a further improvement of an embodiment of the present application, the treatment liquid further comprises a pH regulator, and the pH regulator adopts at least one of sodium citrate and disodium hydrogen phosphate.

[0010] As a further improvement of an embodiment of the present application, the chemical components of the coating solution used in the coating process, calculated by solid mass, include: 100 parts by mass of aluminum dihydrogen phosphate and / or magnesium dihydrogen phosphate; 10~40 parts by mass of water-based organic resin; 1~5 parts by mass of polyol; 0.05~0.5 parts by mass of wetting regulator; Wherein, the water-based organic resin is selected from at least one of water-based epoxy resin, acrylic resin and polyester resin, the polyol is selected from at least one of ethylene glycol, propylene glycol and glycerin, and the wetting regulator is selected from at least one of acetylenic diol wetting agents, fatty alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene-polyoxypropylene ether, and polyoxyethylene-polyoxypropylene block copolymer.

[0011] As a further improvement of an embodiment of the present application, in the insulating coating coating process, the steel strip is coated and then cured, the curing temperature is 480~520°C, and the curing time is 120~180s.

[0012] As a further improvement of an embodiment of the present application, in the hot rolling process, the continuous casting slab sequentially undergoes heating, rough rolling and finish rolling to obtain a steel strip; the finish rolling stage includes the following steps: Collect the cross-sectional profile data of the steel strip in real time, and the cross-sectional profile data of the steel strip at least includes the height difference h between the highest point on the surface of the steel strip and the reference point; Compare the height difference h between the highest point on the surface of the steel strip and the reference point with the preset height difference h0; If h<h0, maintain the current target finish rolling crown; If h≥h0, trigger the adjustment of the target finish rolling crown; Wherein, the adjustment of the target finish rolling crown includes: increasing the target finish rolling crown of the subsequent steel strip.

[0013] As a further improvement of an embodiment of the present application, the adjusting by increasing the target finish rolling crown of the subsequent steel strip includes: At the n-th adjustment, control the increment ΔC of the target finish rolling crown n Satisfy: ΔC n =k×(α×h n-1×C n-1 )÷8, where n≥1 and is an integer, k is 0.85~1.15, α=0.1+0.02×(100×Si-0.2), where the element symbol Si represents the mass percentage of Si element in the non-oriented silicon steel, h n-1 C0 represents the height difference between the highest point on the surface of the finished strip and the reference point before the nth adjustment, and C0 represents the target crown of the finished strip before the first adjustment.

[0014] As a further improvement to one embodiment of this application, the finishing rolling stage further includes the following steps: After adjusting the target crown of the finishing mill, it is determined whether the adjusted target crown of the finishing mill reaches the preset upper limit C. max ; If so, then stop the finishing mill and replace the work rolls.

[0015] As a further improvement to one embodiment of this application, the finishing rolling stage further includes the following steps: When the crown of the finishing mill target reaches the preset trigger condition, roll wear compensation is triggered. The roll wear compensation includes: adjusting the roll shifting amount of the finishing work roll to compensate for the strip crown.

[0016] As a further improvement to one embodiment of this application, the preset triggering condition includes: the crown of the precision rolling target reaches a first preset value C. y And h is still ≥ h0, where C y <C max .

[0017] As a further improvement to one embodiment of this application, the method of adjusting the roll shifting amount of the finishing mill work roll to compensate for the strip crown includes: During the finishing rolling of the first strip after triggering roll wear compensation, the amount of roll shifting of the finishing work roll is increased by ΔS1. Determine whether the height difference between the highest point on the surface of the first strip and the reference point exceeds h0; If not, then terminate the roll wear compensation. If so, the amount of roll shifting of the finishing mill work roll is increased by ΔS2; ΔS2>ΔS1.

[0018] As a further improvement to one embodiment of this application, the method of adjusting the roll shifting amount of the finishing mill work roll to compensate for the strip crown also includes: After controlling the increase of the roll shifting amount of the finishing mill work roll by ΔS2, determine whether the height difference between the highest point of the produced strip surface and the reference point exceeds h0. If not, then terminate the roll wear compensation. If so, during subsequent strip finishing rolling, the amount of roll shifting of the finishing work rolls is controlled to increase by ΔS3 / piece of strip until the height difference between the highest point of the strip surface and the reference point is <h0, at which point the roll wear compensation is terminated. Among them, ΔS3 satisfies: ΔS3=ΔS1.

[0019] As a further improvement to one embodiment of this application, the finishing rolling stage further includes the following steps: When the preset conditions are met, stop the finishing mill and replace the finishing mill work rolls; The preset conditions include: the roll shifting allowance of the finishing work roll is less than S0, or the target crown of the finishing roll reaches the preset upper limit C. max Furthermore, the height difference between the highest point on the surface of the strip and the reference point is ≥h0.

[0020] As a further improvement of one embodiment of this application, in the cold rolling process, when cold rolling strips with a height difference h ≥ h0 between the highest point on the strip surface and the reference point, the surface roughness Ra of the cold rolling work rolls is controlled to be ≥ 0.7 μm.

[0021] To achieve one of the above-mentioned objectives, one embodiment of this application provides a non-oriented silicon steel, which is prepared using the non-oriented silicon steel production method described above.

[0022] As a further improvement to one embodiment of this application, referring to GB / T 2522-2017 Test Method for Insulation Resistance and Adhesion of Coating on Electrical Steel Strip (Sheet), the adhesion level between the insulating coating of the non-oriented silicon steel and the steel strip substrate was measured to be Grade A.

[0023] Compared with the prior art, the beneficial effects of this application include: This application discloses a non-oriented silicon steel and its production method. By controlling the morphology of the work rolls on the final stand of the cold rolling mill, the cold-rolled strip can achieve a surface state with moderate roughness and a relatively fine and uniform distribution of microscopic peaks. This provides a more stable substrate surface condition for subsequent annealing, surface activation, and insulating coating application. This is beneficial for increasing the coating thickness of the insulating coating, raising the upper limit of the insulating coating thickness from 1.0 μm to 1.5 μm or even higher, to prevent the coating thickness from being too thin and failing to achieve the insulating effect. It also helps to improve the spreading stability and thickness distribution uniformity of the insulating coating on the strip surface. Combined with the activation treatment of the strip surface before the coating process, the chemical bonding between the components in the insulating coating and the activated strip surface is more stable, thereby improving the adhesion stability of the insulating coating on the strip surface, and further improving the distribution uniformity of the insulating coating. It also helps to increase the coating thickness of the insulating coating, raising the upper limit of the insulating coating thickness from 1.0 μm to 1.5 μm or even higher, to prevent the coating thickness from being too thin and failing to achieve the insulating effect. Detailed Implementation

[0024] Hereinafter, the present application will be described in detail with reference to specific embodiments. However, these embodiments do not limit the present application, and any structural, method, or functional transformations made by those of ordinary skill in the art based on these embodiments shall fall within the protection scope of the present application.

[0025] One embodiment of the present application provides a method for producing non-oriented silicon steel, and non-oriented silicon steel prepared by the production method.

[0026] The method for producing the non-oriented silicon steel includes sequentially performed hot rolling, normalizing, cold rolling, annealing, activation treatment, and coating processes.

[0027] Hereinafter, each process of the method for producing the non-oriented silicon steel will be described in detail.

[0028] (1) Hot rolling process In the hot rolling process, a continuous casting slab sequentially undergoes heating, rough rolling and finish rolling to obtain a steel strip.

[0029] In one embodiment, the finish rolling stage includes the following steps: Collect cross-section profile data of the steel strip in real time, where the cross-section profile data of the steel strip at least includes a height difference h between the highest point on the surface of the steel strip and a reference point; Compare the height difference h between the highest point on the surface of the steel strip and the reference point with a preset height difference h0; If h<h0, maintain the current target finish rolling crown; If h≥h0, trigger the adjustment of the target finish rolling crown; Wherein, the adjustment of the target finish rolling crown includes: increasing the target finish rolling crown of subsequent steel strips.

[0030] Finish rolling is carried out in a finishing mill, and the target finish rolling crown refers to the preset target crown of the finishing mill. By setting the target finish rolling crown, the crown of the steel strip obtained by finish rolling can be controlled.

[0031] By collecting the cross-section profile data of the steel strip in real time during the finish rolling stage and adjusting the target finish rolling crown accordingly, the control of the surface profile of the steel strip can be realized, occasional defects on the surface of the steel strip can be reduced, the influence on the uniformity of the coating during the subsequent application of the insulating coating can be reduced, and the thickness deviation of the insulating coating in the width direction of the steel strip can be decreased, thereby improving the batch stability and use reliability of the finished non-oriented silicon steel product.

[0032] In one embodiment, the thickness of the steel strip obtained from the hot rolling process is 2.30 to 2.50 mm, and the preset height difference h0 between the highest point on the surface of the steel strip and the reference point is 7.5 to 8.5 μm.

[0033] In another embodiment, the thickness of the strip obtained by the hot rolling process is >2.50mm, and the preset height difference h0 between the highest point of the strip surface and the reference point is >8.5μm.

[0034] In another embodiment, the thickness of the strip obtained by the hot rolling process is <2.30mm, and the preset height difference h0 between the highest point on the strip surface and the reference point is <7.5μm.

[0035] Thus, by setting the preset height difference h0 between the highest point on the strip surface and the reference point based on the thickness of the strip obtained from the hot rolling process, it is possible to avoid excessively high local high points on the strip surface.

[0036] The initial target crown of the finishing mill, that is, the initial preset target crown of the finishing mill, is C0, where C0 is 18~20μm.

[0037] In one embodiment, increasing the target crown of the subsequent strip for finishing to make adjustments includes: During the nth adjustment, the increase in the crown of the finishing mill target is controlled by ΔC. n Satisfy: ΔC n =k×(α×h n-1 ×C n-1 )÷8.

[0038] Where n ≥ 1 and is an integer, k is 0.85~1.15, and α = 0.1 + 0.02 × (100 × Si - 0.2), the element symbol Si in the formula represents the mass percentage of Si element in the non-oriented silicon steel. For example, if the mass percentage of Si element in the non-oriented silicon steel is 0.2%, then Si is substituted into the formula for calculating α as 0.2%.

[0039] h n-1 C0 represents the height difference between the highest point of the surface of the finished strip and the reference point before the nth adjustment, and C0 represents the target crown of the finished strip before the first adjustment, which is also the initial target crown of the finished strip.

[0040] Thus, as the Si content in non-oriented silicon steel increases, α also increases linearly, thereby increasing the target crown of the finishing mill by ΔC during the nth adjustment. n Except for the height difference h between the highest point of the surface of the finished strip before the nth adjustment and the reference point. n-1 and the current target convexity C n-1 In addition, it can also differentiate the increase in the target crown of finishing rolling according to different Si content steel grades, thereby avoiding the use of the same target crown adjustment parameters for finishing rolling for different Si content steel grades, which is conducive to improving the adaptability of the target crown adjustment of finishing rolling to non-oriented silicon steel with different Si content.

[0041] In one embodiment, the chemical composition of the non-oriented silicon steel, by mass percentage, includes: Mn 0.20~1.0%, Al 0.20~1.0%, C≤0.003%, P≤0.04%, S≤0.003%, Si 0.2~2.25%, with the remainder being Fe and unavoidable impurities.

[0042] Correspondingly, the value of α ranges from 0.100 to 0.141.

[0043] In one embodiment, the finishing rolling stage further includes the following steps: After adjusting the target crown of the finishing mill, it is determined whether the adjusted target crown of the finishing mill reaches the preset upper limit C. max ; If so, then stop the finishing mill and replace the work rolls.

[0044] The finishing mill includes pairs of work rolls, with each pair of work rolls positioned one above the other. The strip passes between the upper and lower work rolls to achieve rolling.

[0045] Thus, on the one hand, when the target crown of the finishing mill has been increased to the preset upper limit, it indicates that there is no room for further adjustment by simply relying on the target crown adjustment; at this time, replacing the work roll can avoid continuing to roll under the condition of work roll wear, and can also eliminate the continuous occurrence of local high points caused by the continued deterioration of the wear condition of the roll, thereby avoiding the continuous occurrence of surface contour abnormalities such as local high points on the strip surface, thereby improving the stability of the transverse cross-sectional contour of the strip, and providing stable substrate conditions for the uniform coating of the subsequent insulating coating.

[0046] In one embodiment, the thickness of the strip obtained from the hot rolling process is 2.30~2.50 mm, and the preset upper limit C of the target crown in the finishing rolling is... max It is 37~39μm.

[0047] In another embodiment, the thickness of the strip obtained from the hot rolling process is >2.50 mm, and the preset upper limit C of the target crown of the finishing rolling is... max >39μm.

[0048] In another embodiment, the thickness of the strip obtained from the hot rolling process is <2.30 mm, and the preset upper limit C of the target crown of the finishing rolling is... max <37μm.

[0049] Thus, the preset upper limit C of the target crown of the finishing rolling is set according to the thickness of the strip obtained from the hot rolling process. max This can prevent excessively high local high points on the strip surface.

[0050] In one embodiment, the finishing rolling stage further includes the step of: When the crown of the finishing mill target reaches the preset trigger condition, roll wear compensation is triggered. The roll wear compensation includes: adjusting the roll shifting amount of the finishing work roll to compensate for the strip crown.

[0051] Once the target crown of the finishing mill has been increased to a certain extent, further adjustments to the target crown of the finishing mill will result in excessive crown of the hot-rolled plate, which in turn leads to an increase in the difference in transverse thickness distribution at the cold rolling inlet, as well as an increase in the difference between plates after cold rolling, a decrease in the uniformity of the transverse cross section of the substrate, and consequently, a decrease in the distribution stability of the coating solution during coating and an increase in the transverse film thickness deviation of the insulating coating.

[0052] The preset triggering conditions include: the crown of the precision rolling target reaches a first preset value C. y And h is still ≥ h0, where C y <C max .

[0053] Understandably, C y Initial finish rolling target crown C0.

[0054] Thus, by setting C y <C max And the target crown of the finishing mill reaches C y When h is still ≥ h0, roll wear compensation is triggered. This can be triggered before the finishing target crown reaches the preset upper limit, allowing the finishing target crown adjustment and work roll misalignment compensation to form a graded control. While preserving the subsequent finishing target crown adjustment margin, it compensates for local high points caused by roll wear, thereby avoiding the need to rely solely on continuously increasing the finishing target crown for shape control and reducing the premature achievement of C. max The probability of needing to stop and replace the work rolls is reduced, thus extending the lifespan of the work rolls.

[0055] In one embodiment, the thickness of the strip obtained from the hot rolling process is 2.30~2.50 mm, and the first preset value C of the target crown of the finishing rolling is... y The value is 31~33μm.

[0056] In another embodiment, the thickness of the strip obtained from the hot rolling process is >2.50 mm, and the first preset value C of the target crown of the finishing rolling is... y >33μm.

[0057] In another embodiment, the thickness of the strip obtained from the hot rolling process is <2.30 mm, and the first preset value C of the target crown of the finishing rolling is... y <31μm.

[0058] In one embodiment, the method of adjusting the roll shifting amount of the finishing mill work rolls to compensate for the strip crown includes: During the finishing rolling of the first strip after triggering roll wear compensation, the amount of roll shifting of the finishing work roll is increased by ΔS1. Determine whether the height difference between the highest point on the surface of the first strip and the reference point exceeds h0; If not, then terminate the roll wear compensation. If so, the amount of roll shifting of the finishing mill work roll is increased by ΔS2; ΔS2>ΔS1.

[0059] In this way, by using graded compensation, the compensation intensity can be increased when the initial compensation effect is insufficient, without having to use a large amount of roll shifting at the initial stage of roll wear compensation. This balances the roll shifting compensation effect with the roll shifting allowance of the work roll, and reserves adjustment margin for subsequent continuous compensation.

[0060] In one embodiment, ΔS1 is 2 mm and ΔS2 is 3 mm.

[0061] In one embodiment, the method of adjusting the roll shifting amount of the finishing work roll to compensate for the strip crown further includes: After controlling the increase of the roll shifting amount of the finishing mill work roll by ΔS2, determine whether the height difference between the highest point of the produced strip surface and the reference point exceeds h0. If not, then terminate the roll wear compensation. If so, during subsequent strip finishing rolling, the amount of roll shifting of the finishing work rolls is controlled to increase by ΔS3 / piece of strip until the height difference between the highest point on the surface of the strip and the reference point is <h0, at which point the roll wear compensation is terminated.

[0062] In this way, the height difference between the local high point and the reference point on the strip surface can be stably controlled within h0, reducing the generation of strips with abnormal local contours, and providing substrate conditions with more stable transverse contours for subsequent cold rolling and uniform coating of insulating coating.

[0063] Wherein, ΔS3 satisfies: ΔS3=ΔS1. Thus, ΔS3<ΔS2, after initially using a small amount of roll shifting ΔS1 for roll wear compensation, a larger amount of roll shifting ΔS2 can be used for enhanced compensation, and then a small amount of roll shifting ΔS3 can be used for continuous roll wear compensation.

[0064] In one embodiment, ΔS1 is 2mm, ΔS2 is 3mm, and ΔS3 is 2mm.

[0065] In one embodiment, the finishing rolling stage further includes the step of: When the preset conditions are met, stop the finishing mill and replace the finishing mill work rolls; The preset conditions include: the roll shifting allowance of the finishing work roll is less than S0, or the target crown of the finishing roll reaches the preset upper limit C. max Furthermore, the height difference between the highest point on the surface of the strip and the reference point is ≥h0.

[0066] This can prevent excessive roll slippage that could lead to work roll failure, or prevent excessively high local peaks on the strip surface.

[0067] In one embodiment, the length of the finishing work roll is 1450 mm, and S0 is 5 mm.

[0068] In one embodiment, the uniform heating temperature is 1080~1150℃, the heating time is ≥180min; the finishing temperature of rough rolling is 880~950℃, the finishing temperature of finish rolling is 830~895℃, and the coiling temperature is 610~680℃.

[0069] (2) Normalizing process In one embodiment, the normalization temperature is 840~950°C and the normalization time is 180~200s.

[0070] (3) Cold rolling process The strip steel after the normalizing process is cold-rolled using a cold rolling mill. Specifically, a five-stand cold rolling mill can be used, with each stand having six work rolls arranged in pairs, one above the other. The five-stand cold rolling mill consists of stands S1 to S5 arranged sequentially.

[0071] The surface of the work rolls of the cold rolling mill stand, i.e., the S5 stand, is controlled to meet the following requirements: Rpc value > 200 rolls / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005.

[0072] Thus, by controlling the morphology of the work rolls on the final stand of the cold rolling mill, the cold-rolled strip can obtain a surface state with moderate roughness and a relatively fine and uniform distribution of microscopic peaks. This provides a more stable substrate surface condition for subsequent annealing, surface activation, and insulating coating, which is beneficial to increasing the coating thickness of the insulating coating. The upper limit of the insulating coating thickness can be increased from 1.0μm to 1.5μm or even higher, so as to avoid the coating thickness being too thin and failing to achieve the insulating effect. It is also beneficial to improve the spreading stability and thickness distribution uniformity of the insulating coating on the strip surface.

[0073] In one embodiment, when cold rolling a strip with a height difference h ≥ h0 between the highest point on the strip surface and the reference point, the surface roughness Ra of the cold rolling work roll is controlled to be ≥ 0.7 μm.

[0074] Under the condition of a high surface roughness of Ra≥0.7μm, the cold rolling work roll has a better surface condition. Combined with the reduction deformation during the cold rolling process, it can further homogenize the local contour anomalies on the strip surface formed by the previous hot rolling process, reduce the influence of local high points on the surface condition of the cold-rolled strip, thereby improving the uniformity of the surface contour and surface condition of the cold-rolled strip, and providing stable substrate conditions for subsequent annealing and uniform coating of insulating coating.

[0075] In practical applications, the work rolls have a high and relatively stable surface roughness in the early stage of use after replacement, Ra≥0.7μm. By arranging the strip with a height difference h≥h0 between the highest point of the strip surface and the reference point in the early stage of use after the work rolls are replaced for cold rolling, cold rolling can be carried out under the condition that the surface roughness Ra≥0.7μm of the cold rolling work rolls can be achieved.

[0076] In one embodiment, the total reduction rate of the cold rolling process is 80-85%.

[0077] In one embodiment, the work rolls of the S1 and S2 frames are rolls with edge roll profiles. Specifically, the edge roll profile chamfer of the work roll of the S1 frame is 90 μm, and the chamfer insertion is 150 mm; the edge roll profile chamfer of the work roll of the S2 frame is 70 μm, and the chamfer insertion is 170 mm.

[0078] By setting different chamfering and chamfering insertion amounts on the edge rolls of the S1 and S2 stands in the front section of the cold rolling mill, the transverse cross-section of the strip entering the cold rolling mill is gradually adjusted by utilizing the mechanical control effect of the work roll shape on the rolling deformation in the width direction of the strip. Specifically, the S1 stand uses a larger chamfering amount to initially adjust the rolling state of the strip edge, while the S2 stand uses a smaller chamfering amount and a larger chamfering insertion amount to further adjust the edge-affected area. This allows the transverse cross-sectional differences formed in the previous processes to be gradually balanced in the front section of the cold rolling mill, improving the thickness distribution between the edge and middle of the strip.

[0079] Thus, by adjusting the contours of the strip's edges and center using stands S1 and S2, the uniformity of the strip's transverse cross-sectional contour is improved; furthermore, by controlling the microscopic surface morphology of the strip using stand S5, stable substrate surface conditions can be provided for subsequent annealing, surface activation, and insulating coating application, thereby improving the spreading stability and thickness distribution uniformity of the insulating coating on the strip surface.

[0080] (4) Annealing process In one embodiment, the annealing temperature is 880~950℃ and the annealing time is 180~300s.

[0081] In one embodiment, the dew point during the annealing process is -30 to -20°C. The protective atmosphere is a mixture of H2 and N2, wherein the volume percentage of H2 is ≥50%; or, the protective atmosphere is pure N2.

[0082] (5) Activation treatment process The cold-rolled strip steel obtained from the cold rolling process is activated using a treatment solution for 10-30 seconds. The chemical composition of the treatment solution, by mass percentage, includes: 4-5% citric acid, 0.1-0.5% phosphate buffer, and 0.02-0.1% surface tension adjusting component. The pH of the treatment solution is 5.7-6.2.

[0083] Thus, by activating the surface of the strip steel, the chemical bond between the components in the insulating coating and the activated surface of the strip steel becomes more stable, thereby improving the adhesion stability of the insulating coating on the surface of the strip steel, and further improving the uniformity of the distribution of the insulating coating. It also helps to increase the coating thickness of the insulating coating, raising the upper limit of the insulating coating thickness from 1.0μm to 1.5μm or even higher, so as to avoid the coating thickness being too thin and failing to achieve the insulation effect.

[0084] In one embodiment, the phosphate buffer is selected from at least one of sodium dihydrogen phosphate and disodium hydrogen phosphate.

[0085] In one embodiment, the surface tension regulating component is selected from nonionic surfactants.

[0086] Nonionic surfactants possess excellent wetting properties and do not introduce additional charged hydrophilic groups found in ionic surfactants. Through the synergistic effect of surface tension regulating components with citric acid and phosphate buffer, the activation treatment solution can achieve more uniform contact with the steel strip substrate surface, providing a stable surface condition for the subsequent uniform coating of the insulating layer.

[0087] The nonionic surfactant is selected from at least one of fatty alcohol polyoxyethylene ether, secondary alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene-polyoxypropylene ether, and ethoxylated acetylenic diol.

[0088] In one embodiment, the treatment solution further includes a pH adjuster, wherein the pH adjuster is at least one selected from sodium citrate and disodium hydrogen phosphate. The pH adjuster can be used to adjust the pH of the treatment solution to 5.7-6.2.

[0089] (6) Coating process An insulating coating is applied to the surface of the strip steel after the activation process.

[0090] In one embodiment, the surface of the strip is coated with an insulating coating and then cured at a curing temperature of 480~520°C for 120~180 seconds.

[0091] By synergistically controlling the curing temperature and curing time, the insulating coating can be fully sintered and cured to form a stable coating structure, thereby obtaining good surface quality, protective performance and insulation performance.

[0092] If the curing temperature is too low or the curing time is insufficient, the coating will not be fully cured and will easily absorb moisture, leading to a decrease in the protective performance of the coating surface. If the curing temperature is too high or the curing time is too long, the steel strip surface may turn yellow and the insulation performance of the coating may be affected.

[0093] In one embodiment, the chemical composition of the coating solution used in the coating process, based on solid mass, includes: 100 parts by weight of aluminum dihydrogen phosphate and / or magnesium dihydrogen phosphate; 10-40 parts by weight of water-based organic resin; 1-5 parts by weight of polyol; Wetting regulator 0.05~0.5 parts by weight; The waterborne organic resin is selected from at least one of waterborne epoxy resin, acrylic resin and polyester resin; the polyol is selected from at least one of ethylene glycol, propylene glycol and glycerin; and the wetting regulator is selected from at least one of acetylenic diol wetting agents, fatty alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene-polyoxypropylene ether, and polyoxyethylene-polyoxypropylene block copolymer.

[0094] Thus, the insulating coating on the strip surface after the coating process contains metal phosphate components but no Cr. The chemical bond between the metal phosphate components in the insulating coating and the activated strip surface is more stable, thereby improving the adhesion stability of the insulating coating on the strip surface, which in turn improves the uniformity of the insulating coating distribution and also helps to increase the coating thickness.

[0095] This application also provides a non-oriented silicon steel according to one embodiment. This non-oriented silicon steel is prepared using the production method described above.

[0096] The thickness of the non-oriented silicon steel strip substrate is 0.35~0.50mm, and the thickness of the insulating coating attached to the surface of the strip substrate is 0.8~1.5μm.

[0097] If the insulating coating is too thin, it will not achieve the desired insulation effect; if the insulating coating is too thick, it will easily lead to insufficient adhesion of the coating and a small stacking factor, resulting in an increase in the proportion of non-magnetic coating and a decrease in magnetic properties.

[0098] The lateral coating uniformity of the insulating coating was detected using X-ray fluorescence spectrometry (XRF). Details are as follows: n detection points are set along the width of the strip, and the phosphorus content (Pi) per unit area in the insulating coating at each detection point is measured, with units of g / m². 2 Calculate the average value of P element per unit area at each test point. The maximum relative deviation of P element per unit area at each test point from the average value characterizes the lateral coating uniformity of the insulating coating.

[0099] Since the coating solution used in the coating process is aluminum dihydrogen phosphate and / or magnesium dihydrogen phosphate, that is, a phosphate-containing insulating coating system is used, the element P is used as a characteristic element of the insulating coating. The lateral distribution of its unit area content can characterize the relative coating amount distribution of the insulating coating in the strip width direction. The relative deviation of the unit area content of the element P relative to the average value characterizes the lateral thickness deviation of the insulating coating.

[0100] Testing revealed that the transverse thickness deviation of the insulating coating on the non-oriented silicon steel was within the range of 8.0% to 9.8%, indicating excellent uniformity of the insulating coating in the width direction of the strip and excellent consistency of the inter-sheet electromagnetic properties of the non-oriented silicon steel products.

[0101] Referring to GB / T 2522-2017 Test Method for Insulation Resistance and Adhesion of Coating on Electrical Steel Strip (Sheet), the adhesion level between the insulating coating of the non-oriented silicon steel and the steel strip substrate was measured to be Grade A.

[0102] Referring to GB / T 3655-2022, the method for measuring the magnetic properties of electrical steel strips (sheets) using Epstein squares was used to measure the iron loss P of non-oriented silicon steel. 1.5 / 50 ≤3.2W / kg, magnetic induction B 50 ≥1.68T.

[0103] The detailed descriptions listed above are merely specific descriptions of feasible implementation methods of this application, and are not intended to limit the scope of protection of this application. All equivalent implementation methods or modifications made without departing from the spirit of the art of this application should be included within the scope of protection of this application.

[0104] The beneficial effects of this application are further illustrated below through specific embodiments 1-3 and comparative example 1. All three embodiments use the production method of non-oriented silicon steel according to this application to prepare non-oriented silicon steel. Of course, these three embodiments are only a part of the numerous variations contained in this application, and not all of them.

[0105] Example 1 The chemical composition of the non-oriented silicon steel in this embodiment, by mass percentage, includes: Mn 0.50%, Al 0.50%, C 0.0025%, P 0.02%, S 0.002%, Si 1.50%, with the remainder being Fe and unavoidable impurities.

[0106] The production method of this non-oriented silicon steel includes the following steps.

[0107] (1) Hot rolling process The continuous casting slab sequentially undergoes heating, rough rolling and finish rolling to obtain a steel strip with a thickness of 2.30 mm. The soaking temperature during heating is 1120°C, and the heating time is 200 min; the finishing temperature of rough rolling is 920°C, the finishing temperature of finish rolling is 860°C, and the coiling temperature is 650°C. The finish rolling is performed on a finishing mill.

[0108] The finish rolling stage includes the following steps: Collect cross-sectional profile data of the steel strip in real time, wherein the cross-sectional profile data of the steel strip at least includes the height difference h between the highest point on the steel strip surface and a reference point; Compare the height difference h between the highest point on the steel strip surface and the reference point with a preset height difference h0; If h<h0, maintain the current target finish rolling crown; If h≥h0, trigger the adjustment of the target finish rolling crown; Wherein, the adjustment of the target finish rolling crown comprises: increasing the target finish rolling crown of the subsequent steel strip.

[0109] Specifically, increasing the target finish rolling crown of the subsequent steel strip for adjustment comprises: During the n-th adjustment, controlling the increment ΔC of the target finish rolling crown n satisfies: ΔC n =k×(α×h n-1 ×C n-1 )÷8.

[0110] Wherein, n≥1 and is an integer, k=1, α=0.126.

[0111] In this embodiment, the preset height difference h0 between the highest point on the steel strip surface and the reference point is 8 μm. The initial target finish rolling crown C0 is 18 μm.

[0112] In this embodiment, the finish rolling stage further comprises the following step: After the adjustment of the target finish rolling crown, judge whether the adjusted target finish rolling crown reaches the preset upper limit C max ; If yes, control the finishing mill to shut down and replace the work rolls.

[0113] In this embodiment, the preset upper limit C of the target finish rolling crown max is 38 μm.

[0114] In this embodiment, the finish rolling stage further comprises the step: When the target finish rolling crown meets a preset trigger condition, trigger roll wear compensation; Wherein, the roll wear compensation comprises: adjusting the roll shifting amount of the finish rolling work rolls to compensate the steel strip crown.

[0115] The preset triggering conditions include: the crown of the precision rolling target reaches a first preset value C. y And h is still ≥ h0, where C y It is 32μm.

[0116] The method of adjusting the roll shifting amount of the finishing mill work rolls to compensate for the strip crown includes: During the finishing rolling of the first strip after triggering roll wear compensation, the amount of roll shifting of the finishing work roll is increased by ΔS1. Determine whether the height difference between the highest point on the surface of the first strip and the reference point exceeds h0; If not, then terminate the roll wear compensation. If so, the amount of roll shifting of the finishing mill work roll is increased by ΔS2; After controlling the increase of the roll shifting amount of the finishing mill work roll by ΔS2, determine whether the height difference between the highest point of the produced strip surface and the reference point exceeds h0. If not, then terminate the roll wear compensation. If so, during subsequent strip finishing rolling, the amount of roll shifting of the finishing work rolls is controlled to increase by ΔS3 / piece of strip until the height difference between the highest point on the surface of the strip and the reference point is <h0, at which point the roll wear compensation is terminated.

[0117] Wherein, ΔS1 is 2mm, ΔS2 is 3mm, and ΔS3 is 2mm.

[0118] The finishing rolling stage also includes the following steps: When the preset conditions are met, stop the finishing mill and replace the finishing mill work rolls; The preset conditions include: the roll shifting allowance of the finishing work roll is less than S0, or the target crown of the finishing roll reaches the preset upper limit C. max Furthermore, the height difference between the highest point on the surface of the strip and the reference point is ≥h0.

[0119] Where S0 is 5mm.

[0120] (2) Normalizing process The normalization temperature is 860℃ and the normalization time is 190s.

[0121] (3) Cold rolling process A five-stand cold rolling mill is used to cold roll the strip after the normalizing process. Each stand has six work rolls, which are arranged in pairs, one above the other. The five-stand cold rolling mill consists of stands S1 to S5 arranged sequentially.

[0122] When cold rolling strips with a height difference h ≥ h0 between the highest point on the strip surface and the reference point, the surface roughness Ra of the cold rolling work rolls should be controlled to be ≥ 0.7 μm.

[0123] The surface of the work rolls of the cold rolling mill stand, i.e., the S5 stand, meets the following requirements: Rpc value > 200 rolls / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005.

[0124] The total reduction rate of the cold rolling process is 80%. The work rolls of the S1 and S2 stands are rolls with edge roll profiles. The edge roll profile chamfer of the work rolls of the S1 stand is 90μm, and the chamfer insertion is 150mm; the edge roll profile chamfer of the work rolls of the S2 stand is 70μm, and the chamfer insertion is 170mm.

[0125] (4) Annealing process The annealing temperature is 880℃, and the annealing time is 300s. The dew point is -20℃. The protective atmosphere is pure N2.

[0126] (5) Activation treatment process The cold-rolled strip steel obtained from the cold rolling process was activated using a treatment solution for 20 seconds. The chemical composition of the treatment solution, by mass percentage, included: 4.5% citric acid, 0.3% sodium dihydrogen phosphate, 0.05% fatty alcohol polyoxyethylene ether, and the remainder being water. Sodium citrate was used to adjust the pH of the treatment solution to 6.0.

[0127] (6) Coating process After the activation process, an insulating coating is applied to the surface of the strip steel and then cured at a temperature of 500℃ for 150 seconds.

[0128] The chemical composition of the coating solution used in the coating process, by solid mass, includes: 100 parts by mass of aluminum dihydrogen phosphate, 25 parts by mass of waterborne epoxy resin, 3 parts by mass of propylene glycol, and 0.2 parts by mass of ethoxylated acetylenol.

[0129] The thickness of the non-oriented silicon steel strip substrate is 0.35 mm, and the thickness of the insulating coating attached to the surface of the strip substrate is 1.1 μm.

[0130] X-ray fluorescence spectrometry (XRF) was used to detect the transverse coating uniformity of the insulating coating. In this embodiment, the transverse thickness deviation of the insulating coating for each strip within the same production batch was within the range of 8.0% to 9.5%, and the difference in transverse thickness deviation between strips was small. This indicates excellent uniformity of the insulating coating in the width direction of the strip, excellent consistency of the inter-sheet electromagnetic properties of the non-oriented silicon steel product, and good consistency of the transverse thickness deviation of the insulating coating for each strip within the same production batch.

[0131] Referring to GB / T 2522-2017 Test Method for Insulation Resistance and Adhesion of Coating on Electrical Steel Strip (Sheet), the adhesion level between the insulating coating of the non-oriented silicon steel and the steel strip substrate was measured to be Grade A.

[0132] Referring to GB / T 3655-2022, the method for measuring the magnetic properties of electrical steel strips (sheets) using Epstein squares was used to measure the iron loss P of non-oriented silicon steel. 1.5 / 50 ≤3.2W / kg, magnetic induction B 50 ≥1.68T.

[0133] Example 2 The chemical composition of the non-oriented silicon steel in this embodiment, by mass percentage, includes: Mn 0.50%, Al 0.50%, C 0.0025%, P 0.02%, S 0.002%, Si 1.50%, with the remainder being Fe and unavoidable impurities.

[0134] The production method of this non-oriented silicon steel includes the following steps.

[0135] (1) Hot rolling process The continuously cast billet undergoes heating, rough rolling, and finish rolling in sequence to obtain a strip steel with a thickness of 2.30 mm. The soaking temperature during heating is 1090℃, and the heating time is 190 min. The finishing temperature of rough rolling is 890℃, the finishing temperature is 840℃, and the coiling temperature is 620℃. Finish rolling is performed on a finishing mill.

[0136] (2) Normalizing process The normalization temperature is 850℃ and the normalization time is 185s.

[0137] (3) Cold rolling process A five-stand cold rolling mill is used to cold roll the strip after the normalizing process. Each stand has six work rolls, which are arranged in pairs, one above the other. The five-stand cold rolling mill consists of stands S1 to S5 arranged sequentially.

[0138] When cold rolling strips with a height difference h ≥ h0 between the highest point on the strip surface and the reference point, the surface roughness Ra of the cold rolling work rolls should be controlled to be ≥ 0.7 μm.

[0139] The surface of the work rolls of the cold rolling mill stand, i.e., the S5 stand, meets the following requirements: Rpc value > 200 rolls / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005.

[0140] The total reduction rate of the cold rolling process is 82%. The work rolls of the S1 and S2 stands are rolls with edge roll profiles. The edge roll profile chamfer of the work rolls of the S1 stand is 90μm, and the chamfer insertion is 150mm; the edge roll profile chamfer of the work rolls of the S2 stand is 70μm, and the chamfer insertion is 170mm.

[0141] (4) Annealing process The annealing temperature is 890℃, and the annealing time is 200s. The dew point is -28℃. The protective atmosphere is a mixture of H2 and N2, with H2 comprising 50% by volume.

[0142] (5) Activation treatment process The cold-rolled strip steel obtained from the cold rolling process was activated using a treatment solution for 10 seconds. The chemical composition of the treatment solution, by mass percentage, included: 4.5% citric acid, 0.4% sodium dihydrogen phosphate, 0.05% fatty alcohol polyoxyethylene-polyoxypropylene ether, and the remainder being water. Sodium citrate was used to adjust the pH of the treatment solution to 5.7.

[0143] (6) Coating process After the activation process, an insulating coating is applied to the surface of the strip steel, which is then cured at a temperature of 480℃ for 120 seconds.

[0144] The chemical composition of the coating solution used in the coating process, by solid mass, includes: 100 parts by mass of magnesium dihydrogen phosphate, 35 parts by mass of acrylic resin, 5 parts by mass of ethylene glycol, and 0.4 parts by mass of fatty alcohol polyoxyethylene-polyoxypropylene ether.

[0145] The thickness of the non-oriented silicon steel strip substrate is 0.35 mm, and the thickness of the insulating coating attached to the surface of the strip substrate is 1.1 μm.

[0146] X-ray fluorescence spectrometry (XRF) was used to detect the transverse coating uniformity of the insulating coating. In this example, the transverse thickness deviation of the insulating coating for each strip within the same production batch was within the range of 8.0% to 9.8%, and the difference in transverse thickness deviation between strips was small. This indicates excellent uniformity of the insulating coating in the width direction of the strip, excellent consistency of the inter-sheet electromagnetic properties of the non-oriented silicon steel product, and good consistency of the transverse thickness deviation of the insulating coating for each strip within the same production batch.

[0147] Referring to GB / T 2522-2017 Test Method for Insulation Resistance and Adhesion of Coating on Electrical Steel Strip (Sheet), the adhesion level between the insulating coating of the non-oriented silicon steel and the steel strip substrate was measured to be Grade A.

[0148] Referring to GB / T 3655-2022, the method for measuring the magnetic properties of electrical steel strips (sheets) using Epstein squares was used to measure the iron loss P of non-oriented silicon steel. 1.5 / 50 ≤3.2W / kg, magnetic induction B 50 ≥1.68T.

[0149] Example 3 The chemical composition of the non-oriented silicon steel in this embodiment, by mass percentage, includes: Mn 0.80%, Al 0.30%, C 0.0023%, P 0.02%, S 0.002%, Si 2.0%, with the remainder being Fe and unavoidable impurities.

[0150] The production method of this non-oriented silicon steel includes the following steps.

[0151] (1) Hot rolling process The continuously cast billet undergoes heating, rough rolling, and finish rolling in sequence to obtain a strip steel with a thickness of 2.30 mm. The soaking temperature during heating is 1140℃, and the heating time is 210 min. The finishing temperature of rough rolling is 940℃, the finishing temperature is 885℃, and the coiling temperature is 670℃. Finish rolling is performed on a finishing mill.

[0152] (2) Normalizing process The normalization temperature was 930℃ and the normalization time was 195s.

[0153] (3) Cold rolling process A five-stand cold rolling mill is used to cold roll the strip after the normalizing process. Each stand has six work rolls, which are arranged in pairs, one above the other. The five-stand cold rolling mill consists of stands S1 to S5 arranged sequentially.

[0154] When cold rolling strips with a height difference h ≥ h0 between the highest point on the strip surface and the reference point, the surface roughness Ra of the cold rolling work rolls should be controlled to be ≥ 0.7 μm.

[0155] The surface of the work rolls of the cold rolling mill stand, i.e., the S5 stand, meets the following requirements: Rpc value > 200 rolls / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005.

[0156] The total reduction rate of the cold rolling process is 85%. The work rolls of the S1 and S2 stands are rolls with edge roll profiles. The edge roll profile chamfer of the work rolls of the S1 stand is 90μm, and the chamfer insertion is 150mm; the edge roll profile chamfer of the work rolls of the S2 stand is 70μm, and the chamfer insertion is 170mm.

[0157] (4) Annealing process The annealing temperature was 940℃, and the annealing time was 280s. The dew point was -22℃. The protective atmosphere was a mixture of H2 and N2, with H2 comprising 70% by volume.

[0158] (5) Activation treatment process The cold-rolled strip steel obtained from the cold rolling process was activated using a treatment solution for 30 seconds. The chemical composition of the treatment solution, by mass percentage, included: 4.0% citric acid, 0.3% disodium hydrogen phosphate, 0.06% ethoxylated acetylenic diol, and the remainder being water. Sodium citrate was used to adjust the pH of the treatment solution to 6.2.

[0159] (6) Coating process After the activation process, an insulating coating is applied to the surface of the strip steel and then cured at a temperature of 520℃ for 180 seconds.

[0160] The chemical composition of the coating solution used in the coating process, by solid mass, includes: 100 parts by mass of aluminum dihydrogen phosphate, 40 parts by mass of waterborne epoxy resin, 4 parts by mass of propylene glycol, and 0.3 parts by mass of ethoxylated acetylenol.

[0161] The thickness of the non-oriented silicon steel strip substrate is 0.35 mm, and the thickness of the insulating coating attached to the surface of the strip substrate is 1.1 μm.

[0162] X-ray fluorescence spectrometry (XRF) was used to detect the transverse coating uniformity of the insulating coating. In this example, the transverse thickness deviation of the insulating coating for each strip within the same production batch was within the range of 8.0% to 9.8%, and the difference in transverse thickness deviation between strips was small. This indicates excellent uniformity of the insulating coating in the width direction of the strip, excellent consistency of the inter-sheet electromagnetic properties of the non-oriented silicon steel product, and good consistency of the transverse thickness deviation of the insulating coating for each strip within the same production batch.

[0163] Referring to GB / T 2522-2017 Test Method for Insulation Resistance and Adhesion of Coating on Electrical Steel Strip (Sheet), the adhesion level between the insulating coating of the non-oriented silicon steel and the steel strip substrate was measured to be Grade A.

[0164] Referring to GB / T 3655-2022, the method for measuring the magnetic properties of electrical steel strips (sheets) using Epstein squares was used to measure the iron loss P of non-oriented silicon steel. 1.5 / 50 ≤3.2W / kg, magnetic induction B 50 ≥1.68T.

[0165] Comparative Example 1 The chemical composition of the non-oriented silicon steel in this comparative example, by mass percentage, includes: Mn 0.50%, Al 0.50%, C 0.0025%, P 0.02%, S 0.002%, Si 1.50%, with the remainder being Fe and unavoidable impurities.

[0166] The production method of this non-oriented silicon steel includes the following steps.

[0167] (1) Hot rolling process The continuously cast billet undergoes heating, rough rolling, and finish rolling in sequence to obtain a strip steel with a thickness of 2.30 mm. The soaking temperature during heating is 1120℃, and the heating time is 200 min. The finishing temperature of rough rolling is 920℃, the finishing temperature is 860℃, and the coiling temperature is 650℃. Finish rolling is performed on a finishing mill.

[0168] (2) Normalizing process The normalization temperature is 860℃ and the normalization time is 190s.

[0169] (3) Cold rolling process A five-stand cold rolling mill is used to cold roll the strip after the normalizing process. Each stand has six work rolls, which are arranged in pairs, one above the other. The five-stand cold rolling mill consists of stands S1 to S5 arranged sequentially.

[0170] The surface of the work rolls of the cold rolling mill stand, i.e., the S5 stand, meets the following requirements: Rpc value > 200 rolls / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005.

[0171] The total reduction rate of the cold rolling process is 80%. The work rolls of the S1 and S2 stands are rolls with edge roll profiles. The edge roll profile chamfer of the work rolls of the S1 stand is 90μm, and the chamfer insertion is 150mm; the edge roll profile chamfer of the work rolls of the S2 stand is 70μm, and the chamfer insertion is 170mm.

[0172] (4) Annealing process The annealing temperature is 880℃, and the annealing time is 300s. The dew point is -20℃. The protective atmosphere is pure N2.

[0173] (5) Coating process After applying an insulating coating to the surface of the steel strip, it is cured at a temperature of 500℃ for 150 seconds.

[0174] The chemical composition of the coating solution used in the coating process, by solid mass, includes: 100 parts by mass of aluminum dihydrogen phosphate, 25 parts by mass of waterborne epoxy resin, 3 parts by mass of propylene glycol, and 0.2 parts by mass of ethoxylated acetylenol.

[0175] The thickness of the resulting non-oriented silicon steel strip substrate is 0.50 mm, and the thickness of the insulating coating attached to the surface of the strip substrate is 0.8 μm.

[0176] The transverse coating uniformity of the insulating coating was tested using X-ray fluorescence spectrometry (XRF). The results showed that in this comparative example, the transverse thickness deviation of the insulating coating in each strip within the same production batch exceeded 10%, and the differences in transverse thickness deviation between strips were significant. In other words, compared to the example, the transverse thickness deviation of the insulating coating in this comparative example of non-oriented silicon steel is large, resulting in poor consistency in the inter-sheet electromagnetic properties of the non-oriented silicon steel products.

[0177] Referring to GB / T 2522-2017 Test Method for Insulation Resistance and Adhesion of Coating on Electrical Steel Strips (Sheets), the adhesion level between the insulation coating and the steel substrate of each strip in the same production batch was found to be Class A for some and Class B for others.

[0178] Referring to GB / T 3655-2022, the method for measuring the magnetic properties of electrical steel strips (sheets) using Epstein squares was used to measure the iron loss P of non-oriented silicon steel. 1.5 / 50 ≤3.2W / kg, magnetic induction B 50 ≥1.68T.

[0179] It should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This way of describing the specification is only for clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A method for producing non-oriented silicon steel, characterized in that, The production method includes the procedures of hot rolling, normalizing, cold rolling, annealing, activation treatment, and coating; In the cold rolling procedure, the surface of the work roll of the last stand in cold rolling satisfies: Rpc value > 200 pcs / cm, 0.4 < Ra < 1.0 μm, 0.0002 < Ra / Rpc < 0.005; In the activation treatment procedure, the cold-rolled strip obtained from the cold rolling procedure is subjected to activation treatment using a treatment solution, with a treatment time of 10 to 30 s. The chemical components of the treatment solution, in mass percentage, include: 4 to 5% of citric acid, 0.1 to 0.5% of phosphate buffer, and 0.02 to 0.1% of surface tension regulating component, and the pH of the treatment solution is 5.7 to 6.2; In the coating procedure, an insulating coating is applied to the surface of the strip.

2. The method for producing non-oriented silicon steel according to claim 1, characterized in that, The phosphate buffer is selected from at least one of sodium dihydrogen phosphate and disodium hydrogen phosphate.

3. The method for producing non-oriented silicon steel according to claim 1, characterized in that, The surface tension regulating component is selected from non-ionic surfactants; The non-ionic surfactant is selected from at least one of fatty alcohol polyoxyethylene ether, secondary alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene-polyoxypropylene ether, and ethoxylated acetylenic diol.

4. The method for producing non-oriented silicon steel according to claim 1, characterized in that, The treatment solution further includes a pH regulator, which is at least one of sodium citrate and disodium hydrogen phosphate.

5. The method for producing non-oriented silicon steel according to claim 1, characterized in that, The chemical components of the coating solution used in the coating procedure, based on the solid mass, include: 100 parts by mass of aluminum dihydrogen phosphate and / or magnesium dihydrogen phosphate; 10 to 40 parts by mass of water-based organic resin; 1 to 5 parts by mass of polyol; 0.05 to 0.5 parts by mass of wetting regulator; Wherein, the water-based organic resin is selected from at least one of water-based epoxy resin, acrylic resin and polyester resin, the polyol is selected from at least one of ethylene glycol, propylene glycol and glycerol, and the wetting regulator is selected from at least one of acetylenic diol-based wetting agents, fatty alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene-polyoxypropylene ether, and polyoxyethylene-polyoxypropylene block copolymer.

6. The method for producing non-oriented silicon steel according to claim 1, characterized in that, In the insulating coating application procedure, the strip is cured after coating, with a curing temperature of 480 to 520°C and a curing time of 120 to 180 s.

7. The method for producing non-oriented silicon steel according to claim 1, characterized in that, In the hot rolling procedure, the continuous casting slab sequentially undergoes heating, rough rolling and finish rolling to obtain a strip; the finish rolling stage includes the following steps: Collect cross-sectional profile data of the strip in real time, wherein the cross-sectional profile data of the strip at least includes the height difference h between the highest point on the strip surface and the reference point; Compare the height difference h between the highest point on the strip surface and the reference point with the preset height difference h0; If h < h0, maintain the current target finish rolling crown; If h ≥ h0, trigger the adjustment of the target finish rolling crown; Wherein, the adjustment of the target finish rolling crown includes: increasing the target finish rolling crown of subsequent strips.

8. The method for producing non-oriented silicon steel according to claim 7, characterized in that, The adjustment by increasing the target finish rolling crown of subsequent strips includes: During the nth adjustment, the increase in the crown of the finishing mill target is controlled by ΔC. n Satisfy: ΔC n =k×(α×h n-1 ×C n-1 )÷8, where n≥1 and is an integer, k is 0.85~1.15, α=0.1+0.02×(100×Si-0.2), where the element symbol Si represents the mass percentage of Si element in the non-oriented silicon steel, h n-1 C0 represents the height difference between the highest point on the surface of the finished strip and the reference point before the nth adjustment, and C0 represents the target crown of the finished strip before the first adjustment.

9. The method for producing non-oriented silicon steel according to claim 7, characterized in that, The finish rolling stage further includes the following steps: After adjusting the target crown of the finishing mill, it is determined whether the adjusted target crown of the finishing mill reaches the preset upper limit C. max ; If yes, control the finish rolling mill to stop and replace the work rolls.

10. The method for producing non-oriented silicon steel according to claim 7, characterized in that, The finish rolling stage further includes the step: When the target finish rolling crown meets the preset trigger condition, trigger roll wear compensation; Wherein, the roll wear compensation includes: adjusting the roll shifting amount of the finish rolling work rolls to compensate for the strip crown.

11. The method for producing non-oriented silicon steel according to claim 10, characterized in that, The preset triggering conditions include: the crown of the precision rolling target reaches a first preset value C. y And h is still ≥ h0, where C y <C max .

12. The method for producing non-oriented silicon steel according to claim 10, characterized in that, The compensation for the strip crown by adjusting the roll shifting amount of the finish rolling work rolls includes: During the finishing rolling of the first strip after triggering roll wear compensation, the amount of roll shifting of the finishing work roll is increased by ΔS1. Determine whether the height difference between the highest point on the surface of the first strip and the reference point exceeds h0; If not, then terminate the roll wear compensation. If so, the amount of roll shifting of the finishing mill work roll is increased by ΔS2; ΔS2>ΔS1.

13. The method for producing non-oriented silicon steel according to claim 12, characterized in that, The method of adjusting the roll shifting of the finishing mill rolls to compensate for strip crown also includes: After controlling the increase of the roll shifting amount of the finishing mill work roll by ΔS2, determine whether the height difference between the highest point of the produced strip surface and the reference point exceeds h0. If not, then terminate the roll wear compensation. If so, during subsequent strip finishing rolling, the amount of roll shifting of the finishing work rolls is controlled to increase by ΔS3 / piece of strip until the height difference between the highest point of the strip surface and the reference point is <h0, at which point the roll wear compensation is terminated. Among them, ΔS3 satisfies: ΔS3=ΔS1.

14. The method for producing non-oriented silicon steel according to claim 7, characterized in that, The finishing rolling stage also includes the following steps: When the preset conditions are met, stop the finishing mill and replace the finishing mill work rolls; The preset conditions include: the roll shifting allowance of the finishing work roll is less than S0, or the target crown of the finishing roll reaches the preset upper limit C. max Furthermore, the height difference between the highest point on the surface of the strip and the reference point is ≥h0.

15. The method for producing non-oriented silicon steel according to claim 7, characterized in that, In the cold rolling process, when cold rolling strips with a height difference h ≥ h0 between the highest point on the strip surface and the reference point, the surface roughness Ra of the cold rolling work rolls is controlled to be ≥ 0.7 μm.

16. A non-oriented silicon steel, characterized in that, It is prepared by the production method described in any one of claims 1 to 15.

17. The non-oriented silicon steel according to claim 16, characterized in that, Referring to GB / T 2522-2017 Test Method for Insulation Resistance and Adhesion of Coating on Electrical Steel Strip (Sheet), the adhesion level between the insulating coating of the non-oriented silicon steel and the steel strip substrate was measured to be Grade A.