A method for promoting rapid melting and separation of metal components from multi-source resin gasification ash slag

By adding flux and enriching agent, and using electro-effect heating, low-energy melting and separation of multi-source resin gasification ash is achieved, which solves the problem of difficult resource utilization of ash in the existing technology and realizes efficient metal recovery and ash detoxification.

CN123108302APending Publication Date: 2026-11-17GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611474448.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are insufficient for efficiently recovering metal components from multi-source resin gasification ash, and the high cost of metallurgical recovery makes it difficult to utilize the ash as a resource.

Method used

By adding fluxes and enriching agents, low-energy melting and separation of multi-source resin gasification ash is achieved by using electro-effect heating, reducing the melting temperature and promoting the separation of heterogeneous materials. Fluxes such as CaO, SiO2, K2O, Al2O3 and CuO and enriching agents such as CuO and Cu2O are used, combined with electro-effect heating to achieve self-reforming melting of ash.

Benefits of technology

It has achieved low-energy and rapid melting and separation of multi-source resin gasification ash, reducing energy consumption and pollution, broadening the path of resource utilization, and simplifying the operation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108302A_ABST
    Figure CN123108302A_ABST
Patent Text Reader

Abstract

This invention discloses a method for promoting the rapid melting and separation of metal components from multi-source resin gasification ash. The method includes the following steps: (1) determining the composition of the multi-source resin gasification ash; (2) selecting a fluxing-enriching agent based on the composition of the multi-source resin gasification ash, and adjusting the mixing ratio of the fluxing-enriching agent with the components of the multi-source resin gasification ash to react with the components of the multi-source resin gasification ash to generate low-melting-point compounds; (3) mixing the multi-source resin gasification ash and the fluxing-enriching agent, subjecting the resulting mixture to electrothermal heating and melting, and collecting and recovering the lower layer of metal after the mixture has completely melted and separated into layers. This invention addresses the inherent characteristics of multi-source resin gasification ash by adding a fluxing-enriching agent, utilizing the colligative effect and conductivity of the eutectic to lower the ash melting point, simplifying the material flow of the system, and saving related fuel and energy consumption compared to traditional pyrometallurgical smelting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of comprehensive utilization technology of solid waste, and in particular to a method for promoting the rapid melting and separation of metal components from multi-source resin gasification ash slag. Background Technology

[0002] Resin-based solid waste is one of the main sources of municipal solid waste, including electronic motherboards, construction waste, and decommissioned new energy components. With the rapid development of emerging industries such as new energy and smart devices in recent years, its output has exploded. Resin-based waste has a complex composition, often highly composite with inorganic materials such as metals, and frequently contains bromine-chlorine flame retardants. Gasification is a highly efficient method for treating multi-source resin-based solid waste, offering advantages such as high energy utilization efficiency, controllable pollution, flexible scale, and ease of achieving multi-product resource utilization. In recent years, technologies such as pressurized gasification and chemical looping gasification have been widely developed and partially commercialized. The development of new gasification technologies allows for more precise control of reaction temperatures, enabling more efficient pollution control and energy recovery. However, because the system temperature is lower than traditional incineration and gasification methods, the resulting ash cannot be smelted in situ within the furnace. Resin-based solid wastes, such as those from electronic motherboards and decommissioned new energy components, contain metals. The use of heavy metals like copper makes it difficult to recycle the ash as building materials or dispose of it in landfills. Therefore, recovering these metals through metallurgical methods and rendering the ash harmless is essential for the efficient recycling of multi-source resin waste. However, metallurgical recycling is costly, necessitating the development of new energy-efficient treatment methods. Summary of the Invention

[0003] The purpose of this invention is to provide a method for promoting the rapid melting and separation of metal components from multi-source resin gasification ash. The method proposed in this invention combines the intrinsic characteristics of multi-source resin ash, and by adding metal flux and enriching agent, the melting temperature of ash is reduced, the electrical conductivity and heat generation characteristics of the system are improved, thereby promoting the separation of heterogeneous materials in ash and reducing smelting energy consumption.

[0004] This invention is achieved through the following technical solutions:

[0005] This invention protects a method for promoting the rapid melting and separation of metal components from multi-source resin gasification ash slag, comprising the following steps:

[0006] (1) Composition determination: The composition of the ash residue from the multi-source resin gasification was determined;

[0007] (2) Selection of flux-enriching agent: Based on the composition of the gasification ash of multi-source resin, select flux or a mixture of flux and enriching agent as flux-enriching agent, and adjust the mixing ratio of flux-enriching agent and the composition of multi-source resin gasification ash so that the flux-enriching agent reacts with the composition of multi-source resin gasification ash to generate low melting point compounds.

[0008] (3) Electro-effect melting and separation reaction: The multi-source resin gasification ash and flux-enrichment agent are mixed, and the resulting mixture is heated and melted by electro-effect. After the mixture is completely melted and separated into layers, the lower layer metal is collected and recovered.

[0009] The method proposed in this invention is applied to the gasification ash residue of resin-based solid waste. Utilizing the high metal content and strong conductivity of the ash residue, it achieves low-energy self-reforming and smelting of the ash residue through electro-effect heating, thereby enriching the metal components. This facilitates the recovery of metal components while simultaneously detoxifying the slag portion of the ash residue, enabling further recycling. Preferably, in step (1), the composition and mass fraction of the multi-source resin gasification ash residue are determined, and the components include SiO2, Al2O3, CaO, and CuO.

[0010] Preferably, the multi-source resin gasification ash composition determination method used in step (1) includes X-ray fluorescence spectroscopy (XRF) and inductively coupled plasma spectroscopy (ICP) after full component digestion.

[0011] Preferably, the fluxing agent in step (2) is selected from at least one of CaO, SiO2, K2O, Al2O3 and Na2O, and the enriching agent is selected from at least one of CuO, Cu2O and Cu.

[0012] Since the CaO and CuO contents in the multi-source resin gasification ash vary significantly, the composition of the flux-enriching agent is determined based on the mass fraction of CaO and CuO in the multi-source resin gasification ash. The mixing ratio of the flux-enriching agent and the multi-source resin gasification ash is adjusted so that the flux-enriching agent reacts with the multi-source resin gasification ash to generate low-melting-point compounds and produce a low-temperature eutectic effect. This promotes the rapid melting of the multi-source resin gasification ash at a lower temperature and the rapid enrichment of metals, thereby saving energy in the treatment system and achieving efficient treatment and resource recovery of the multi-source resin gasification ash.

[0013] This invention targets the composition of multi-source resin gasification ash slag, adding Cu and its oxides, or copper-rich ash slag, as the metal enriching agent, reducing dependence on specific compound metal enriching agents. Simultaneously, the amount of flux and metal enriching agent added is determined by measuring the composition of the multi-source resin gasification ash slag. Due to the unique composition of multi-source resin gasification ash slag, the addition of its flux and enriching agent is specific. With the addition of specific flux and metal enriching agent, this invention utilizes the electro-effect to achieve the heating and melting process of the ash slag. This melting process does not require the addition of reducing gases, and the heating and cooling are rapid with a high energy conversion rate, saving resources and energy consumption in the melting process.

[0014] Preferably, adjusting the mixing ratio of flux-enriching agent and multi-source resin gasification ash in step (2) specifically includes the following steps:

[0015] (a) Determine the content of Al2O3 components;

[0016] (b) Based on the Al2O3 content, a ternary phase diagram of CaO, SiO2 and CuO was established. The optimal ratio range of each component in the low-temperature eutectic region was determined using the ternary phase diagram to ensure that the mixture forms a low-viscosity melt with good fluidity in the range of 1100°C-1250°C.

[0017] (c) Based on the actual composition fluctuations of ash and slag, the amount of flux-enriching agent added is determined by phase diagram boundary calibration.

[0018] Step b involves establishing the ternary phase diagram as follows: ① Consult the database for the physical properties of Al2O3, CaO, SiO2, and CuO above 1000°C, and the compound composition of the three species under these temperature conditions. ② Based on the Al2O3 content determined in step a, vary the contents of CaO, SiO2, and CuO to simulate the species distribution under these conditions. ③ Based on the simulation results, establish coordinate axes for the contents of CaO, SiO2, and CuO on the three sides of an equilateral triangle, and plot the ternary phase diagram according to the simulation results.

[0019] Step c consists of the following steps: ① Locate the point on the ternary phase diagram based on the actual composition of the ash. ② Find the lower-temperature liquid region near this point, which should meet the condition of CuO content above 8%. ③ Based on the coordinates of this lower-temperature liquid region, add a certain amount of CaO and CuO to the ash to make the composition of the mixture conform to the coordinates.

[0020] Preferably, in step (2), the mixing ratio of the flux-enriching agent and the multi-source resin gasification ash is determined so that the final slag basicity is controlled at 1.0-1.4, and the CuO content accounts for more than 8 wt% of the mass of the multi-source resin gasification ash. The slag basicity is the mass ratio of basic oxides (CaO, MgO) to acidic oxides (SiO2, Al2O3).

[0021] Further optimization yields a slag basicity of 1.2 and a CuO content of 15%–25% of the mass of the multi-source resin gasification ash. These standards can be achieved by mixing metal-rich ash with gold-removing ash.

[0022] Further preferred, in step (c), the flux-enriching agent is CaO and / or CuO, and the amount of flux-enriching agent added is 5-20 wt% of the mass of the multi-source resin gasification ash.

[0023] Preferably, in step (3), the mixture is placed in an electro-effect melting device, and the mixture is energized by the metal-rich conductivity of the mixture, and the mixture is melted by the heat effect generated by the energization.

[0024] Further preferred, the electro-effect melting device is an electric arc / resistance melting furnace. During the melting process, an inert gas is introduced into the electric arc / resistance melting furnace. After the mixture melts, it separates into layers due to density differences. The lower layer of molten metal is then removed to achieve enrichment and separation.

[0025] Further optimization involves using high-purity nitrogen or high-purity argon as the inert gas.

[0026] Preferably, the reaction conditions of the electric arc / resistance melting furnace are: reaction voltage 380 V, reaction current 80-120 A, melting time 20-60 min, and furnace temperature 1500°C-1800°C.

[0027] Compared with the prior art, the beneficial effects of the present invention are:

[0028] 1. This invention addresses the inherent characteristics of multi-source resin gasification ash by adding inexpensive oxides such as CaO or CuO. Utilizing the colligative effect and conductivity of the eutectic, the melting point of the ash is reduced, simplifying the material flow of the system. Compared to traditional pyrometallurgical smelting, this invention saves on related fuel and energy consumption.

[0029] 2. This invention is applied to the gasification ash residue of resin-based solid waste, which broadens the resource utilization pathways of resin-based solid waste and realizes the low-energy and low-pollution utilization of resin-based solid waste.

[0030] 3. The preparation method proposed in this invention is simple to operate and requires no additional cost. It can be further promoted and applied to the resource and energy utilization of other similar ash slags.

[0031] 4. This invention achieves the melting of ash slag through the electro-effect method, which effectively targets the metal-rich conductive characteristics of multi-source resin ash slag. Compared with traditional smelting methods, the reaction process has a simple material flow, a short recovery cycle, and low secondary pollution. Attached Figure Description

[0032] Figure 1 This is the ternary phase diagram of SiO2, CaO and CuO of the present invention;

[0033] Figure 2 This is a schematic diagram of the structure of an electric arc / resistance melting furnace;

[0034] Explanation of reference numerals in the attached drawings: 1. Support base; 2. Rotary shaft assembly; 3. Water-cooled furnace shell; 4. Castable refractory layer; 5. Refractory insulation layer; 6. Crucible; 7. Electrode lifting assembly; 8. Water inlet pipe; 9. Water outlet pipe. Detailed Implementation

[0035] The present invention will be further described in detail below with reference to embodiments. These embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions in the art or as recommended by the manufacturer; the raw materials and reagents used, unless otherwise specified, are considered to be commercially available materials and reagents that can be obtained through conventional markets. The multi-source resin ash in the following embodiments is the ash from the gasification of electronic board waste recovered in an electronic recycling plant. Figure 2 As shown, the electric arc / resistance melting furnace used in the following embodiments consists of a support base 1, a rotating shaft assembly 2, a water-cooled furnace shell 3, a castable layer 4, a refractory insulation layer 5, a crucible 6, an electrode lifting assembly 7, a water inlet pipe 8, and a water outlet pipe 9. The fixed end of the rotating shaft assembly 2 is mounted on the support base 1, and the rotating end is connected to the water-cooled furnace shell 3. The water-cooled furnace shell 3 is provided with the castable layer 4, the refractory insulation layer 5, and the crucible 6 sequentially from the outside in. The electrode lifting assembly 7 is positioned above the water-cooled furnace shell 3, with its electrode rod penetrating the interior of the water-cooled furnace shell 3 and facing the furnace chamber of the crucible 6. The water inlet pipe 8 and the water outlet pipe 9 are connected to the inlet and outlet of the water-cooled furnace shell 3, respectively. The support base 1 is rotatably connected to the water-cooled furnace shell 3 via the rotating shaft assembly 2, allowing the water-cooled furnace shell 3 to tilt around the axis of the rotating shaft assembly 2. Both the water inlet pipe 8 and the water outlet pipe 9 are connected to the cooling water jacket of the water-cooled furnace shell 3, forming a circulating cooling circuit.

[0036] In this process, ash / mixture is fed into crucible 6 through a furnace nozzle. A graphite electrode on the electrode lifting assembly 7 is inserted into the ash. A bottom electrode is designed at the bottom of the crucible. The graphite electrode descends via the electrode lifting assembly and is energized, creating a potential difference with the bottom electrode and generating an electric arc and current. This electro-effect rapidly heats the ash until it melts. After melting for a period of time, a rotating shaft assembly on the support base tilts the furnace at a certain angle, opening the outlet to allow the lower layer of metal to flow out and be collected. A water-cooled furnace shell is installed outside the furnace to ensure sample collection and furnace safety.

[0037] Example 1

[0038] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 96% of it consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 49.80%, 11.17%, 8.84%, and 25.92%, respectively.

[0039] No further treatment was performed on the ash residue. Ash flow temperature and viscosity-temperature curves were tested, and the results are shown in Table 1.

[0040] Send the mixture to Figure 2 The electric arc melting furnace shown utilizes the electro-effect to heat the mixture. The reaction voltage is 380 V, the reaction current is 120 A, the melting time is 20 min, and the furnace temperature is maintained at approximately 1800°C. The reaction atmosphere is nitrogen, and the gas flow rate is 100 mL / min. The molten slag and metal separate into layers inside the furnace. The lower metal layer is collected, and its composition is tested. By mass, the elemental distribution is as follows: Cu: 90.35%, O: 7.65%, Fe: 0.75%, Ca: 0.36%, Cr, Ni, Ba, Mg, etc.: 0.89%.

[0041] Example 2

[0042] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 96% of it consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 49.80%, 11.17%, 8.84%, and 25.92%, respectively.

[0043] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established, as follows: Figure 1 As shown in the phase diagram, it is speculated that 10 wt.% of powdered CaO with a particle size less than 0.2 mm was added to the ash as a flux and mixed evenly. The ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0044] The mixture was fed into the same electric arc melting furnace as in Example 1. The mixture was heated using the electric effect, with a reaction voltage of 380 V, a reaction current of 80 A, a melting time of 1 h, and the furnace temperature maintained at approximately 1600°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 90.01%, O: 8.22%, Fe: 0.81%, Ca: 0.23%, Cr, Ni, Ba, Mg, etc.: 0.73%. Compared to Example 1, this method achieved the same effect as Example 1, but with a significant reduction in the required current and temperature.

[0045] Example 3

[0046] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0047] No further treatment was performed on the ash residue. Ash flow temperature and viscosity-temperature curves were tested, and the results are shown in Table 1.

[0048] The mixture was fed into the same electric arc melting furnace as in Example 1, and heated using the electro-effect. The reaction voltage was 380 V, the reaction current was 120 A, the melting time was 1 h, and the furnace temperature was maintained at approximately 1600°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 3.17%, O: 56.32%, Fe: 1.71%, Ca: 15.63%, Si: 22.19%, Cr, Ni, Ba, Mg, etc.: 0.98%. Compared to Examples 1 and 2, the lower layer showed insufficient metal enrichment.

[0049] Example 4

[0050] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0051] Using Al2O3 content as a standard (similar to Example 1), a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that 10 wt.% of powdered CaO with a particle size less than 0.2 mm was added to the ash slag as a flux and mixed evenly. The ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0052] The mixture was fed into the same electric arc melting furnace as in Example 1, and heated using the electro-effect. The reaction voltage was 380 V, the reaction current was 80 A, the melting time was 1 h, and the furnace temperature was maintained at approximately 1500°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 4.62%, O: 58.15%, Fe: 1.92%, Ca: 20.65%, Si: 13.79%, Cr, Ni, Ba, Mg, etc.: 0.87%. Compared to Example 3, the required current and temperature for the reaction were significantly reduced.

[0053] Example 5

[0054] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0055] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 10 wt.% of powdered CaO with a particle size less than 0.2 mm from the ash slag as a flux and 5 wt.% of powdered CuO with a particle size less than 0.2 mm from the ash slag as a metal enriching agent and mixing them evenly was appropriate. The ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0056] The mixture was fed into the same electric arc melting furnace as in Example 1. The mixture was heated using the electro-effect, with a reaction voltage of 380 V, a reaction current of 80 A, a melting time of 1 h, and the furnace temperature maintained at approximately 1600°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers within the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 88.26%, O: 8.06%, Fe: 0.66%, Ca: 0.27%, Cr, Ni, Ba, Mg, etc.: 2.75%. Compared to Example 3, the required current and temperature were significantly reduced, and the metal enrichment was better.

[0057] Example 6

[0058] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0059] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 10 wt.% powdered CaO with a particle size less than 0.2 mm from the ash slag as a flux and 10 wt.% powdered CuO with a particle size less than 0.2 mm from the ash slag as a metal enriching agent, and mixing them evenly, would be appropriate. Ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0060] The mixture was fed into the same electric arc melting furnace as in Example 1, and heated using the electric effect. The reaction voltage was 380 V, the reaction current was 80 A, the melting time was 1 h, and the furnace temperature was maintained at approximately 1600°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 90.36%, O: 7.89%, Fe: 0.53%, Ca: 0.25%, Cr, Ni, Ba, Mg, etc.: 0.97%. Compared to Example 5, the metal enrichment was higher, and the molten slag had better fluidity at the same temperature.

[0061] Example 7

[0062] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. ICP analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 53.25%, 19.97%, 13.06%, and 1.66%, respectively.

[0063] Using Al2O3 content as a standard (similar to Example 1), a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that 5 wt.% of powdered CaO with a particle size less than 0.2 mm was added to the ash slag as a flux, and 10 wt.% of CuO with a particle size less than 0.2 mm was added as a metal enriching agent. Ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0064] The mixture was fed into the same electric arc melting furnace as in Example 1, and heated using the electric effect. The reaction voltage was 380 V, the reaction current was 100 A, the melting time was 1 h, and the furnace temperature was maintained at approximately 1700°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 90.29%, O: 7.92%, Fe: 0.39%, Ca: 0.11%, Cr, Ni, Ba, Mg, etc.: 1.29%. Compared to Example 5, the metal enrichment was higher, but the reaction temperature and current were also higher.

[0065] Example 8

[0066] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0067] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 5 wt.% powdered CaO with a particle size less than 0.2 mm from the ash slag as a flux and adding 5 wt.% powdered CuO with a particle size less than 0.2 mm from the ash slag as a metal enriching agent and mixing them evenly was appropriate. Ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0068] The mixture was fed into the same electric arc melting furnace as in Example 1, and heated using the electric effect. The reaction voltage was 380 V, the reaction current was 100 A, the melting time was 1 h, and the furnace temperature was maintained at approximately 1700°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 87.32%, O: 9.51%, Fe: 0.27%, Ca: 0.16%, Si: 2.03%, Cr, Ni, Ba, Mg, etc.: 0.71%. Compared to Example 5, both the reaction temperature and current were higher.

[0069] Example 9

[0070] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0071] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 5 wt.% of powdered CaO with a particle size less than 0.2 mm to the ash slag was appropriate as a flux. Ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0072] The mixture was fed into the same electric arc melting furnace as in Example 1. The mixture was heated using the electric effect, with a reaction voltage of 380 V, a reaction current of 100 A, a melting time of 1 h, and the furnace temperature maintained at approximately 1700°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers inside the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 4.33%, O: 60.12%, Fe: 1.25%, Ca: 20.36%, Si: 13.20%, Cr, Ni, Ba, Mg, etc.: 0.74%.

[0073] Example 10

[0074] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0075] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 5 wt% of powdered CuO with a particle size less than 0.2 mm to the ash slag as a metal enriching agent and mixing it evenly was appropriate. The ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0076] The mixture was fed into the same electric arc melting furnace as in Example 1, and heated using the electric effect. The reaction voltage was 380V, the reaction current was 100A, the melting time was 1 hour, and the furnace temperature was maintained at approximately 1700°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 89.32%, O: 8.27%, Fe: 0.51%, Ca: 0.15%, Cr, Ni, Ba, Mg, etc.: 1.75%. Compared to Example 3, the metal enrichment was better, the reaction current was lower, but the ash melting temperature was higher.

[0077] Example 11

[0078] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 89.5% consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass percentages of SiO2, CaO, Al2O3, and CuO obtained from three tests were 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0079] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 20 wt% of powdered CuO with a particle size less than 0.2 mm to the ash slag as a metal enriching agent and mixing it evenly was appropriate. Ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0080] The mixture was fed into the same electric arc melting furnace as in Example 1, and heated using the electric effect. The reaction voltage was 380 V, the reaction current was 100 A, the melting time was 1 h, and the furnace temperature was maintained at approximately 1700°C. The reaction atmosphere was nitrogen, and the gas flow rate was 100 mL / min. The molten slag and metal separated into layers in the furnace. The lower metal layer was collected, and its composition was tested. By mass, the elemental distribution was as follows: Cu: 90.36%, O: 8.14%, Fe: 0.56%, Ca: 0.11%, Cr, Ni, Ba, Mg, etc.: 0.83%. Compared to Example 10, the CuO input was higher, but the parameters were similar.

[0081] Example 12

[0082] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 96% of it consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 49.80%, 11.17%, 8.84%, and 25.92%, respectively.

[0083] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 10 wt.% powdered CaO with a particle size less than 0.2 mm from the ash slag as a flux and 5 wt.% powdered CuO with a particle size less than 0.2 mm from the ash slag as a metal enriching agent, and mixing them evenly, was recommended. The ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0084] The mixture is fed to, for example Figure 2 The electric arc melting furnace shown utilizes the electro-effect to heat the mixture. The reaction voltage is 380 V, the reaction current is 100 A, the melting time is 1 h, and the furnace temperature is maintained at approximately 1700°C. The reaction atmosphere is nitrogen, and the gas flow rate is 100 mL / min. The molten slag and metal separate into layers within the furnace. The lower metal layer is collected, and its composition is tested. By mass, the elemental distribution is as follows: Cu: 91.33%, O: 7.99%, Fe: 0.21%, Ca: 0.10%, Cr, Ni, Ba, Mg, etc.: 0.37%. Compared to Example 2, the metal enrichment is slightly higher, but the reaction current and melting temperature are significantly increased.

[0085] Example 13

[0086] The ash residue from the crushing and gasification of recycled electronic waste was further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis of the ash powder revealed that, by mass, over 96% of it consisted of four oxides: SiO2, CaO, Al2O3, and CuO. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 49.80%, 11.17%, 8.84%, and 25.92%, respectively.

[0087] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, it was deduced that adding 5 wt.% of powdered CuO with a particle size less than 0.2 mm to the ash slag as a metal enriching agent and mixing it evenly was appropriate. Ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0088] The mixture is fed to, for example Figure 2 The electric arc melting furnace shown utilizes the electro-effect to heat the mixture. The reaction voltage is 380 V, the reaction current is 120 A, the melting time is 1 h, and the furnace temperature is maintained at approximately 1800°C. The reaction atmosphere is nitrogen, and the gas flow rate is 100 mL / min. The molten slag and metal separate into layers within the furnace. The lower metal layer is collected, and its composition is tested. By mass, the elemental distribution is as follows: Cu: 90.97%, O: 8.03%, Fe: 0.61%, Ca: 0.17%, Cr, Ni, Ba, Mg, etc.: 0.22%. Compared to Example 2, the metal enrichment is similar, but the reaction current and melting temperature are significantly increased.

[0089] Example 14

[0090] Two types of ash residue from the crushing and gasification of recycled electronic waste were further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis was used to determine the composition of the ash powder. Ash residue #1, by mass, consisted of over 96% SiO2, CaO, Al2O3, and CuO oxides. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 49.80%, 11.17%, 8.84%, and 25.92%, respectively. Ash residue #2, by mass, consisted of over 89.5% SiO2, CaO, Al2O3, and CuO oxides. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0091] Using Al2O3 content as a standard, a ternary phase diagram of SiO2, CaO, and CuO was established. Based on the phase diagram, the two types of ash were mixed uniformly at a mass ratio of 1:1. The ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0092] The mixture is fed to, for example Figure 2 The electric arc melting furnace shown utilizes the electro-effect to heat the mixture. The reaction voltage is 380 V, the reaction current is 80 A, the melting time is 1 h, and the furnace temperature is maintained at approximately 1600°C. The reaction atmosphere is nitrogen, and the gas flow rate is 100 mL / min. The molten slag and metal separate into layers inside the furnace. The lower metal layer is collected, and its composition is tested. By mass, the elemental distribution is as follows: Cu: 90.21%, O: 8.11%, Fe: 0.32%, Ca: 0.26%, Cr, Ni, Ba, Mg, etc.: 1.1%. The melting process is similar to that in Example 2.

[0093] Example 15

[0094] Two types of ash residue from the crushing and gasification of recycled electronic waste were further pulverized and sieved to obtain ash powder with a particle size of less than 0.2 mm. XRF analysis was used to determine the composition of the ash powder. Ash residue #1, by mass, consisted of over 96% SiO2, CaO, Al2O3, and CuO oxides. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 49.80%, 11.17%, 8.84%, and 25.92%, respectively. Ash residue #2, by mass, consisted of over 89.5% SiO2, CaO, Al2O3, and CuO oxides. The average mass content of SiO2, CaO, Al2O3, and CuO obtained from three tests was 55.25%, 20.08%, 12.89%, and 1.57%, respectively.

[0095] A ternary phase diagram of SiO2, CaO, and CuO was established using Al2O3 content as the standard. Based on the phase diagram, the two types of ash residues and 10 wt.% CaO were mixed uniformly. The ash flow temperature and viscosity-temperature curves of the mixture were tested, and the results are shown in Table 1.

[0096] The mixture is fed to, for example Figure 2The electric arc melting furnace shown utilizes the electro-effect to heat the mixture. The reaction voltage is 380V, the reaction current is 80A, the melting time is 1 hour, and the furnace temperature is maintained at approximately 1600°C. The reaction atmosphere is nitrogen, and the gas flow rate is 100mL / min. The molten slag and metal separate into layers within the furnace. The lower metal layer is collected, and its composition is tested. By mass, the elemental distribution is as follows: Cu: 90.75%, O: 8.11%, Fe: 0.21%, Ca: 0.45%, Cr, Ni, Ba, Mg, etc.: 0.50%. Compared to Example 14, the molten slag exhibits better fluidity at the same temperature.

[0097] The reaction conditions for Examples 1-15 are shown in Table 1.

[0098] Table 1 Reaction conditions for Examples 1-15

[0099] The above description of the embodiments is only for the purpose of helping to understand the technical solution and core idea of ​​the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

Claims

1. A method for promoting rapid melting and separation of metal components from multi-source resin gasification ash, characterized in that, Includes the following steps: (1) Composition determination: The composition of the ash residue from the multi-source resin gasification was determined; (2) Selection of flux-enriching agent: Based on the composition of the gasification ash of multi-source resin, select flux or a mixture of flux and enriching agent as flux-enriching agent, and adjust the mixing ratio of flux-enriching agent and the composition of multi-source resin gasification ash so that the flux-enriching agent reacts with the composition of multi-source resin gasification ash to generate low melting point compounds. (3) Electro-effect melting and separation reaction: The multi-source resin gasification ash and flux-enrichment agent are mixed, and the resulting mixture is heated and melted by electro-effect. After the mixture is completely melted and separated into layers, the lower layer metal is collected and recovered.

2. The method of claim 1, wherein, In step (1), the composition of the multi-source resin gasification ash and the mass fraction of each component are determined. The components include SiO2, Al2O3, CaO and CuO.

3. The method of claim 1, wherein, The fluxing agent mentioned in step (2) is selected from at least one of CaO, SiO2, K2O, Al2O3 and Na2O, and the enriching agent is selected from at least one of CuO, Cu2O and Cu.

4. The method according to claim 1 or 3, characterized in that, Step (2) involves adjusting the mixing ratio of flux-enriching agent and multi-source resin gasification ash, specifically including the following steps: (a) Determine the content of Al2O3 components; (b) Based on the Al2O3 content, a ternary phase diagram of CaO, SiO2 and CuO was established. The optimal ratio range of each component in the low-temperature eutectic region was determined using the ternary phase diagram to ensure that the mixture forms a low-viscosity melt with good fluidity in the range of 1100°C-1250°C. (c) Based on the actual composition fluctuations of ash and slag, the amount of flux-enriching agent added is determined by phase diagram boundary calibration.

5. The method according to claim 1 or 3, characterized in that, In step (2), the mixing ratio of the flux-enriching agent and the multi-source resin gasification ash is determined so that the final slag basicity is controlled at 1.0-1.4 and the CuO content accounts for more than 8 wt% of the mass of the multi-source resin gasification ash.

6. The method of claim 5, wherein, In step (c), the flux-enriching agent is CaO and / or CuO, and the amount of flux-enriching agent added is 5-20 wt% of the mass of the multi-source resin gasification ash.

7. The method according to claim 1 or 3, characterized in that, In step (3), the mixture is placed in an electro-effect melting device, and the mixture is energized by the metal-rich conductivity of the mixture, and the mixture is melted by the heat effect generated by the energization.

8. The method of claim 7, wherein, The electro-effect melting device is an electric arc / resistance melting furnace. During the melting process, an inert gas is introduced into the electric arc / resistance melting furnace. After the mixture melts, it separates into layers due to density differences. The lower layer of molten metal is then removed to achieve enrichment and separation.

9. The method of claim 8, wherein, The inert gas is high-purity nitrogen or high-purity argon.

10. The method of claim 7, wherein, The reaction conditions for the electric arc / resistance melting furnace are: reaction voltage 380 V, reaction current 80-120 A, melting time 20-60 min, and furnace temperature 1500°C-1800°C.