A Short-Process Manufacturing Method for High-Performance 8021 Aluminum Foil Without Mid-Process Removal
By using hot rolling self-annealing and online cleaning technology, the problem of functional conflict between intermediate annealing and finished product annealing in aluminum foil production has been solved, resulting in shorter aluminum foil production cycle, increased elongation, improved surface quality, and maintained tensile strength. This solves the production efficiency and quality problems existing in the prior art.
Patent Information
- Application Number
- CN202611593289.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-15
- Publication Date
- 2026-11-17
AI Technical Summary
The existing aluminum foil production process has a conflict between intermediate annealing and finished product annealing functions, resulting in long production cycles, low elongation, insufficient tensile strength and poor surface quality, and failing to effectively unlock the window for short process optimization.
Hot rolling self-annealing is used to replace intermediate annealing, and degreasing is performed before online cleaning. Through efficient hot rolling self-annealing and online cleaning technology, short-term recrystallization of finished product annealing is achieved, eliminating intermediate annealing to shorten the production cycle, improve elongation and tensile strength, and improve surface quality.
It achieves a reduction of more than 30 hours in aluminum foil production cycle, a 0° elongation rate no lower than that of conventional processes, a lower yield strength ratio, a tensile strength maintained at 100-120MPa, and a surface free of oil spots and black oil. It improves process controllability and high elongation, while taking into account both high puncture resistance and surface quality.
Smart Images

Figure CN123108340A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum foil production technology, specifically to a short-process manufacturing method for high-performance 8021 aluminum foil without intermediate removal. Background Technology
[0002] Aluminum foil for lithium-ion battery pouch aluminum-plastic film is a key substrate for the outer packaging of pouch batteries. The finished product thickness is typically 0.040–0.050 mm, with 8021 grade being the main type. Its Fe content is 1.2–1.7 wt%, and Si content is no more than 0.15 wt%. Currently, downstream applications urgently require improved tensile strength and high elongation of aluminum foil due to the puncture resistance requirements of the products.
[0003] The current mainstream process is as follows: melting and casting, homogenization, hot rolling, cold rolling to intermediate thickness, intermediate annealing, secondary cold rolling, foil rolling, and finished product annealing. This process has two inherent contradictions that are mutually restrictive.
[0004] Firstly, intermediate annealing is the only means to complete recrystallization resetting. The role of intermediate annealing is to interrupt the accumulation of cold deformation, eliminate work hardening, and reset the texture. The greater the amount of cold deformation, the stronger the rolling texture components such as Cu, S, and Bs. If it is not interrupted midway, recrystallization textures such as Cube and Goss are difficult to nucleate, and a large amount of deformed structure remains after the finished product is annealed. Therefore, the publicly disclosed 8021 aluminum-plastic film foil preparation process generally retains intermediate annealing or equivalent steps. For example, in a method for preparing 8021 aluminum alloy foil for high stamping performance lithium battery soft packs, intermediate annealing is set after cold rolling to an intermediate thickness, and a second cold rolling to 0.24-0.28 mm is required after intermediate annealing; a method for controlling the anisotropy of lithium battery aluminum-plastic film foil includes a complete intermediate annealing step; another process involves intermediate annealing at 365℃ for 3 h at a thickness of 0.5 mm, or intermediate annealing at 260-300℃ for 1-4 h.
[0005] Whether eliminating intermediate annealing, i.e., the so-called direct rolling or short-process route, is feasible has been proven wrong by existing trial production. The inventors of this application, in the early trial production at Southwest Aluminum, arranged two processes without intermediate annealing: one without intermediate annealing, and the other without intermediate annealing but with the hot-rolling temperature increased to 360℃, both of which retained a large amount of cold-rolled deformed microstructure. While the direct rolling process significantly improved tensile strength, achieving the highest yield strength among all processes, its elongation in the 0° direction was poor, and its yield strength ratio, reaching 0.62–0.69, was the highest among all processes, exhibiting the weakest work hardening ability.
[0006] Secondly, finished product annealing is forced to simultaneously perform both degreasing and softening tasks, thus requiring a low-temperature, long-time process, which in turn damages the elongation. After foil rolling, residual rolling oil remains on the foil surface, and finished product annealing must simultaneously remove this oil. Degreasing relies on oil volatilization or pyrolysis, but excessively high temperatures can cause oil cracking, resulting in yellow spots, oil stickiness, and interlayer adhesion. Therefore, a low-temperature, long-time strategy is commonly adopted. Existing literature records that most aluminum foil manufacturers, both domestically and internationally, use low-temperature, long-time annealing processes, prioritizing the lowest possible temperature while ensuring effective degreasing, without considering whether the aluminum foil has fully recrystallized, resulting in incomplete recrystallization annealing and ultimately low product elongation. Commercial degreasing annealing also uses metal temperatures of 250–300℃ and holding times of 30–60 h. The applicant's trial production process also uses 245℃×35 h and 225℃×35 h. Laboratory annealing results showed that prolonged holding time reduced elongation, with holding times of 10 h and 5 h yielding better elongation than holding times of 35 h. The study also indicated that when the annealing temperature increased from 240℃ to 360℃, the Al-Fe-Si foil grains grew from approximately 5.2 μm to approximately 9.6 μm. Above 300℃, grain agglomeration intensified, and the elongation decreased with increasing annealing temperature.
[0007] This leads to the following cycle: to remove oil, the temperature must be lowered and the holding time extended. Although prolonged holding completes the oil removal, it causes grain growth, texture deterioration, and a decrease in elongation. If the temperature is increased to improve recrystallization, oil spots and adhesion will occur. The conflict between the requirements for oil removal and the requirements for microstructure control within the same process is a structural contradiction that has long remained unresolved in this field.
[0008] Existing attempts at improvement have not addressed this contradiction. Firstly, using a furnace cover for external insulation, maintaining the temperature at 210℃ for 50–90 hours before moving to external insulation, still results in a total cycle of 60–100 hours. Secondly, introducing ozone into the annealing furnace to enhance degreasing can shorten the time by approximately 30%, but requires additional ozone generation and safety protection measures, and remains a long-term process. Thirdly, blowing residual oil onto the foil surface with hot air before annealing can reduce the total annealing time by 15–25 hours, but this is only gaseous blowing, with limited ability to remove the oil film adhering to the foil surface, resulting in a long annealing time. Fourthly, using oil-absorbing paper to absorb oil, followed by hot water washing and hot air drying before annealing, still requires a prolonged low-temperature degreasing process at 160–230℃ before annealing, thus lengthening the total cycle. Fifth, the temperature rise in the deformation zones of roughing and intermediate rolling is used to raise the metal temperature to 200-300℃, which is equivalent to an intermediate recovery annealing. However, this temperature rise is a local recovery in the foil rolling section and cannot reset the hot-rolled genetic structure. Sixth, a short process of continuous casting and rolling is used to produce 8021 container foil without intermediate annealing. However, the finished product annealing is still 220℃ negative pressure for 4 hours followed by 285℃ positive pressure for 25-35 hours, retaining a low-temperature degreasing section. The total cycle is more than 30 hours, and the product is a high-strength container foil with a tensile strength of 150-160 MPa, with an elongation requirement of not less than 15%.
[0009] In summary, there are two unresolved issues in this field: First, no one has moved the recrystallization reset function from the intermediate annealing process to the hot rolling process. After the intermediate annealing is eliminated, the microstructure of the hot-rolled plate is considered a predetermined input, and it can only be passively improved by increasing the final hot rolling temperature, but this method has been proven ineffective. Second, no one has separated the degreasing function from the finished product annealing. Existing pre-degreasing solutions all retain the low-temperature degreasing section in the furnace as a fallback, and the total cycle cannot be truly compressed, thus failing to unlock the microstructure optimization window of short-time recrystallization. Summary of the Invention
[0010] The technical problem to be solved by this invention is to overcome the existing defects and provide a high-performance 8021 aluminum foil manufacturing method without intermediate annealing. By replacing intermediate annealing with hot rolling self-annealing and online cleaning and pre-degreasing, the finished product annealing only completes short-term recrystallization. Under the short process of eliminating intermediate annealing, the cycle time is shortened by more than 30 hours, the 0° elongation is not lower than that of conventional processes, the yield strength ratio is reduced, the tensile strength is maintained at 100-120MPa, and the surface is free of oil spots and black oil. At the same time, the process controllability is improved, and high elongation, high puncture resistance and surface quality are taken into account. This can effectively solve the problems in the background technology.
[0011] To achieve the above objectives, the present invention provides the following technical solution: a short-process manufacturing method for high-performance 8021 aluminum foil without intermediate removal, comprising the following steps: S1. Casting: The composition by mass percentage is as follows: Si: 0.05-0.12%, Fe: 1.35-1.60%, Cu: ≤0.02%, Mn: 0.015-0.035%, Mg: ≤0.02%, Zn: ≤0.03%, Cr: ≤0.01%, Ti: 0.018-0.030%, with the balance being Al and unavoidable impurities, wherein no single unavoidable impurity exceeds 0.03%, and the total unavoidable impurities exceed 0.15%. S2. Homogenization: Hold at 600-620℃ for 8-12 h, then cool in the furnace to 480-530℃ before starting rolling; S3, Hot rolling: hot rolled to 3.8-4.5 mm in 13-16 passes, with a final hot rolling temperature of 350-375℃; S4. Hot-rolled self-annealing: After hot rolling, the hot-rolled coil is held in the temperature range of 350-365℃ for 2-8 hours, and then slowly cooled to below 200℃ at an average rate of no more than 25℃ / h; so that the recrystallization volume fraction of the hot-rolled plate is not less than 75%, the difference between the recrystallization volume fraction of the surface layer and the core layer is not greater than 8%, and the electrical conductivity of the hot-rolled plate is not less than 58.5% IACS and is not less than 1.0% IACS higher than that of the comparative hot-rolled plate in the same melting cycle without the aforementioned holding; S5. Cold rolling: The thickness is continuously cold rolled from hot rolling to 0.25-0.30 mm through multiple passes, the total cold rolling deformation rate is not less than 92%, and no intermediate annealing is performed in the entire cold rolling process; S6. Foil rolling: Foil is rolled to a finished thickness of 0.040–0.050 mm; S7. Online cleaning: After foil rolling and before finished product annealing, the foil is continuously cleaned with cleaning agent, squeezed dry, and hot air dried before being wound up, so that the residual oil on the foil surface before entering the furnace is no more than 20 mg / m²; the winding adopts a tension gradient that decreases from the inner layer to the outer layer. S8. Finished product annealing: The cleaned foil roll is continuously heated to a metal temperature of 240-275°C at an average heating rate of not less than 30°C / h, held at that temperature for 4-8 hours, and then cooled; no heat-holding platform below 200°C is set up during the entire finished product annealing process.
[0012] In a preferred embodiment of the present invention, in step S4, the temperature at which the residence takes place is 350–360°C and the time is 3–6 hours.
[0013] As a preferred embodiment of the present invention, in S4, the average grain size of the hot-rolled plate is 20-30 μm; the residual heat after hot rolling is utilized: the hot-rolled coil is stacked in a heat preservation cover, allowing it to cool down naturally from the coiling temperature and be maintained in the temperature range of 350-365°C for 2-8 hours.
[0014] As a preferred embodiment of the present invention, in step S5, the total cold rolling deformation rate is 93% to 94%, and the cumulative deformation rate of steps S5 and S6 is not less than 98%.
[0015] As a preferred embodiment of the present invention, in S7, the cleaning agent is a low-boiling-range cleaning agent with a distillation range not exceeding 190°C, the cleaning agent temperature is 40-60°C, and the contact time with the foil surface is not less than 3 seconds.
[0016] As a preferred embodiment of the present invention, in S7, the squeezing is performed using a combination of squeezing rollers and air knives, with the air knife pressure being 0.2 to 0.5 MPa; and the hot air drying temperature being 80 to 120°C.
[0017] As a preferred embodiment of the present invention, in S7, the decreasing tension gradient is 45 N / mm from the inner layer. 2 Decrease to 25 N / mm for the outer layer 2 The residual oil content on the foil surface before entering the furnace should not exceed 10 mg / m². 2 Furthermore, the surface dyne value is not less than 34 mN / m.
[0018] As a preferred technical solution of the present invention, in S8, the metal temperature is 250-265°C and the holding time is 3-6 hours; after S8, the foil roll is taken out of the furnace and cooled to below 150°C and then naturally cooled to room temperature.
[0019] As a preferred embodiment of the present invention, in S3, the hot rolling is performed in 13 passes, hot rolling to 4.1 mm, and the final hot rolling temperature is 360°C.
[0020] A high elongation lithium battery aluminum-plastic film using 8021 aluminum foil, wherein the aluminum foil has a thickness of 0.040 to 0.050 mm, an elongation of not less than 22% along the rolling direction at 0°, a tensile strength of 100 to 120 MPa, a yield strength ratio of not more than 0.55, and an average grain size of not more than 9 μm.
[0021] Compared with the prior art, the beneficial effects of the present invention are: 1. The high-performance 8021 aluminum foil manufacturing method without intermediate annealing of the present invention shortens the manufacturing cycle: by eliminating intermediate annealing, a heat treatment of 320-360℃ for about 3-20 hours and its logistics turnover can be saved, and the finished product annealing is shortened from 35 hours to 2-8 hours, and the cycle per batch is shortened by more than 30 hours in total, while reducing furnace occupation and energy consumption.
[0022] 2. The high-performance 8021 aluminum foil manufacturing method without intermediate annealing in this invention improves the elongation in the 0° direction: hot rolling self-annealing allows the hot-rolled plate to enter the cold rolling process with a fully recrystallized structure and eliminates the solute drag of solid Fe. Combined with short-time heat preservation to suppress grain growth, the elongation in the 0° direction is still not lower than that of conventional processes even without intermediate annealing, and the yield strength ratio decreases from 0.62 to 0.69.
[0023] 3. The high-performance 8021 aluminum foil manufacturing method without intermediate rolling in this invention retains its strength: the high energy storage characteristics of the direct rolling route without intermediate rolling maintain the tensile strength at a high level.
[0024] 4. The high-performance 8021 aluminum foil manufacturing method without intermediate annealing in this invention improves surface quality: the degreasing process is changed from in-furnace pyrolysis to online cleaning, which avoids the formation of carbon residue by cracking of oil in the furnace from the source, and can eliminate annealing oil spots and surface black oil defects.
[0025] 5. The high-performance 8021 aluminum foil manufacturing method without intermediate stripping in this invention improves process controllability: by using electrical conductivity as the criterion for the degree of hot rolling precipitation, the original lag control that relied on metallographic sampling can be changed to online closed-loop control. Attached Figure Description
[0026] Figure 1 This is a process flow diagram of the present invention; Detailed Implementation
[0027] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0028] A short-process manufacturing method for high-performance 8021 aluminum foil without intermediate removal includes the following steps: S1, Casting: The composition by mass percentage is as follows: Si: 0.05-0.12%, Fe: 1.35-1.60%, Cu: ≤0.02%, Mn: 0.015-0.035%, Mg: ≤0.02%, Zn: ≤0.03%, Cr: ≤0.01%, Ti: 0.018-0.030%, with the balance being Al and unavoidable impurities, wherein no single unavoidable impurity exceeds 0.03%, and the total unavoidable impurities do not exceed 0.15%. The reason for tightening the upper limit of Cu to 0.02 is that the process of adding Cu in the trial production significantly increased the rolling texture of Cu, S, etc., inhibited the development of Cube and Goss recrystallization textures, and resulted in a low proportion of large-angle grain boundaries; while reducing Cu to 0.007 significantly improved the microstructure. S2. Homogenization: Hold at 600-620℃ for 8-12 hours, then cool in the furnace to 500-530℃ before starting rolling; S3. Hot rolling: 13-15 passes of hot rolling to 3.8-4.5 mm, with a final hot rolling temperature of 350-375℃; the number of roughing passes is reduced from the conventional 15 to 13 and the initial rolling temperature is increased, which can increase the deformation per pass, shorten the rolling time, and improve the temperature uniformity of the hot-rolled plate. In the trial production, it has been observed that the finished grain size is refined to the 8-10 μm level. S4. Hot-rolled self-annealing: After hot rolling, the hot-rolled coil is held in the temperature range of 330-365℃ for 2-8 hours, and then slowly cooled to below 200℃ at an average rate of no more than 25℃ / h. This step must simultaneously meet two criteria: First, the recrystallization volume fraction of the hot-rolled plate is not less than 75%, and the difference between the recrystallization volume fraction of the surface layer and the core layer is not greater than 8%; Second, the electrical conductivity of the hot-rolled plate is not less than 58.5% IACS and is at least 1.0% higher than that of the comparative hot-rolled plate in the same melting cycle without the aforementioned holding. The mechanism of this step is as follows: the Fe content of 8021 alloy is as high as about 1.5%, and a large amount of Fe is in a solid solution state at the high temperature of hot rolling. Solid solution Fe not only produces solid solution strengthening and improves deformation resistance, but more importantly, the solute atoms drag grain boundary migration, inhibiting subsequent recrystallization nucleation and growth, and raising the recrystallization temperature. Increasing the hot final rolling temperature only increases the amount of solid solution without providing precipitation time, thus resulting in even higher solid solution Fe. In the trial production, the applicant increased the hot final rolling temperature to 360℃ (the highest among all processes) but did not implement hot rolling self-annealing. The result was that a large amount of cold-rolled deformed structure was still retained, and the yield strength ratio was as high as 0.62–0.69. The reason is this: the final rolling temperature was increased, but no time window was provided for Fe precipitation. Therefore, the variable controlled in this step is the high-temperature residence time after final rolling and the resulting degree of solid solution Fe precipitation, rather than the final rolling temperature.
[0029] The rationale for choosing electrical conductivity as the criterion for precipitation degree is as follows: Solid-solution alloying elements significantly reduce electrical conductivity, while precipitation causes conductivity to rebound, and the two are monotonically correlated. Furthermore, electrical conductivity can be measured online, non-destructively, and within seconds using an eddy current analyzer. Therefore, this criterion can be directly applied to the closed-loop control of hot rolling lines without waiting for metallographic or chemical analysis results. The purpose of the slow cooling section is to prevent rapid cooling from refreezing the precipitated Fe back into the solid-solution state.
[0030] S5. Cold rolling: The thickness is continuously cold rolled from hot-rolled thickness to 0.25-0.30 mm through multiple passes, with a total cold rolling deformation rate of not less than 92%, and no intermediate annealing is performed during the entire cold rolling process; due to the elimination of intermediate annealing, the effective cumulative deformation rate before finished product annealing is the total deformation from hot-rolled thickness to finished product thickness, which is about 98.9% when hot-rolled from 4.1 mm to finished product thickness of 0.045 mm, higher than the approximately 94.7% of the foil rolling section after intermediate annealing in the intermediate annealing route. This high energy storage is the energy storage basis for the kinetics of short-time annealing.
[0031] S6. Foil Rolling: Foil is rolled to a finished thickness of 0.040–0.050 mm, with a deformation rate of 80%–88% in the rolled section; S7. Online Cleaning: After foil rolling and before finished product annealing, the foil is continuously cleaned with a cleaning agent, squeezed dry, and hot-air dried before being wound up, ensuring that the residual oil content on the foil surface before entering the furnace is no more than 20 mg / m². The cleaning agent is a low-boiling-range cleaning agent with a distillation range not exceeding 190℃, the cleaning agent temperature is 40–60℃, and the contact time with the foil surface is no less than 3 seconds. Squeezing is performed using a combination of squeeze rollers and air knives, with an air knife pressure of 0.2–0.5 MPa. The hot-air drying temperature is 80–120℃. The winding adopts a tension gradient that decreases from the inner layer to the outer layer; preferably 45 N / mm from the inner layer. 2 Decrease to 25 N / mm for the outer layer 2 The residual oil content on the foil surface before entering the furnace should not exceed 10 mg / m². 2 And the surface dyne value is not less than 34 mN / m; Setting a decreasing tension gradient is to address interlayer adhesion: after the oil film on the foil surface is removed, the interlayer insulation of the foil is lost during annealing, posing a risk of adhesion. This is one of the practical reasons why existing pre-degreasing schemes always retain a low-temperature degreasing section in the furnace. Gradient winding with low tension on the outer layer and high tension on the inner layer allows the interlayer compressive stress generated by thermal expansion at high temperatures to decrease from the outside to the inside, thereby suppressing adhesion without relying on oil film isolation. Therefore, this feature is a necessary technical means rather than an optional optimization.
[0032] S8. Finished product annealing: The cleaned foil roll is continuously heated to a metal temperature of 240-275°C at an average heating rate of not less than 30°C / h, held for 2-8 hours and then cooled; it is taken out of the furnace and cooled to below 150°C and then naturally cooled to room temperature; no holding platform below 200°C is set in the entire annealing process, nor is an intermediate platform for heating and cooling set.
[0033] The annealing temperature was chosen in the medium range rather than higher for two reasons: First, the elongation after holding at this temperature for 35 hours in the trial production was lower than that after holding for 5–10 hours; second, when the annealing temperature increased from 240℃ to 360℃, the grain size increased from approximately 5.2 μm to approximately 9.6 μm, and grain agglomeration intensified significantly above 300℃, with the elongation in the 0° direction decreasing as the annealing temperature increased. The objective of this application is to minimize the high-temperature dwell time while ensuring complete recrystallization, rather than trading time for higher temperatures.
[0034] A high elongation lithium battery aluminum-plastic film using 8021 aluminum foil, wherein the aluminum foil has a thickness of 0.040 to 0.050 mm, an elongation of not less than 22% along the rolling direction at 0°, a tensile strength of 100 to 120 MPa, a yield strength ratio of not more than 0.55, and an average grain size of not more than 9 μm.
[0035] Example 1: A short-process manufacturing method for high-performance 8021 aluminum foil without intermediate removal, comprising the following steps: S1, casting: The composition by mass percentage is: Si: 0.067%, Fe: 1.522%, Cu: ≤0.007%, Mn: 0.023%, Mg: ≤0.008%, Ti: 0.023%, with the balance being Al and unavoidable impurities; S2. Homogenization: Hold at 610℃ for 9 hours, then cool in the furnace to 520℃ before starting rolling. S3, Hot rolling: hot rolled to 4.1mm in 13 passes, with a final hot rolling temperature of 360℃; S4. Hot-rolled self-annealing: After hot rolling, the hot-rolled coil is held at 350°C for 4 hours, and then slowly cooled to below 200°C at an average rate of no more than 25°C / h. This step must simultaneously meet two criteria: First, the recrystallization volume fraction of the hot-rolled plate is not less than 90%, the difference between the recrystallization volume fraction of the surface layer and the core layer is not greater than 8%, and the average grain size is 20-45μm; Second, the electrical conductivity of the hot-rolled plate is not less than 58.5%IACS and is at least 1.0%IACS higher than that of the comparative hot-rolled plate in the same melting cycle without the aforementioned holding. S5, Cold rolling: The total deformation rate of cold rolling from the hot-rolled thickness to 4.1-1.7-0.85-0.48-0.30mm is 92.7%, and no intermediate annealing is performed in the entire cold rolling process; S6. Foil Rolling: Foil is rolled to a finished thickness of 0.045mm, with a foil rolling section deformation rate of 85% and a cumulative deformation rate of 98.9%. S7. Online Cleaning: After foil rolling and before finished product annealing, the foil is continuously cleaned with a cleaning agent, squeezed dry, and hot-air dried before being wound up, so that the residual oil content on the foil surface before entering the furnace is no more than 20 mg / m²; the cleaning agent is a low-boiling-range cleaning agent with a distillation range not exceeding 190℃, the cleaning agent temperature is 45℃, and the contact time with the foil surface is 5s; the squeezing is carried out by a combination of squeezing rollers and air knives, and the air knife pressure is 0.35MPa; the hot air drying temperature is 100℃; the winding adopts a tension gradient that decreases from the inner layer to the outer layer; the tension decreases from 45 N / mm² to 25 N / mm² during winding. S8. Finished product annealing: The cleaned foil roll is continuously heated to a metal temperature of 260°C at an average heating rate of 30°C / h, held at that temperature for 5 hours and then cooled; after being taken out of the furnace, it is cooled to below 150°C and then naturally cooled to room temperature.
[0036] Finished product properties: tensile strength 95~105 MPa, elongation in the 0° direction ≥22%, yield strength ratio ≤0.55.
[0037] Example 2 differs from Example 1 in that: hot rolling to 3.8 mm with a final hot rolling temperature of 340℃; hot rolling self-annealing at 330℃ for 8 hours, followed by slow cooling to 200℃; cold rolling to 0.30 mm with a total cold rolling deformation rate of 92.1%, without intermediate annealing; foil rolling to 0.050 mm with a foil section deformation rate of 83.3% and a cumulative deformation rate of 98.7%; residual oil content before furnace entry after online cleaning not exceeding 10 mg / m²; finished product annealing with a heating rate of 30℃ / h to a metal temperature of 240℃, holding for 8 hours, without a low-temperature holding platform.
[0038] Example 3: The difference from Example 1 is as follows: hot rolling to 4.5 mm, hot final rolling temperature 375℃; hot rolling self-annealing at 365℃ for 2 h, slow cooling to 200℃; cold rolling to 0.25 mm, total cold rolling deformation rate 94.4%, no intermediate annealing; foil rolling to 0.040 mm, foil rolling segment deformation rate 84.0%, cumulative deformation rate 99.1%; residual oil content before entering the furnace after online cleaning is no more than 10 mg / m²; finished product annealing is carried out at 30℃ / h to a metal temperature of 275℃, held for 2 h, no low-temperature holding platform is set.
[0039] Comparative Example 1: The composition, homogenization, and hot rolling parameters were the same as in Example 1, but the hot-rolled coil was directly air-cooled without hot-rolled self-annealing; it was cold-rolled to 0.30 mm without intermediate annealing; the foil was rolled to 0.045 mm; the finished product was annealed according to the conventional process of holding at 245℃ for 35 h, including a long period of low temperature. Results: The yield strength ratio of the finished product was 0.62–0.69, the elongation was poor, and the yield strength was the highest among all processes. This comparative example shows that simply increasing the hot-rolling temperature without providing a precipitation time window cannot improve the recrystallization sufficiency of the non-intermediate annealing route.
[0040] Comparative Example 2: Hot rolling self-annealing and direct rolling without intermediate annealing were implemented, but online cleaning was omitted, and the finished product annealing was still performed at 245℃ for 35 hours. Result: Due to the excessively long holding time, grain growth occurred, and the elongation was lower than in Example 1. This comparative example illustrates that the short-time system cannot be activated when the degreasing task is not removed during annealing.
[0041] Comparative Example 3: Hot-rolled self-annealing, direct rolling without intermediate annealing, and online cleaning were all the same as in Example 1, except that the finished product annealing was changed to a holding time of 320℃ for 5 hours. Results: Grain growth reached over 9 μm, and the elongation in the 0° direction was lower than in Example 1. This comparative example illustrates that complete recrystallization should be achieved by shortening the high-temperature dwell time rather than increasing the annealing temperature.
[0042] Comparative Example 4: Conventional intermediate annealing process: cold rolling to 0.85 mm, intermediate annealing at 320℃, foil rolling to 0.045 mm, holding at 245℃ for 35 h. This serves as the elongation benchmark.
[0043] All parts not disclosed in this invention are prior art, and their specific structures, materials, and working principles will not be described in detail. Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions, and variations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A short-process manufacturing method for high-performance 8021 aluminum foil without intermediate removal, characterized in that, Includes the following steps: S1. Casting: The composition by mass percentage is as follows: Si: 0.05-0.12%, Fe: 1.35-1.60%, Cu: ≤0.02%, Mn: 0.015-0.035%, Mg: ≤0.02%, Zn: ≤0.03%, Cr: ≤0.01%, Ti: 0.018-0.030%, with the balance being Al and unavoidable impurities, wherein no single unavoidable impurity exceeds 0.03%, and the total unavoidable impurities exceed 0.15%. S2. Homogenization: Hold at 600-620℃ for 8-12 h, then cool in the furnace to 480-530℃ before starting rolling; S3, Hot rolling: hot rolled to 3.8-4.5 mm in 13-16 passes, with a final hot rolling temperature of 350-375℃; S4. Hot-rolled self-annealing: After hot rolling, the hot-rolled coil is held in the temperature range of 350-365℃ for 2-8 hours, and then slowly cooled to below 200℃ at an average rate of no more than 25℃ / h; so that the recrystallization volume fraction of the hot-rolled plate is not less than 75%, the difference between the recrystallization volume fraction of the surface layer and the core layer is not greater than 8%, and the electrical conductivity of the hot-rolled plate is not less than 58.5% IACS and is not less than 1.0% IACS higher than that of the comparative hot-rolled plate in the same melting cycle without the aforementioned holding; S5. Cold rolling: The thickness is continuously cold rolled from hot rolling to 0.25-0.30 mm through multiple passes, the total cold rolling deformation rate is not less than 92%, and no intermediate annealing is performed in the entire cold rolling process; S6. Foil rolling: Foil is rolled to a finished thickness of 0.040–0.050 mm; S7. Online cleaning: After foil rolling and before finished product annealing, the foil is continuously cleaned with cleaning agent, squeezed dry, and hot air dried before being wound up, so that the residual oil on the foil surface before entering the furnace is no more than 20 mg / m²; the winding adopts a tension gradient that decreases from the inner layer to the outer layer. S8. Finished product annealing: The cleaned foil roll is continuously heated to a metal temperature of 240-275°C at an average heating rate of not less than 30°C / h, held at that temperature for 4-8 hours, and then cooled; no heat-holding platform below 200°C is set up during the entire finished product annealing process.
2. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S4, the temperature is 350–360℃ and the time is 3–6 h.
3. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S4, the average grain size of the hot-rolled plate is 20-30 μm; the residual heat after hot rolling is utilized: the hot-rolled coils are stacked in a heat insulation cover, allowing them to cool down naturally from the coiling temperature and be maintained in the temperature range of 350-365°C for 2-8 hours.
4. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S5, the total cold rolling deformation rate is 93% to 94%, and the cumulative deformation rate between steps S5 and S6 is not less than 98%.
5. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S7, the cleaning agent is a low-boiling-range cleaning agent with a distillation range not exceeding 190℃, the cleaning agent temperature is 40~60℃, and the contact time with the foil surface is not less than 3s.
6. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S7, the squeezing process uses a combination of squeezing rollers and air knives, with an air knife pressure of 0.2–0.5 MPa; the hot air drying temperature is 80–120℃.
7. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S7, the decreasing tension gradient is 45 N / mm from the inner layer. 2 Decrease to 25 N / mm for the outer layer 2 The residual oil content on the foil surface before entering the furnace should not exceed 10 mg / m². 2 Furthermore, the surface dyne value is not less than 34 mN / m.
8. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S8, the metal temperature is 250-265℃ and the holding time is 3-6 h; after S8, the foil roll is taken out of the furnace and cooled to below 150℃ and then naturally cooled to room temperature.
9. The high-performance 8021 aluminum foil manufacturing method without intermediate removal and with a short process according to claim 1, characterized in that: In S3, hot rolling is performed in 13 passes, hot rolling to 4.1 mm, and the final hot rolling temperature is 360℃.
10. A high-elongation lithium battery aluminum-plastic film made of 8021 aluminum foil, manufactured using the high-performance 8021 aluminum foil manufacturing method without intermediate removal process as described in any one of claims 1 to 9, characterized in that: The aluminum foil has a thickness of 0.040 to 0.050 mm, an elongation of not less than 22% along the rolling direction at 0°, a tensile strength of 100 to 120 MPa, a yield strength ratio of not more than 0.55, and an average grain size of not more than 9 μm.