A three-dimensional porous MXene / vermiculite composite electrode film, its preparation method and application

Three-dimensional porous MXene/vermiculite composite electrode films were prepared by electrostatic self-assembly and ice template method, which solved the problems of stacking MXene-based electrodes and introducing binders, and achieved efficient and low-cost uranyl ion adsorption and recovery.

CN123108290APending Publication Date: 2026-11-17EAST CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611296357.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing MXene-based uranium extraction electrodes suffer from problems such as severe nanosheet stacking, the need to introduce binders leading to loss of active sites and secondary pollution, complex preparation processes, and high costs.

Method used

Three-dimensional porous MXene/vermiculite composite electrode films were prepared by electrostatic self-assembly and ice template method. Vermiculite nanosheets were used as interlayer spacers and active sites to construct a three-dimensional porous conductive network, avoiding the stacking of MXene nanosheets and improving conductivity and adsorption performance.

Benefits of technology

It achieves high adsorption selectivity and high adsorption capacity, reduces preparation costs, and improves the structural stability and recyclability of the electrode membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108290A_ABST
    Figure CN123108290A_ABST
Patent Text Reader

Abstract

This invention discloses a three-dimensional porous MXene / vermiculite composite electrode membrane, its preparation method, and its applications, belonging to the field of environmental protection technology. The invention first constructs a three-dimensional porous MXene / vermiculite composite electrode membrane by electrostatic self-assembly of MXene and aminated vermiculite (AVMT) combined with freeze-drying. This composite electrode membrane utilizes the large specific surface area and excellent conductivity of MXene to lay the foundation for the removal of uranyl ions using square wave exchange electrochemical methods. The insertion of vermiculite nanosheets effectively inhibits the spontaneous stacking of MXene, expands the interlayer spacing, increases the number of active sites, and the constructed conductive network promotes ion accessibility, further enhancing the removal capacity of uranyl ions and stabilizing the interlayer space. It can be used for the efficient removal of uranyl ions in solution systems using square wave exchange methods, showing promising application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a membrane electrode, particularly to a three-dimensional porous MXene / vermiculite composite electrode membrane, and also to its preparation method and application in electrochemical adsorption of uranium, belonging to the field of electrochemical uranium extraction technology. Background Technology

[0002] Uranium-containing wastewater generated during nuclear industry operations poses a potential threat to the ecological environment due to the chemical toxicity, radioactivity, and long half-life of uranium. How to efficiently and selectively recover uranium resources from low-concentration uranium-containing water bodies has become a key issue in the fields of environmental remediation and resource recycling.

[0003] Currently, methods for uranium separation and recovery mainly include adsorption, solvent extraction, ion exchange, precipitation, and membrane separation. Among these, adsorption has received widespread attention due to its simplicity and relatively controllable cost. In recent years, electrochemical-assisted extraction technology, especially square wave voltage-driven electroextraction (SWE), has emerged due to its high extraction capacity, good selectivity, and the ability to eliminate competing ion interference through periodic potential switching. SWE technology utilizes high-frequency square wave voltage to rapidly migrate heavy metal / nucleus ions to the vicinity of the working electrode, exhibiting excellent kinetic characteristics.

[0004] However, SWE technology faces bottlenecks in electrode material design for practical applications. Traditional electrodes typically consist of three parts: a conductive matrix, an active material, and additives (binders, conductive agents). While additives ensure the stability of the electrode system, they can lead to an irreversible decrease in conductivity, hindering electron transfer. Simultaneously, additive components severely restrict the release of the active material's active space, causing pore adhesion and blockage. Furthermore, the addition of additional conductive agents also compromises system stability. These problems have long plagued researchers.

[0005] Ti3C2T x As a representative material of the MXene family, MXene is considered an ideal matrix material for uranium electroadsorption / electrocatalytic reduction due to its excellent metallic conductivity, abundant surface functional groups (-OH, -O, etc.), and high hydrophilicity. However, MXene faces two prominent structural bottlenecks in practical applications: First, the severe stacking of nanosheets. The strong van der Waals forces between MXene nanosheets make them prone to tight stacking during drying or use, resulting in the burial of a large number of active sites, blockage of ion transport channels, and a sharp decrease in specific surface area. Second, poor scalability. Existing MXene-based self-supporting membranes are mostly prepared by vacuum-assisted filtration and dense stacking, which is a complex process that is difficult to scale up. Moreover, most systems require the introduction of binders to maintain structural integrity. However, binders not only block pores but also cause component shedding during electroextraction, resulting in secondary pollution and reduced cycle stability.

[0006] To suppress stacking, researchers have tried various strategies, including the introduction of intercalating agents, polymer composites, and foam template methods. However, these methods often involve expensive additives, multi-step post-processing, and complex synthetic routes, resulting in high costs and process complexity. Meanwhile, natural vermiculite (VMT), an abundant and inexpensive layered silicate clay mineral (approximately $30 / ton), possesses a naturally negatively charged basal surface and exchangeable cations in its interlayer. After exfoliation, it can yield two-dimensional nanosheets rich in hydroxyl and oxygen functional groups, which possess the ability to interact with uranyl ions (UO2). 2+ The natural affinity of vermiculite for coordination. However, pure vermiculite materials have poor electrical conductivity and cannot be directly used in electrochemical extraction systems. Summary of the Invention

[0007] To address the shortcomings of existing MXene-based uranium extraction electrodes, such as severe nanosheet stacking, the need to introduce binders leading to loss of active sites and secondary pollution, complex preparation processes, and high costs.

[0008] The first objective of this invention is to provide a three-dimensional porous MXene / vermiculite composite electrode film, wherein the composite electrode film is made of Ti3C2T x The three-dimensional layered structure formed by electrostatic assembly of PM nanosheets and aminated vermiculite nanosheets utilizes vermiculite nanosheets as interlayer spacers and active sites, as well as a three-dimensional porous conductive network, endowing it with excellent structural stability, conductivity and adsorption properties. In particular, it has adsorption selectivity for uranyl ions and can be used for the adsorption of U(VI) in water.

[0009] The second objective of this invention is to provide a method for preparing a three-dimensional porous MXene / vermiculite composite electrode film. The preparation process of this composite electrode film is simple, low-cost, and can be scaled up for production.

[0010] The third objective of this invention is to provide an application of a three-dimensional porous MXene / vermiculite composite electrode membrane for the square wave exchange electrochemical adsorption of uranyl ions in a solution system. This membrane has advantages such as high adsorption capacity, strong adsorption selectivity, and the ability to be recycled multiple times, and is expected to be used for uranium extraction from seawater.

[0011] To achieve the above-mentioned technical objectives, the present invention provides a method for preparing a three-dimensional porous MXene / vermiculite composite electrode film, which includes the following steps:

[0012] S1: Ti3AlC2 powder was etched in an HCl-LiF mixed solution and then ultrasonically exfoliated to obtain Ti3C2T. x Nanosheet suspension;

[0013] S2: The bulk vermiculite was subjected to sodium treatment, lithium exchange, oxidative exfoliation and ultrasonic treatment in sequence to obtain a vermiculite nanosheet suspension; the vermiculite nanosheet suspension was subjected to an amino-containing silane coupling agent to obtain an amino-modified vermiculite nanosheet suspension.

[0014] S3: Ti3C2T x After mixing the nanosheet suspension with the aminated vermiculite nanosheet suspension, the mixture is deposited on the base film by vacuum filtration and then freeze-dried to obtain the three-dimensional porous MXene / vermiculite composite electrode film.

[0015] The key to the preparation method of the three-dimensional porous MXene / vermiculite composite electrode film provided by this invention lies in: methane is sodium-treated, lithium-treated, and exfoliated to form vermiculite nanosheets; the surface of the vermiculite nanosheets is then modified with amino groups to impart a positive surface charge; and finally, the nanosheets are subjected to Ti3C2T… x Electrostatic self-assembly between nanosheets and vermiculite nanosheets forms a stable three-dimensional layered structure material. Further processing using freeze-drying allows the use of ice crystals formed by water molecules as self-sacrificing templates, promoting the construction of a 3D porous network. This releases a larger specific surface area and more active sites, greatly improving the adsorption capacity of the membrane electrode.

[0016] As a preferred embodiment, the concentration of LiF in the HCl-LiF mixed solution is 60~100 mg / mL, and the concentration of HCl is 6~10 mol / L.

[0017] As a preferred embodiment, the ratio of the Ti3AlC2 powder to the HCl-LiF mixed solution is measured according to a mass ratio of Ti3AlC2 to LiF of 1:(1.5~2.0).

[0018] As a preferred embodiment, the etching conditions are: a stirring reaction at 35~45℃ and a stirring rate of 400~800rpm for 30~60 h.

[0019] As a preferred embodiment, the conditions for ultrasonic ablation are: output power of 100~400W and frequency of 30~50KHz.

[0020] As a preferred embodiment, the conditions for the sodium treatment are: using a saturated NaCl solution as the sodium treatment solution, a temperature of 160~200℃, and a time of 18~30 h.

[0021] As a preferred embodiment, the conditions for the lithiation exchange are: using a 1.5~2.5 mol / L LiCl solution as the lithiation solution, a temperature of 60~80 ℃, and a time of 6~12 h.

[0022] As a preferred embodiment, the oxidative stripping conditions are as follows: using hydrogen peroxide as the oxidizing solution, reacting in a sealed vessel at a temperature of 115~125℃ for 6~10 h.

[0023] As a preferred embodiment, the amount of the amino-containing silane coupling agent is 5-15% of the molar amount of vermiculite nanosheets in the vermiculite nanosheet suspension. An example of an amino-containing silane coupling agent is 3-aminopropyltriethoxysilane.

[0024] As a preferred embodiment, the conditions for the ammoniation reaction are: pH 8.0~9.0, temperature 75~85℃, and time 7~9h.

[0025] As a preferred embodiment, the Ti3C2T x The nanosheet suspension and the aminated vermiculite nanosheet suspension were prepared according to the Ti3C2T ratio. x The mass ratio of nanosheets to amino-modified vermiculite nanosheets is 1~3:1~3.

[0026] As a preferred embodiment, the freeze-drying conditions are: freeze-drying at a temperature below -50°C for 20~30 hours.

[0027] This invention also provides a three-dimensional porous MXene / vermiculite composite electrode membrane, which is obtained by the aforementioned preparation method. The three-dimensional porous MXene / vermiculite composite electrode membrane of this invention uses MXene nanosheets as the electrode framework and vermiculite nanosheets as structural supports and active sites to support the interlayer space of MXene, establish a conductive network, improve ion accessibility, and enhance electrochemical removal capability.

[0028] This invention also provides an application of a three-dimensional porous MXene / vermiculite composite electrode membrane, which serves as the working electrode in a dual-electrode system for the square-wave exchange electrochemical adsorption of uranyl ions in a solution system.

[0029] The method for preparing the three-dimensional porous MXene / vermiculite composite electrode film of the present invention includes the following steps:

[0030] 1) Ti3C2T x Preparation of the nanosheet suspension: First, Ti3AlC2 powder was added to a mixed solution of concentrated hydrochloric acid (HCl) and lithium fluoride (LiF). The mixture was stirred uniformly at 400-800 rpm for 30-60 hours at a constant temperature of 35-45℃. The resulting black solid precipitate was washed with dilute hydrochloric acid and centrifuged multiple times. After the supernatant became turbid, it was sonicated for 1-3 hours at an output power of 100-400 W and a frequency of 30-50 kHz. Finally, it was centrifuged at 3000-5000 rpm for 20-40 minutes. The resulting upper suspension was Ti3C2T x Nanosheet suspension.

[0031] 2) Preparation of amino-modified vermiculite (AVMT) nanosheet dispersion: Bulk vermiculite was placed in a saturated NaCl solution and refluxed at 160–200 °C for 18–30 h for ion exchange, followed by LiCl interlayer lithiation exchange. The conditions for lithiation exchange are as follows: using a 1.5~2.5 mol / L LiCl solution as the lithiation solution, a temperature of 60~80℃, and a time of 6~12 h, followed by H2O2 oxidation and exfoliation. The conditions for oxidation and exfoliation are as follows: using hydrogen peroxide (30wt%) as the oxidizing solution, reacting in a sealed vessel at a temperature of 115~125℃ for 6~10 h, followed by ultrasonic treatment and centrifugation to obtain a single-layer VMT nanosheet dispersion; then reacting with the silane coupling agent APTES at a pH of 8.0~9.0 and a temperature of 75~85℃ for 7~9 h to graft amino groups onto the vermiculite surface, resulting in a positively charged aminated vermiculite (AVMT) nanosheet dispersion.

[0032] 3) Ti3C2T x Nanosheet suspension and AVMT dispersion were prepared according to Ti3C2T x The mixture was mixed with AVMT at a mass ratio of 1:3 to 3:1 and stirred for 0.5 to 1.5 hours to ensure thorough mixing. The resulting gray-black suspension was then deposited onto the base film by vacuum-assisted filtration. After being freeze-dried at -60°C for 24 to 48 hours, the product 3D-TV was obtained. 3D-TV was used directly as a self-supporting electrode film without further calcination. The final product was named 3D-TV.

[0033] The three-dimensional porous MXene / vermiculite composite electrode membrane of the present invention is used for the removal of uranyl ions in a solution system by square wave exchange method.

[0034] The three-dimensional porous MXene / vermiculite composite electrode membrane was added to a solution system containing uranyl ions. A square wave exchange dual-electrode system supported by an arbitrary waveform generator was used to react at room temperature for a specified time under a certain voltage. The pH of the solution system containing uranyl ions was adjusted to the range of 2.0–7.0 using a pH adjuster. The electrochemical removal time of the three-dimensional porous MXene / vermiculite composite electrode membrane in the solution system containing uranyl ions was 5–800 min. The concentration of uranyl ions in the solution system ranged from 5–200 mg / L. During the square wave exchange process, the operating AC voltage was 0 and -5 V, the operating frequency was 100–500 Hz, preferably 400 Hz, and the duty cycle was 0–100%, preferably 50%. The initial phase was 0–360°, preferably 180°.

[0035] Compared with the prior art, the beneficial effects of the technical solution of the present invention are as follows:

[0036] (1) The present invention prepares a three-dimensional porous MXene / vermiculite composite electrode film by electrostatic self-assembly and ice template freeze-drying method, which has the advantages of simple preparation method, low cost and strong stability.

[0037] (2) The three-dimensional porous MXene / vermiculite composite electrode film prepared by the present invention effectively inhibits the collapse of MXene pores by the three-dimensional porous structure formed by the ice template method, increases the interlayer spacing of MXene, forms a conductive network, promotes ion migration, restricts the spontaneous stacking of MXene, and releases active sites.

[0038] (3) The three-dimensional porous MXene / vermiculite composite electrode film prepared by the present invention has a large removal capacity, low energy consumption and stable system under the technical support of square wave exchange method.

[0039] (4) The three-dimensional porous MXene / vermiculite composite electrode membrane prepared in this invention showed good removal capacity, stable structure and excellent circulation performance in the uranium removal experiment in wastewater supported by square wave exchange method. Attached Figure Description

[0040] Figure 1 This is a schematic diagram of 3D-TV synthesis.

[0041] Figure 2 This is a SEM image of a 3D-TV.

[0042] Figure 3 This is the XRD pattern of a 3D-TV.

[0043] Figure 4 The graph shows the effect of operating voltage on the electrochemical removal of uranyl ions in 3D-TV.

[0044] Figure 5 This is a graph showing the amount of uranium removed by electrochemical removal in 3D-TV.

[0045] Figure 6 SEM and EDS images of the electrochemical removal of 3D-TV.

[0046] Figure 7 Performance diagram of electrochemical removal of uranyl ions from 3D-TV simulated wastewater.

[0047] Figure 8 This is a graph showing the cyclic stability performance of 3D-TV. Detailed Implementation

[0048] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with embodiments. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0049] Example 1

[0050] Preparation method and property characterization of three-dimensional porous MXene / vermiculite composite electrode 3D-TV.

[0051] 2g of Ti3AlC2 was washed with deionized water and ethanol, respectively, and then transferred to a vacuum furnace at 60℃ for drying for 24 h and stored. 40 mL of HCl (9 mol / L) was added to a polytetrafluoroethylene beaker, and 3.2 g of LiF was weighed and slowly added to the solution. After thorough stirring, the mixture was transferred to a water bath at 40℃ and stirred at 600 rpm for 30 min. Within half an hour, dried Ti3AlC2 was slowly added to the solution, and the mixture was stirred for 48 h. The resulting black liquid was washed with a centrifuge to remove unreacted LiF and other substances. The residue was washed with dilute hydrochloric acid (2 mol / L), centrifuged several times with deionized water (5000 rpm) until the upper layer could not be centrifuged further. The mixture was then transferred to an ultrasonic ice bath under argon atmosphere (200 W, 40 kHz) for 4 hours, and then centrifuged at 3500 rpm for 20 min. The resulting suspension was stored at 4℃ under argon atmosphere to prevent oxidation.

[0052] Further, 2.0 g of lumpy vermiculite (VMT, 325 mesh) was added to 60 mL of saturated NaCl aqueous solution, placed in a polytetrafluoroethylene-lined autoclave, and refluxed / hydrothermally heated at 180 °C for 24 h with continuous stirring. After removal, the solution was centrifuged and discarded, then repeatedly washed with deionized water until no chloride ions were detected (AgNO3 detection), yielding NaCl. + Saturated vermiculite. The above product was redispersed in 60 mL of 2 mol / L LiCl solution and stirred at 70 °C for 8 h to perform Li... + / Na +Interlayer exchange. Centrifuge and wash until neutral. Redisperse Li-containing vermiculite in 60 mL of 30 wt% H2O2 and react in a closed, stirred environment at 120 °C for approximately 8 h to achieve interlayer expansion and partial oxidative exfoliation. After cooling to room temperature, transfer the suspension to an ultrasonic bath and sonicate for 2 h. Then, centrifuge at 3500 rpm for 30 min and collect the upper stable colloid, which is the monolayer VMT nanosheet dispersion. Transfer the VMT nanosheet dispersion to a three-necked flask, add APTES (3-aminopropyltriethoxysilane, molar amount approximately 10 mol% of VMT Si sites), adjust the pH to weakly alkaline (approximately 8.5), and reflux in an oil bath at 80 °C for 8 h with nitrogen protection and stirring. After the reaction is complete, centrifuge to collect the solid, wash repeatedly with an ethanol / water mixture until the filtrate is odorless, and redisperse in water using ultrasound to obtain a positively charged AVMT nanosheet dispersion.

[0053] The nanosheet suspension was mixed with AVMT at a 1:1 mass ratio and stirred for 2 h to ensure thorough mixing. The resulting gray-black suspension was then deposited onto the substrate film via vacuum-assisted filtration. After 24 h of vacuum freeze-drying at -50 °C, the product 3D-TV was obtained. No further calcination was required, and the final product was named 3D-T1V1.

[0054] Figure 1 This is a schematic diagram of the 3D-TV synthesis process.

[0055] Figure 2 This is a SEM image of a 3D-TV. The MXene interlayer exhibits a distinct three-dimensional porous network structure. Vermiculite nanosheets can be effectively inserted into the MXene interlayer to form bridges for ion transport and enhance the overall structural stability.

[0056] Figure 3 This is an XRD pattern. Ti3C2T x A diffraction peak representing the (002) crystal plane appeared at 7.04°. The (002) peak of 3D-TV shifted to 6.53°, corresponding to an increase in interlayer spacing from 1.25 nm to 1.35 nm. This proves that the insertion of vermiculite effectively increased the interlayer spacing of MXene and suppressed stacking.

[0057] Example 2

[0058] Electrochemical removal of uranyl ions by a three-dimensional porous MXene / vermiculite composite electrode (3D-TV).

[0059] Figure 4The effect of different voltages on the electrochemical uranium removal performance (t=720 min, pH=5, v / m=20, CO=200 mg / L, Frequency=400 Hz) was investigated: at -5 V, the pure MXene membrane exhibited a maximum adsorption capacity of 714 mg / g, while the 3D-TV membrane reached a maximum adsorption capacity of 1852 mg / g. Because 3D-TV contains vermiculite components, its three-dimensional porous structure and abundant active sites are conducive to the migration and enrichment of U(VI). Therefore, under the same conditions, 3D-TV can achieve a higher removal capacity.

[0060] The time-varying curves of 3D-TV electrochemical uranium removal performance under the conditions of V=-5 V, pH=5, v / m=20, CO=200 mg / L, and Frequency=400 Hz are shown below. Figure 5 As shown, 3D-TV exhibits excellent removal capabilities at high concentrations. In a 200 mg / L U(VI) solution, the electrochemical removal capacity of 3D-TV reaches as high as 1852 mg / g. Its high conductivity and optimized three-dimensional porous structure enable 3D-TV to achieve higher efficiency and capacity during the separation process.

[0061] Figure 6 These are SEM and EDS images of the electrode surface after electrochemical uranium removal testing. Uranium is attached to the material surface in the form of sodium uranate hydrate (Na2U2O7), which facilitates recovery and enrichment.

[0062] Example 3

[0063] 3D-TV Cyclic Stability and Selectivity Testing of Three-Dimensional Porous MXene / Vermiculite Composite Electrode

[0064] like Figure 7 The competing ions were Cd, Ce, Zn, K, La, Co, and Cr, with a concentration of 50 mg / L, which was five times the concentration of U(VI). When the competing ions were present, the electrochemical removal of U(VI) by 3D-TV remained stable, with a distribution coefficient K0. d (U) = 190.28 L / g. 3D-TV exhibits higher selectivity and efficiency in the electrochemical removal of U(VI).

[0065] like Figure 8 The stability of 3D-TV was tested by cyclic elution using 0.01 mol / L dilute nitric acid as the eluent. After five cycles, the removal efficiency of 3D-TV remained at 88%, indicating good reusability.

[0066] This invention prepares a three-dimensional porous MXene / vermiculite composite electrode membrane (3D-TV) using an electrostatic self-assembly ice template method, which exhibits excellent electrochemical uranyl ion removal capability.

[0067] The three-dimensional porous MXene / vermiculite composite electrode membrane (3D-TV) prepared by this invention uses MXene as the electrode framework and vermiculite as the structural support and active site to support the interlayer space of MXene, establish a conductive network, improve ion accessibility, and enhance electrochemical removal capability.

[0068] The three-dimensional porous MXene / vermiculite composite electrode membrane (3D-TV) prepared by this invention, with the support of square wave exchange technology, yields easily recoverable sodium uranate hydrate insoluble uranium solid, facilitating recovery and enrichment, simplifying removal and elution steps, and reducing recycling costs.

[0069] The embodiments described above are merely preferred embodiments of the present invention, and while the descriptions are specific and detailed, they are not intended to limit the present invention. It should be noted that various changes and modifications can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the concept and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a three-dimensional porous MXene / vermiculite composite electrode film, characterized in that: Includes the following steps: S1: Ti3AlC2 powder was etched in an HCl-LiF mixed solution and then ultrasonically exfoliated to obtain Ti3C2T. x Nanosheet suspension; S2: The bulk vermiculite was subjected to sodium treatment, lithium exchange, oxidative exfoliation and ultrasonic treatment in sequence to obtain a vermiculite nanosheet suspension; the vermiculite nanosheet suspension was subjected to an amino-containing silane coupling agent to obtain an amino-modified vermiculite nanosheet suspension. S3: Ti3C2T x After mixing the nanosheet suspension with the aminated vermiculite nanosheet suspension, the mixture is deposited on the base film by vacuum filtration and then freeze-dried to obtain the three-dimensional porous MXene / vermiculite composite electrode film.

2. The method for preparing a three-dimensional porous MXene / vermiculite composite electrode film according to claim 1, characterized in that: The concentration of LiF in the HCl-LiF mixed solution is 60~100 mg / mL, and the concentration of HCl is 6~10 mol / L; The ratio of Ti3AlC2 powder to the HCl-LiF mixed solution is measured according to a mass ratio of Ti3AlC2 to LiF of 1:(1.5~2.0).

3. The method for preparing a three-dimensional porous MXene / vermiculite composite electrode film according to claim 1, characterized in that: The etching conditions are: at a temperature of 35~45℃, the reaction is stirred at a rate of 400~800 rpm for 30~60 h; The conditions for ultrasonic ablation are: output power of 100~400W and frequency of 30~50KHz.

4. The method for preparing a three-dimensional porous MXene / vermiculite composite electrode film according to claim 1, characterized in that: The conditions for the sodium treatment are as follows: using a saturated NaCl solution as the sodium treatment solution, the temperature is 160~200℃, and the time is 18~30 h. The conditions for the lithiation exchange are as follows: using a 1.5~2.5 mol / L LiCl solution as the lithiation solution, a temperature of 60~80 ℃, and a time of 6~12 h.

5. The method for preparing a three-dimensional porous MXene / vermiculite composite electrode film according to claim 1, characterized in that: The conditions for the oxidative stripping are as follows: using hydrogen peroxide as the oxidizing solution, reacting in a sealed vessel at a temperature of 115~125℃ for 6~10 h.

6. The method for preparing a three-dimensional porous MXene / vermiculite composite electrode film according to claim 1, characterized in that: The amount of the amino-containing silane coupling agent used is 5-15% of the molar amount of vermiculite nanosheets in the vermiculite nanosheet suspension; The conditions for the ammoniation reaction are: pH 8.0~9.0, temperature 75~85℃, and time 7~9h.

7. The method for preparing a three-dimensional porous MXene / vermiculite composite electrode film according to claim 1, characterized in that: The Ti3C2T x The nanosheet suspension and the aminated vermiculite nanosheet suspension were prepared according to the Ti3C2T ratio. x The mass ratio of nanosheets to amino-modified vermiculite nanosheets is 1~3:1~3.

8. The method for preparing a three-dimensional porous MXene / vermiculite composite electrode film according to claim 1, characterized in that: The freeze-drying conditions are as follows: freeze-drying at a temperature below -50°C for 20 to 30 hours.

9. A three-dimensional porous MXene / vermiculite composite electrode film, characterized in that: It is obtained by the preparation method described in any one of claims 1 to 8.

10. The application of the three-dimensional porous MXene / vermiculite composite electrode film according to claim 9, characterized in that: It is used as the working electrode in a two-electrode system for the square-wave exchange electrochemical adsorption of uranyl ions in a solution system.