A multi-stage stepped temperature control heat treatment method for iron-nickel based alloy castings

By employing a multi-stage stepped temperature-controlled heat treatment method, the problems of dendritic segregation and compositional inhomogeneity in iron-nickel-based alloy castings were solved, thereby improving the uniformity of microstructure and high-temperature performance, and significantly enhancing the strength and toughness of the alloy.

CN123108281APending Publication Date: 2026-11-17KOCEL STEEL +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611327997.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Iron-nickel based alloys are prone to significant dendritic segregation and compositional inhomogeneity during the casting process, which affects their high-temperature performance and stability. Furthermore, the problem of coarse grains at high temperatures is difficult to solve, leading to increased production difficulty and unstable performance.

Method used

A multi-stage, stepped temperature-controlled heat treatment method is adopted, including a first heat treatment and a second solution cooling and aging treatment. By controlling the heating rate and holding time, component segregation is eliminated and the microstructure is optimized.

Benefits of technology

It significantly improves the uniformity of the alloy's composition and microstructure, enhances its high-temperature strength and fatigue resistance, and improves the alloy's overall mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108281A_ABST
    Figure CN123108281A_ABST
Patent Text Reader

Abstract

This application relates to the technical field of metal heat treatment, specifically to a multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings, comprising the following steps: S1: Melting and casting, the iron-nickel-based alloy is melted into molten steel and then cast to obtain the casting; S2: Shaking and removing sand, after the casting is poured, it is cooled in a sand mold, and after its temperature drops to the set target range, it is shaken out, and the inner cavity and surface sand of the casting are cleaned; S3: First heat treatment, the casting is placed in a furnace at 500~800℃ for the first heat treatment, and a multi-stage stepped temperature control method is used for homogenization treatment, followed by cooling; S4: Riser cutting, the riser of the casting after step S3 is removed and polished; S5: Second heat treatment, the casting after step S4 is subjected to solution treatment and slow cooling aging treatment. This application, through multi-stage stepped heat treatment, significantly improves compositional segregation and dendrite segregation, greatly enhances the uniformity of the microstructure, and significantly improves the high-temperature strength of the alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metal heat treatment technology, and more specifically, to a multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings. Background Technology

[0002] Iron-nickel-based alloys, as a candidate material for the core structure of next-generation ultra-supercritical units, are expected to become an ideal choice for key pressure-bearing components such as main steam valves and high- and intermediate-pressure rotors due to their excellent high-temperature creep strength and resistance to steam oxidation. This alloy achieves high-temperature stability through a γ' phase strengthening mechanism, and its development and application respond to the urgent need for improved energy efficiency in coal-fired power units under the national "dual-carbon" strategy.

[0003] However, the complex composition of this alloy, containing multiple elements such as Cr, Mo, and Nb, presents significant challenges during the casting process. Due to its complex composition, significant dendritic segregation easily forms during solidification, resulting in the precipitation of various brittle phases in the as-cast microstructure. This compositional segregation leads to inhomogeneity in the alloy's microstructure, thus affecting its performance stability. Furthermore, the problem of coarse grains at high temperatures is difficult to resolve during subsequent high-temperature heat treatment. Coarse grains reduce the alloy's strength, toughness, and fatigue resistance, significantly negatively impacting its application in ultra-supercritical units. This inhomogeneity in composition and microstructure not only greatly increases the difficulty of casting production but also directly affects the stability of material properties. Summary of the Invention

[0004] The purpose of this invention is to provide a multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings. By controlling the heat treatment process parameters, the method can eliminate component segregation in the alloy, optimize the microstructure, and improve the strength and microstructure stability of the alloy.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: A multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings includes the following steps: S1: Melting and casting, which involves melting an iron-nickel-based alloy into molten steel and then casting it to obtain a casting. S2: Shaping and sand removal. After the casting is poured, it is cooled in the sand mold. After the temperature drops to the set target range, the shaping operation is carried out. After shaping, the inner cavity and surface sand of the casting are cleaned. S3: First heat treatment. The casting is placed in the furnace at 500~800℃ for the first heat treatment, and a multi-stage stepped temperature control method is used for homogenization treatment, followed by cooling. S4: Riser cutting, the riser is removed and polished on the casting after step S3; S5: Second heat treatment, which involves solution cooling and aging of the casting after step S4.

[0006] Preferably, the chemical composition of the iron-nickel-based alloy, by mass percentage, includes: Fe: 40%~45%, Cr: 14.0%~17%, Mo: 0.3%~0.7%, W: 0.3%~0.7%, Al: 1.1%~1.6%, Ti: 1.3%~1.8%, Si: ≤0.2%, C: ≤0.06%, P: ≤0.015%, S: ≤0.01%, with the remainder being Ni and other trace elements.

[0007] Preferably, the smelting and casting process in step S1 includes: refining the iron-nickel-based alloy into molten steel through multiple steps in an electric arc furnace, a ladle refining furnace, a vacuum oxygen blowing decarburization furnace, and a ladle refining furnace, and then casting the steel into a casting.

[0008] Preferably, in step S2, the time for the box-making operation is controlled within 1 hour.

[0009] Preferably, in step S3, the initial heat treatment heating stage employs no less than four stepped heating stages, with each stage having a heating rate ≤30℃ / h, and sequentially including the following holding points: holding at 840~860℃ in the γ′ phase subsolid solution zone for 2~5h; holding at 1090~1110℃ at the initial carbide dissolution temperature for 2~5h; holding at 1160~1190℃ in the near homogenization temperature control zone for 10~15h; and holding at ≥1180℃ in the γ phase fully diffusion temperature zone for ≥30h.

[0010] Preferably, in step S3, the cooling stage of the first heat treatment is as follows: slowly cooling to below 1100~1190℃ at a rate of ≤20℃ / h, then passing through the carbide precipitation zone at a cooling rate of ≤40℃ / h, and then air-cooling at ≤200℃ after exiting the furnace.

[0011] Preferably, in step S4, the riser cutting process is as follows: a portion of the riser is removed using a flame cutting method, with a cutting allowance of 100-150mm remaining at the root of each riser. During the cutting process, the cutting area is covered with an insulating cloth to control the cooling rate. After all risers are removed, the root allowance and patch are removed by grinding, and the riser is then ground to the target size range.

[0012] Preferably, in step S5, the heating stage of the second heat treatment is as follows: heating to the solution zone of 980~1020℃ at a heating rate of ≤40℃ / h, and holding at that temperature for 8~12h.

[0013] Preferably, the solution cooling and aging treatment performed on the casting after step S4 results in the casting finally being in an under-aged state. The solution cooling and aging treatment includes: cooling at a slow cooling rate of ≤20℃ / h to the γ' phase precipitation range of 920~940℃, holding at that temperature for 1~3h; then rapidly cooling at a cooling rate of 50~70℃ / h to the phase transformation suppression range of 700~800℃; and finally cooling at a slow cooling rate of ≤20℃ / h to below 200℃.

[0014] This application utilizes multi-stage step heat treatment to significantly improve compositional segregation and dendrite segregation, greatly enhance the uniformity of the microstructure, and significantly improve the high-temperature strength of the alloy. Attached Figure Description

[0015] Figure 1 This is a schematic flowchart of the heat treatment method for multi-stage stepped temperature control of iron-nickel-based alloy castings provided in the embodiments of this application.

[0016] Figure 2 This is an example diagram of the metallographic structure provided in the embodiments of this application.

[0017] Figure 3 This is an example diagram of the γ' phase detection results provided in an embodiment of this application. Detailed Implementation

[0018] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings. Preferred embodiments of this application are shown in the drawings. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0020] Please refer to Figure 1 , Figure 1 This is a schematic flowchart of the multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings provided in this application embodiment. The specific steps are as follows: S1: Melting and casting. The iron-nickel-based alloy is refined into molten steel through multiple steps in an electric arc furnace (EAF), ladle refining furnace (LF), vacuum oxygen blowing decarburization furnace (VOD), and ladle refining furnace (LF), before being cast into a casting. The chemical composition of the iron-nickel-based alloy, by mass percentage, includes: Fe: 40%~45%, Cr: 14.0%~17%, Mo: 0.3%~0.7%, W: 0.3%~0.7%, Al: 1.1%~1.6%, Ti: 1.3%~1.8%, Si: ≤0.2%, C: ≤0.06%, P: ≤0.015%, S: ≤0.01%, with the remainder being Ni and other trace elements.

[0021] S2: Shafting and Sand Removal. After the casting is poured, it is cooled in the sand mold. Once the temperature drops to the target range of 500~800℃, the slag removal operation is performed. The slag removal operation time is strictly controlled within 1 hour. After slag removal, the internal cavity and surface sand of the casting are cleaned.

[0022] S3: First heat treatment. The casting is placed in the furnace at 500~800℃ for the first heat treatment, and a multi-stage temperature control method is used for homogenization.

[0023] The heating stage employs four steps, with the heating rate controlled at ≤30℃ / h in each stage. The temperature is maintained at the following points in sequence: 2-5 h in the γ′ phase subsolid solution zone at 840-860℃; 2-5 h in the initial carbide dissolution temperature zone at 1090-1110℃; 10-15 h in the near homogenization temperature control zone at 1160-1190℃; and ≥30 h in the γ phase fully diffusion temperature zone at ≥1180℃.

[0024] Cooling stage: Slowly cool to below 1100~1190℃ at a rate of ≤20℃ / h, then pass through the carbide precipitation zone at a cooling rate of ≤40℃ / h, and air cool at ≤200℃ after exiting the furnace.

[0025] S4: Riser cutting. Part of the riser is removed using flame cutting, leaving a 100-150mm cutting allowance at the root of each riser. During the cutting process, the cutting area is covered with insulation cloth to control the cooling rate. After all risers are removed, the root allowance and patch can be removed, and the riser can be ground to the target size range. This process can be achieved by combining robotic grinding with manual grinding.

[0026] S5: Second heat treatment, which involves solution cooling and slow aging of the casting after step S4, so that the casting is finally in a sub-aged state.

[0027] Heating stage: Heat to the solution zone of 980~1020℃ at a heating rate of ≤40℃ / h, and hold for 8~12h.

[0028] Solution cooling and aging process: Cool to the γ' phase precipitation range of 920~940℃ at a slow cooling rate of ≤20℃ / h, and hold for 1~3h; then cool to the phase transformation suppression range of 700~800℃ at a cooling rate of 50~70℃ / h; finally cool to below 200℃ at a slow cooling rate of ≤20℃ / h.

[0029] The metallographic structure and tensile properties of the iron-nickel-based alloy castings prepared in this embodiment were observed. Figure 2 The metallographic structure example diagram shown, and Figure 3 An example image of the γ' phase detection results is shown; the tensile property test results are shown in Table 1. After treatment by the method of this application, the as-cast dendrites have been completely eliminated, the microstructure is dominated by the γ phase with a small amount of γ' phase, and the microstructure uniformity has been greatly improved.

[0030] Table 1: Test conditions Tensile strength (MPa) Yield strength (MPa) Elongation after fracture (%) room temperature 771 372 19.4 650℃ 584 358 16.1 As shown in Table 1, the casting exhibits excellent tensile properties at both room temperature and 650℃ using the multi-stage stepped temperature control heat treatment method of this invention, demonstrating the significant effect of this process in eliminating segregation, refining the microstructure, and improving the comprehensive mechanical properties of the alloy.

[0031] By adopting the technical solution provided in this application, the problems of compositional segregation and dendrite segregation in the iron-nickel based alloy are significantly improved after two multi-stage step heat treatments, and the uniformity of the alloy structure is greatly enhanced.

[0032] The second heat treatment allows the reinforcing phase in the alloy to fully dissolve into the matrix, forming a homogeneous solid solution. During the subsequent cooling process, the reinforcing phase can precipitate uniformly in the form of fine particles, resulting in a dispersion strengthening effect and significantly improving the high-temperature strength of the alloy.

[0033] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0034] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings, characterized in that, Includes the following steps: S1: Melting and casting, which involves melting an iron-nickel-based alloy into molten steel and then casting it to obtain a casting. S2: Shaping and sand removal. After the casting is poured, it is cooled in the sand mold. After the temperature drops to the set target range, the shaping operation is carried out. After shaping, the inner cavity and surface sand of the casting are cleaned. S3: First heat treatment. The casting is placed in the furnace at 500~800℃ for the first heat treatment, and a multi-stage stepped temperature control method is used for homogenization treatment, followed by cooling. S4: Riser cutting, the riser is removed and polished on the casting after step S3; S5: Second heat treatment, which involves solution cooling and aging of the casting after step S4.

2. The heat treatment method for multi-stage stepped temperature control of iron-nickel based alloy castings according to claim 1, characterized in that, The chemical composition of the iron-nickel-based alloy, by mass percentage, includes: Fe: 40%~45%, Cr: 14.0%~17%, Mo: 0.3%~0.7%, W: 0.3%~0.7%, Al: 1.1%~1.6%, Ti: 1.3%~1.8%, Si: ≤0.2%, C: ≤0.06%, P: ≤0.015%, S: ≤0.01%, with the remainder being Ni and other trace elements.

3. The heat treatment method for multi-stage stepped temperature control of iron-nickel-based alloy castings according to claim 1, characterized in that, The smelting and casting process in step S1 includes: refining the iron-nickel-based alloy into molten steel through multiple steps in an electric arc furnace, a ladle refining furnace, a vacuum oxygen blowing decarburization furnace, and a ladle refining furnace, and then casting the steel into a casting.

4. The heat treatment method for multi-stage stepped temperature control of iron-nickel-based alloy castings according to claim 1, characterized in that, In step S2, the time for the box-making operation is controlled within 1 hour.

5. The heat treatment method for multi-stage stepped temperature control of iron-nickel based alloy castings according to claim 1, characterized in that, In step S3, the initial heat treatment heating stage employs no less than four stepped heating stages, with each stage having a heating rate ≤30℃ / h, and sequentially including the following holding points: holding at 840~860℃ in the γ′ phase subsolid solution zone for 2~5h; holding at 1090~1110℃ at the initial carbide dissolution temperature for 2~5h; holding at 1160~1190℃ in the near homogenization temperature control zone for 10~15h; and holding at ≥1180℃ in the γ phase fully diffusion temperature zone for ≥30h.

6. A multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings according to claim 1 or 5, characterized in that, In step S3, the cooling stage of the first heat treatment is as follows: slowly cooling to below 1100~1190℃ at a rate of ≤20℃ / h, then passing through the carbide precipitation zone at a cooling rate of ≤40℃ / h, and then air-cooling at ≤200℃ after exiting the furnace.

7. The heat treatment method for multi-stage stepped temperature control of iron-nickel based alloy castings according to claim 1, characterized in that, In step S4, the riser cutting process is as follows: a portion of the riser is removed using a flame cutting method, with a cutting allowance of 100-150mm remaining at the root of each riser. During the cutting process, the cutting area is covered with an insulating cloth to control the cooling rate. After all risers are removed, the root allowance and patch are removed by grinding, and the riser is then ground to the target size range.

8. The heat treatment method for multi-stage stepped temperature control of iron-nickel-based alloy castings according to claim 1, characterized in that, In step S5, the heating stage of the second heat treatment is as follows: the temperature is raised to the solution zone of 980~1020℃ at a heating rate of ≤40℃ / h, and held for 8~12h.

9. A multi-stage stepped temperature control heat treatment method for iron-nickel-based alloy castings according to claim 1 or 8, characterized in that, The casting after step S4 is subjected to solution cooling and aging treatment, so that the casting is finally in an under-aged state. The solution cooling and aging treatment includes: cooling to the γ' phase precipitation range of 920~940℃ at a slow cooling rate of ≤20℃ / h, and holding for 1~3h; then rapidly cooling to the phase transformation suppression range of 700~800℃ at a cooling rate of 50~70℃ / h; and finally cooling to below 200℃ at a slow cooling rate of ≤20℃ / h.