Application of a Zr-Ti high-entropy alloy in grain refinement and anti-poisoning of aluminum alloys

By adsorbing and regulating Mn and Fe impurities in 3003 aluminum alloy using Zr-Ti high-entropy alloy refiner, a C15-Laves phase is formed, which solves the problems of easy poisoning and brittle phase control in the modification of 3003 aluminum alloy. This achieves efficient refinement and low-damage modification, and improves the microstructure uniformity and cold working performance of the aluminum alloy.

CN123108342APending Publication Date: 2026-11-17ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611430367.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing 3003 aluminum alloy modification technologies are prone to poisoning, the matrix is ​​easily poisoned, the brittle manganese phase is difficult to control, the cold working structure has poor stability, and the performance fluctuates greatly, which cannot meet the needs of high-end applications.

Method used

Using Zr-Ti high-entropy alloy as a grain refiner, the Ti element adsorbs Mn and Fe impurities, and the Zr element regulates the phase precipitation behavior to form a C15-Laves phase, which provides a high-density nucleation core, inhibits the formation of brittle phases, and achieves anti-poisoning refinement and low matrix damage.

Benefits of technology

It significantly improves the grain uniformity and density of aluminum alloys, eliminates coarse dendrites, improves plasticity and cold working performance, enhances the forming ability and stability of materials, and is suitable for high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108342A_ABST
    Figure CN123108342A_ABST
Patent Text Reader

Abstract

This invention relates to the field of wrought aluminum alloy modification and metal material strengthening technology, specifically to the application of a Zr-Ti high-entropy alloy in aluminum alloy grain refinement and anti-poisoning, wherein the Zr-Ti high-entropy alloy is Ti x Zr 1‑x Cr 0.1 V 0.8 Fe 0.1 Where x = 0.1~0.3, the amount of Zr-Ti high-entropy alloy added is 0.5wt.%~1.5wt.% of the total mass of aluminum alloy; by applying this high-entropy alloy to the grain refinement and anti-poisoning of aluminum alloy, the problems of easy poisoning during grain refinement, easy poisoning of the matrix, difficulty in controlling the brittle manganese phase, poor stability of cold working structure, and large performance fluctuation of existing 3003 aluminum alloy modification technology are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wrought aluminum alloy modification and metal material strengthening technology, specifically to the application of a Zr-Ti high-entropy alloy in aluminum alloy grain refinement and anti-poisoning. Background Technology

[0002] As the most widely used non-heat-treatable rust-resistant aluminum alloy, the comprehensive performance of 3003 aluminum-manganese alloy depends entirely on the as-cast grain structure and the distribution of the second phase. There are no subsequent heat treatment reinforcement methods. Therefore, as-cast structure control, grain refinement, and brittle phase modification are the only core ways to improve its formability and service stability.

[0003] Existing industrial refining and modification technologies have many inherent defects: traditional AlTiB refining agents are prone to poisoning reactions in 3003 aluminum melt containing Mn and Fe. Mn and Fe impurity atoms are adsorbed on the surface of TiB2 and TiAl3 nucleation particles, covering the active nucleation sites, resulting in rapid failure of the refining agent, repeated coarsening of grains, and large batch performance dispersion.

[0004] Existing rare earth and single alloy modification technologies, while achieving a certain degree of grain refinement, generally suffer from modification imbalance: the refinement process easily induces intermetallic compound segregation and grain boundary embrittlement, sacrificing alloy plasticity while refining grains and producing significant matrix poisoning effects, making them unsuitable for the precision cold stamping and ultra-thin rolling forming requirements of 3003 aluminum alloy. Furthermore, existing technologies cannot effectively modify the inherent coarse Al6Mn brittle phase of 3003 alloy. This phase, distributed in coarse and irregular blocks, severely disrupts the matrix and is the core cause of cold working cracking and insufficient toughness in the material.

[0005] Existing publicly available modification technologies cannot specifically address the issues of Mn phase deterioration, refinement poisoning, and matrix poisoning in 3003 aluminum-manganese alloys. Currently, the industry lacks a dedicated high-entropy modification technology for 3003 non-heat-treatable aluminum alloys that combines anti-poisoning refinement, low matrix damage, harmless modification of brittle phases, and stable cold-working microstructure.

[0006] Therefore, developing a Zr-Ti synergistic, anti-poisoning, low-toxicity, and long-term stable high-entropy alloy modification method is of great engineering value and industrial significance for optimizing the microstructure of 3003 aluminum alloy, improving its cold working performance, and expanding its high-end application scenarios.

[0007] In view of the above-mentioned defects, the inventors of this invention have finally obtained this invention after a long period of research and practice. Summary of the Invention

[0008] The purpose of this invention is to solve the problems of easy poisoning during grain refinement, easy poisoning of the matrix, difficulty in controlling the brittle manganese phase, poor stability of cold working structure, and large performance fluctuations in existing 3003 aluminum alloy modification technology. It provides an application of Zr-Ti high-entropy alloy in the grain refinement and anti-poisoning of aluminum alloys.

[0009] To achieve the above objectives, this invention discloses the application of a Zr-Ti high-entropy alloy in grain refinement and anti-poisoning of aluminum alloys, wherein the Zr-Ti high-entropy alloy is a Ti... x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 A high-entropy alloy, wherein x = 0.1~0.3, and the amount of Zr-Ti high-entropy alloy added is 0.5wt.%~1.5wt.% of the total mass of the aluminum alloy.

[0010] The Ti x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 The smelting process of high-entropy alloys is as follows: according to Ti x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 Weigh out Ti, Zr, Cr, V and Fe metal raw materials, place the metal raw materials in a water-cooled copper crucible, and evacuate to a vacuum level not exceeding 3 × 10⁻⁶. -3 The furnace was cleaned three times with high-purity Ar and then arc-melted under Ar protection. The furnace was then melted at 200A for 2 minutes, cooled, turned over, and the melting process was repeated five times. The resulting alloy ingot was then crushed and sieved to a size of 75–150 μm after removing the oxide layer.

[0011] The application specifically includes the following steps:

[0012] S1, made from recycled 3003 aluminum and industrial pure aluminum, Ti x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 High-entropy alloys were used as grain refiners and added to a graphite crucible for melting to obtain uniformly melted aluminum.

[0013] S2, pour the uniformly molten aluminum obtained in step S1 into a preheated graphite mold, and let it cool naturally to room temperature to obtain recycled aluminum ingots.

[0014] S3 involves machining the recycled aluminum ingot to remove the surface oxide scale, resulting in a high-entropy alloy refined 3003 recycled aluminum alloy material.

[0015] In step S1, the chemical composition of the 3003 recycled material, by mass fraction, is: Mn 1.0%~1.5%, Fe≤0.7%, Cu≤0.05%~0.20%, Si≤0.60%, Mg≤0.05%, Zn≤0.05%, with Al as the balance.

[0016] Step S1 further includes raw material pretreatment: mechanically crushing, ultrasonically cleaning, and drying the 3003 recycled material; and processing industrial pure aluminum and Ti... x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 The high-entropy alloy is polished to remove the oxide scale and then cut into small pieces.

[0017] In step S1, the specific smelting process is as follows: the temperature is increased to 790℃~800℃ at a rate of 15℃ / min, held for 40~50 min, the stirring rate is 200 r / min, and the stirring time is 3~5 min.

[0018] In step S2, the preheating process of the graphite mold is as follows: preheat to 200 ℃, with a heating rate of 5 ℃ / min.

[0019] In step S2, the graphite mold has dimensions of 110 mm × 30 mm × 20 mm.

[0020] In step S2, the mass fractions of each element in the recycled aluminum ingot are: Si≤0.60%, Fe≤0.70%, Cu 0.05~0.20%, Mn 1.00%~1.50%, Cr≤0.10%, Ti≤0.10%, and Al is the balance.

[0021] In step S3, the number of alloy grains in the 3003 recycled aluminum alloy material refined by high entropy alloy is 98~305, and the average grain size is 19.53 μm~48.25 μm.

[0022] This invention addresses the specific pain points of 3003 aluminum-manganese alloy. Traditional grain refiners and rare-earth modification systems are easily poisoned by Mn and Fe impurities in 3003 melt, leading to deactivation of nucleation sites and grain refinement failure. Furthermore, the modification process easily generates brittle intermetallic phases, causing matrix poisoning problems such as grain boundary embrittlement and decreased plasticity. This invention features a unique Zr-Ti binary synergistic system. Ti can preferentially adsorb harmful Mn and Fe impurity atoms in the melt, passivating poisoning sites and preventing grain refiner poisoning failure at its source. Zr precisely controls phase precipitation behavior, inhibiting the formation of disordered brittle phases. The binary system provides complementary balance, completely solving the technical bottleneck of traditional technologies that suffer from "easy poisoning during grain refinement and matrix damage during modification," achieving a dual breakthrough of anti-poisoning grain refinement and reduced matrix poisoning.

[0023] The Zr-Ti high-entropy alloy prepared by this invention features a highly stable C15-Laves phase as the main phase, exhibiting excellent lattice compatibility with the aluminum matrix. It can provide a large number of high-density, high-stability heterogeneous nucleation cores in the aluminum melt, efficiently breaking down coarse dendrites and columnar crystals in 3003 aluminum alloy, transforming them into uniform and fine equiaxed crystals. Compared to the shortcomings of traditional grain refiners, such as uneven grain refinement and easy mixing of coarse grains, this invention can significantly improve grain density, reduce grain size variation, and significantly improve the uniformity of the as-cast microstructure. Furthermore, the grain refinement effect is not affected by Mn or Fe impurities and remains stable and undiminished over a long period.

[0024] This invention relies on the Zr-Ti binary adsorption poisoning effect to precisely intervene in the growth orientation and crystallization behavior of the Al6Mn phase, forcing the coarse and sharp blocky manganese phase to transform into fine, rounded, and diffusely distributed granules, completely eliminating the cutting damage of manganese phase to the aluminum matrix; at the same time, it effectively inhibits the local segregation and abnormal coarsening of the manganese phase, and prevents the formation of new harmful inclusion phases during the modification process. Without relying on heat treatment, it achieves the harmless modification of inherent defective phases, and significantly improves the alloy's plasticity and cold working ability.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0026] The present invention discloses a method for modifying 3003 aluminum alloy to resist poisoning and refine its structure using Zr-Ti high-entropy alloys. Designed specifically for the unique properties of non-heat-treatable strengthened aluminum-manganese alloys, this method possesses significant technical advantages and industrialization value. Specific beneficial effects are as follows:

[0027] 1. Excellent anti-toxic and grain refinement effects, with extremely uniform and dense grain structure:

[0028] This invention completely avoids the poisoning and failure problem of traditional grain refiners through a Zr-Ti binary synergistic anti-poisoning mechanism, achieving stable and efficient grain refinement within an addition range of 0.5wt.% to 1.5wt.%. Unmodified 3003 aluminum alloy has coarse grains and uneven microstructure. After modification with this invention's high-entropy alloy, the grain density is significantly increased, the grain size is significantly refined, coarse dendrites and mixed grain defects are completely eliminated, and the matrix microstructure density is greatly improved, optimizing the material forming basis from the source.

[0029] 2. Low-toxicity modification with no side effects, synergistic improvement in strength and plasticity:

[0030] The high-entropy alloy system of this invention exhibits excellent chemical stability. During the modification process, there is no large-scale precipitation of brittle and harmful phases, no grain boundary embrittlement, and no damage to the matrix plasticity, overcoming the limitation of traditional modification techniques that invert strength and plasticity. Under optimal process conditions, the modified 3003 aluminum alloy can achieve a Brinell hardness of 38.22 HBW, a tensile strength of 120 MPa, and an elongation after fracture of 18.5%, achieving simultaneous improvement in strength, hardness, and plasticity, completely solving the pain point of plasticity deterioration in traditional refining modifications.

[0031] 3. Harmless optimization of brittle manganese phase, significantly improving cold working adaptability:

[0032] This invention can modify the coarse, blocky Al6Mn brittle phase of 3003 aluminum alloy into a fine, dispersed granular structure, eliminate the defect of the second phase cutting the matrix, significantly improve the cold working performance of the alloy such as stamping, bending, and rolling, effectively reduce defects such as processing cracking, peeling, and orange peel on the surface, and greatly improve the yield and surface quality of high-end precision 3003 aluminum foil and stamped components.

[0033] 4. Strong process compatibility and high value for industrialization and promotion:

[0034] The modified process of this invention is compatible with existing conventional smelting and casting production lines for 3003 aluminum alloy. It does not require the modification of high-end equipment, has a wide smelting temperature window, strong process controllability, good remelting stability, low element loss rate, no special environmental protection pressure, low carbon and high efficiency, and controllable cost. Attached Figure Description

[0035] Figure 1 Ti is a high-entropy alloy 0.2 Zr 0.8 Cr 0.1 V 1.8 Fe 0.1 Ti 0.2 Zr 0.8 Cr 0.1 V 1.8 Fe 0.1 and Ti 0.2 Zr 0.8 Cr 0.1 V 1.8 Fe 0.1 The X-ray diffraction (XRD) pattern;

[0036] Figure 2 OM electronic images of 100 wt.% recycled aluminum-rich phase alloy material; wherein, (a) is 0.5 wt.% Ti 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 Metallurgical microscope image, (b) shows 1.0 wt.% Ti 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 Metallurgical microscope image, (c) shows 1.5 wt.% Ti. 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 Metallurgical microscope image, (d) represents 1.0 wt.% Ti0.2 Zr 0.8 Cr 0.1 V 1.8 Fe 0.1 Metallurgical microscope image, (e) is 0.5 wt.% Ti 0.3 Zr 0.7 Cr 0.1 V 1.8 Fe 0.1 Metallurgical microscope image;

[0037] Figure 3 In the image, (a) is a metallographic micrograph of the alloy without the addition of high-entropy alloy, and (b) is a metallographic micrograph of the alloy with 1.0 wt.% AlTiB refining agent.

[0038] Figure 4 The stress-strain curves are for samples of different high-entropy alloys and additive amounts in Examples 1-5 and Comparative Example 1. Detailed Implementation

[0039] The above-mentioned and other technical features and advantages of the present invention will be described in more detail below with reference to the accompanying drawings.

[0040] Example 1

[0041] 100wt.% recycled material, with 0.5wt.% added high-entropy alloy:

[0042] S1, Raw material ratio: Weigh 200g of 3003 recycled material (pretreated), Ti 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 1 g of high-entropy alloy.

[0043] S2, Smelting: Add the prepared recycled material and industrial pure aluminum to a crucible and place it in a resistance smelting furnace;

[0044] Heating section: Heat to 790 ℃ at a rate of 15 ℃ / min and hold for 40~50 min to fully melt the recycled material and industrial pure aluminum;

[0045] Stirring: Stir at a stirring rate of 200 r / min for 5 min to allow the raw materials to melt initially and avoid burning off Fe elements due to high temperature.

[0046] After the aluminum alloy has completely melted and been thoroughly stirred, add Ti 0.1 Zr 0.9 Cr 0.1 V 1.8Fe high-entropy alloy powder was wrapped in aluminum foil and pressed into the aluminum melt. The mixture was kept at a temperature of 20 min and then intermittently stirred at a rate of 200 r / min to ensure that the high-entropy alloy particles were uniformly dispersed and completely integrated into the aluminum alloy melt.

[0047] S3: After the aluminum liquid is fully melted, it is poured into a graphite mold preheated to 200℃ and allowed to cool naturally to room temperature to obtain a 3003 recycled aluminum ingot raw material with uniform composition. The mass fraction of each element, as determined by a spectrometer, is as follows: Si 0.266%, Fe 0.664%, Cu 0.04%, Mn 1.07%, Cr 0.033%, Ti 0.032%, with Al as the balance.

[0048] S4, finished product processing: turning to remove surface oxide scale, and processing into standard test specimens for metallographic analysis and tensile testing.

[0049] The material samples prepared in the above steps were subjected to the following microstructure analysis and performance tests, and the results are as follows:

[0050] (1) such as Figure 1 As shown in (a), the prepared high-entropy alloy Ti 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 It is a pure C15-Laves phase;

[0051] (2) The microstructure of the recycled aluminum alloy sample obtained in Example 1 was observed using an optical metallurgical microscope, and the results are as follows: Figure 2 As shown. By Figure 2 (a) As can be seen, the grain distribution in the alloy microstructure is relatively uniform, and the coarse dendrite structure is significantly reduced. Further statistical analysis was performed using Image-pro plus software on at least five random fields of view. The average grain size of the alloy obtained in Example 1 was 29.68 μm, and the number of grains was 211. Compared with the control group without the added refining modifier, the average grain size decreased by 38.49%, and the number of grains increased by 115.31%, indicating that the C15-Laves high-entropy alloy refining modifier prepared in this invention has a significant grain refining and microstructure homogenization effect.

[0052] (3) Mechanical property testing: The Brinell hardness was tested using a Brinell hardness tester (load 1000 kgf, holding pressure 30 s) and an electronic universal testing machine (tensile rate 2 mm / min). The Brinell hardness was 32.8 HBW. Figure 4The stress-strain curves of this embodiment show that the peak engineering stress of the sample reached 105 MPa, and the elongation after fracture was 16%. Compared with Comparative Example 1 without the addition of high-entropy alloy, its tensile strength increased by 14 MPa, and its elongation increased by 3 percentage points. The curves shifted overall towards higher stress and higher strain, indicating that the addition of Zr-Ti high-entropy alloy improved both the material's load-bearing capacity and plasticity. This change is consistent with grain refinement, reduction of coarse dendrites, and improved uniformity of plastic deformation.

[0053] (4) Through observation Figure 2 (a) The grains are significantly refined, coarse dendrites are basically eliminated, the Al6Mn phase is initially refined and passivated, the matrix continuity is improved, no brittle harmful phases are precipitated, and there are no matrix poisoning defects.

[0054] Example 2

[0055] 100wt.% recycled material, with 1.0wt.% added Ti 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 High-entropy alloys:

[0056] The difference between this embodiment and Embodiment 1 is that in step S1, 200 g of 3003 recycled material and Ti... 0.2 Zr 0.8 Cr 0.1 V 1.8 2 g of Fe high-entropy alloy; other process conditions are the same as in Example 1.

[0057] The prepared recycled aluminum ingots, after being analyzed by a spectrometer, showed the following mass fractions of each element: Si 0.277%, Fe 0.699%, Cu 0.07%, Mn 1.025%, Cr 0.048%, Ti 0.055%, with Al as the balance.

[0058] The material sample prepared in Example 2 underwent the following microstructure analysis and performance testing, and the results are as follows:

[0059] (1) such as Figure 1 As shown in (a), the prepared high-entropy alloy Ti 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 It is a pure C15-Laves phase, see Figure 1 ;

[0060] (2) Observation was performed using a metallurgical microscope. Figure 2As shown in (b), the aluminum alloy obtained in Example 3 has an average size of 19.53 μm and a grain number of 305. Compared with the comparative example without the addition of refining modifier, the average grain size is reduced by 51.01% and the grain number is increased by 147.96%.

[0061] (3) Mechanical property testing: The Brinell hardness was tested using a Brinell hardness tester (load 1000 kgf, holding pressure 30s) and an electronic universal testing machine (tensile rate 2 mm / min). The Brinell hardness was 39.35 HBW. Figure 4 The stress-strain curves corresponding to this embodiment show that the peak engineering stress of the sample reaches 125 MPa, and the elongation after fracture reaches 19%. The curve is located at the upper right of all embodiments. Compared with Comparative Example 1, the tensile strength is increased by 34 MPa, and the elongation is increased by 6 percentage points. Compared with Comparative Example 2 with AlTiB refining agent, the tensile strength and elongation are also increased by 27 MPa and 4.5 percentage points, respectively, showing the best strength-plasticity match. This result is consistent with the reduction of grain size to 19.53 μm in this embodiment and the reduction of local stress concentration after the Al6Mn phase is finer and more dispersed.

[0062] (4) Combination Figure 2 The comparison shows that the modified alloy prepared in Example 2 has the best microstructure uniformity and the best grain refinement effect, with a large amount of Al6Mn brittle phase being transformed into fine and dispersed particles.

[0063] Example 3

[0064] 100wt.% recycled material, with 1.5wt.% added Ti 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 High-entropy alloys:

[0065] The difference between this embodiment and Embodiment 1 is that in step S1, 200 g of recycled 3003 aluminum alloy and Ti... 0.3 Zr 0.7 Cr 0.1 V 1.8 3 g of Fe high-entropy alloy; other process conditions were the same as in Example 1.

[0066] The prepared recycled aluminum ingot has the following elemental mass fractions: Si 0.212%, Fe 0.679%, Cu 0.02%, Mn 1.05%, Cr 0.052%, Ti 0.071%, with Al as the balance.

[0067] The material samples prepared in Example 3 were subjected to the following performance tests and microstructure analysis, and the results are as follows:

[0068] (1) such as Figure 1 As shown in (a), the high-entropy alloy Ti prepared in this embodiment... 0.1 Zr 0.9 Cr 0.1 V 1.8 Fe 0.1 It is a pure C15-Laves phase;

[0069] (2) Observation was performed using a metallurgical microscope. Figure 2 As shown in (c), the aluminum alloy obtained in Example 3 has an average size of 23.64 μm and a grain number of 243. Compared with the comparative example without the addition of refining modifier, the average grain size is reduced by 51.01% and the grain number is increased by 147.96%.

[0070] (3) Mechanical property testing: The Brinell hardness was tested using a Brinell hardness tester (load 1000 kgf, holding pressure 30s) and an electronic universal testing machine (tensile rate 2 mm / min). The Brinell hardness was 38.22 HBW. Figure 4 The stress-strain curves of this embodiment show that the peak engineering stress of the sample is 111 MPa, and the elongation after fracture is 16.5%, which are 20 MPa and 3.5 percentage points higher than those of Comparative Example 1, respectively, indicating that this embodiment still has significant strengthening and plasticizing effects. However, compared with Example 2, the peak value and fracture endpoint of the curve have both decreased, indicating that further increasing the amount of high-entropy alloy added has not further improved the strength and plasticity. This change is consistent with the increase in grain size and the decrease in the uniformity of microstructure.

[0071] (4) Combination Figure 2 The comparison shows that in Example 3, as the amount of high-entropy alloy added increases, the uniformity of the alloy structure and the grain refinement effect decrease slightly compared to Example 2.

[0072] Example 4

[0073] 100wt.% recycled material, with 1.0wt.% added Ti 0.2 Zr 0.8 Cr 0.1 V 1.8 Fe 0.1 High-entropy alloys:

[0074] The difference between this embodiment and Embodiment 1 is that in step S1, 200 g of 3003 recycled material and Ti... 0.2 Zr 0.8 Cr 0.1 V 1.8 Fe 0.1 2 g of high-entropy alloy; other process conditions are the same as in Example 1.

[0075] The prepared recycled aluminum ingots, after being analyzed by a spectrometer, showed the following mass fractions of each element: Si 0.277%, Fe 0.699%, Cu 0.07%, Mn 1.025%, Cr 0.048%, Ti 0.055%, with Al as the balance.

[0076] The material sample prepared in Example 4 underwent the following microstructure analysis and performance testing, and the results are as follows:

[0077] (1) such as Figure 1 As shown in (b), the prepared high-entropy alloy Ti 0.2 Zr 0.8 Cr 0.1 V 1.8 Fe 0.1 It is a pure C15-Laves phase;

[0078] (2) Observation was performed using a metallurgical microscope. Figure 2 As shown in (d), the aluminum alloy obtained in Example 3 has an average size of 21.91 μm and a grain number of 282. Compared with the comparative example without the addition of refining modifier, the average grain size is reduced by 57.70% and the grain number is increased by 187.64%.

[0079] (3) Mechanical property testing: The Brinell hardness was tested using a Brinell hardness tester (load 1000 kgf, holding pressure 30s) and an electronic universal testing machine (tensile rate 2 mm / min). The Brinell hardness was 39.01 HBW. Figure 4 The stress-strain curves of this embodiment show that the peak engineering stress of the sample reaches 117 MPa, and the elongation after fracture is 17%. Compared with Comparative Example 1, the tensile strength increases by 26 MPa, and the elongation increases by 4 percentage points; compared with Comparative Example 2 using AlTiB refining agent, the tensile strength and elongation also increase by 19 MPa and 2.5 percentage points, respectively. The curves are generally in the region of high stress and large strain, indicating that this high-entropy alloy composition can maintain good plasticity while improving load-bearing capacity, and has superior comprehensive mechanical properties.

[0080] (4) Combination Figure 2 The comparison shows that the modified alloy prepared in Example 4 has significantly improved microstructure uniformity and grain refinement compared to the alloy without additives.

[0081] Example 5

[0082] 100wt.% recycled material, with 1.0wt.% added Ti 0.3 Zr 0.7 Cr 0.1 V 1.8 Fe 0.1 High-entropy alloys:

[0083] The difference between this embodiment and Embodiment 1 is that in step S1, 200 g of 3003 recycled material and Ti... 0.3 Zr 0.7 Cr 0.1 V 1.8 Fe 0.1 2 g of high-entropy alloy; other process conditions are the same as in Example 1.

[0084] The prepared recycled aluminum ingots, after being analyzed by a spectrometer, showed the following mass fractions of each element: Si 0.281%, Fe 0.665%, Cu 0.07%, Mn 1.07%, Cr 0.041%, Ti 0.067%, with Al as the balance.

[0085] The material sample prepared in Example 5 underwent the following microstructure analysis and performance testing, and the results are as follows:

[0086] (1) such as Figure 1 As shown in (c), the prepared high-entropy alloy Ti 0.3 Zr 0.7 Cr 0.1 V 1.8 Fe 0.1 It is a pure C15-Laves phase, see Figure 1 ;

[0087] (2) Observation was performed using a metallurgical microscope. Figure 2 As shown in (e), the aluminum alloy obtained in Example 3 has an average size of 22.59 μm and a grain number of 271. Compared with the comparative example without the addition of refining modifier, the average grain size is reduced by 53.18% and the grain number is increased by 176.53%.

[0088] (3) Mechanical property testing: The Brinell hardness was tested using a Brinell hardness tester (load 1000 kgf, holding pressure 30s) and an electronic universal testing machine (tensile rate 2 mm / min). The Brinell hardness was 38.59 HBW. Figure 4 The stress-strain curves corresponding to this embodiment show that the peak engineering stress of the sample is 103 MPa, and the elongation after fracture reaches 18%. Its peak stress is lower than that of Examples 2 and 4, but the fracture endpoint of the curve extends significantly to the right. Compared with Comparative Example 1, the tensile strength increases by 12 MPa, and the elongation increases by 5 percentage points, indicating that this embodiment mainly exhibits improved plasticity, maintaining a certain strengthening effect while possessing good deformation capacity. This result is consistent with the reduction of brittle phases in Al6Mn and the improvement of matrix continuity.

[0089] (4) Combination Figure 2 The comparison shows that the modified alloy prepared in Example 5 has a more uniform microstructure, the grain refinement effect is relatively lower than that in Example 2, and the proportion of Al6Mn brittle phase is reduced.

[0090] Comparative Example 1

[0091] 100wt.% recycled material, with 0wt.% added high-entropy alloy:

[0092] S1, Raw material ratio: 200 g of 3003 recycled material.

[0093] S2, Smelting process: exactly the same as in Example 1.

[0094] S3, Casting process: exactly the same as in Example 1. Spectroscopic analysis of the composition (mass fraction): Si 0.231%, Fe 0.614%, Mn 1.23%, Cr 0.01%, Ti 0.22%, Al balance.

[0095] Experimental results:

[0096] (1) Observation was performed using a metallurgical microscope, by Figure 3 As shown in (a), the aluminum alloy obtained in Comparative Example 1 has an average size of 48.25 μm and a grain size of 98.

[0097] (2) Mechanical properties: Hardness: 36.41 HBW; Elongation: 13%; Tensile strength: 91 MPa.

[0098] Comparative Example 2

[0099] 100wt.% recycled material, with 1.0wt.% AlTiB refining agent added:

[0100] S1, Raw material ratio: 200 g of 3003 recycled material.

[0101] S2, Smelting process: exactly the same as in Example 1.

[0102] S3, Casting process: exactly the same as in Example 1. Spectroscopic analysis of the composition (mass fraction): Si 0.245%, Fe 0.664%, Mn 1.07%, Cr 0.01%, Ti 0.09%, Al balance.

[0103] Experimental results:

[0104] (1) Observation was performed using a metallurgical microscope, by Figure 3 As shown in (b), the aluminum alloy obtained in Comparative Example 2 has an average size of 37.21 μm and a grain size of 148.

[0105] (2) Mechanical properties: Hardness: 37.55 HBW; Elongation: 14.5%; Tensile strength: 98 MPa.

[0106] The experimental and test results of Examples 1-5 and Comparative Examples 1-2 are shown in Table 1 below.

[0107] Table 1. Experimental and test results of Examples 1-5 and Comparative Examples 1-2

[0108]

[0109] As shown in Table 1:

[0110] 1. Effect of high-entropy alloy addition on grain refinement:

[0111] As the addition of high-entropy alloy increased from 0 to 1.5 wt.%, the grain number and size initially improved and then deteriorated. Without addition, the grains were coarse, with an average size of 48.25 μm and only 98 grains. With an addition of 0.5 wt.%, the number of nucleation sites increased, the number of grains rose to 211, and the size decreased to 29.68 μm. With an addition of 1.0 wt.%, the nucleation sites were saturated and uniformly dispersed, the number of grains reached a peak of 305, and the average size was the smallest at 19.53 μm, showing the best grain refinement effect. Compared with traditional grain refiners, the addition of high-entropy alloy significantly reduced both grain size and number, and effectively improved performance.

[0112] 2. Aluminum alloy alteration effect:

[0113] When the addition amount is 0.5 wt.%, the grains are significantly refined, coarse dendrites are basically eliminated, the Al6Mn phase is initially refined and passivated, the matrix continuity is improved, no brittle harmful phases precipitate, and no matrix poisoning defects are found. The modified alloy prepared with an addition amount of 1.0 wt.% exhibits the best microstructure uniformity and the best grain refinement effect, with most of the brittle Al6Mn phase transforming into fine, dispersed particles.

[0114] 3. Optimal process comprehensive performance analysis:

[0115] The optimal process combination is 100 wt.% recycled material with a high-entropy alloy addition of 1.0 wt.%. Under these conditions, the alloy has an average grain size of 19.53 μm, a Brinell hardness of 39.35 HBW, an elongation of 19%, and a tensile strength of 125 MPa, achieving the best match between grain refinement and mechanical properties.

[0116] The stress-strain curves show that, compared to the control group without high-entropy alloy, the curves of all examples generally shift towards higher stress and higher strain, indicating that the Zr-Ti high-entropy alloy maintains good plasticity while improving tensile strength. The curve of Example 2 is located in the upper right, demonstrating a superior balance between strength and plasticity. This result is consistent with grain refinement and the reduction in stress concentration and suppression of crack initiation and propagation after the Al6Mn phase becomes smaller and more dispersed.

[0117] The above description is merely a preferred embodiment of the present invention and is illustrative rather than restrictive. Those skilled in the art will understand that many changes, modifications, and even equivalents can be made within the spirit and scope defined by the claims of the present invention, all of which will fall within the protection scope of the present invention.

Claims

1. The application of a Zr-Ti high-entropy alloy in grain refinement and anti-poisoning of aluminum alloys, characterized in that, The Zr-Ti high-entropy alloy is Ti. x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 A high-entropy alloy, wherein x = 0.1~0.3, and the amount of Zr-Ti high-entropy alloy added is 0.5wt.%~1.5wt.% of the total mass of the aluminum alloy.

2. The application of a Zr-Ti high-entropy alloy as described in claim 1 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, The Ti x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 The smelting process of high-entropy alloys is as follows: according to Ti x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 Weigh out Ti, Zr, Cr, V and Fe metal raw materials, place the metal raw materials in a water-cooled copper crucible, and evacuate to a vacuum level not exceeding 3 × 10⁻⁶. -3 The furnace was cleaned three times with high-purity Ar and then arc-melted under Ar protection. The furnace was then melted at 200A for 2 minutes, cooled, turned over, and the melting process was repeated five times. The resulting alloy ingot was then crushed and sieved to a size of 75–150 μm after removing the oxide layer.

3. The application of a Zr-Ti high-entropy alloy as described in claim 1 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, The application specifically includes the following steps: S1, made from recycled 3003 aluminum and industrial pure aluminum, Ti x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 High-entropy alloys were used as grain refiners and added to a graphite crucible for melting to obtain uniformly melted aluminum. S2, pour the uniformly molten aluminum obtained in step S1 into a preheated graphite mold, and let it cool naturally to room temperature to obtain recycled aluminum ingots. S3 involves machining the recycled aluminum ingot to remove the surface oxide scale, resulting in a high-entropy alloy refined 3003 recycled aluminum alloy material.

4. The application of a Zr-Ti high-entropy alloy as described in claim 2 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, In step S1, the chemical composition of the 3003 recycled material, by mass fraction, is: Mn 1.0%~1.5%, Fe≤0.7%, Cu≤0.05%~0.20%, Si≤0.60%, Mg≤0.05%, Zn≤0.05%, with Al as the balance.

5. The application of a Zr-Ti high-entropy alloy as described in claim 2 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, Step S1 further includes raw material pretreatment: mechanically crushing, ultrasonically cleaning, and drying the 3003 recycled material; and processing industrial pure aluminum and Ti... x Zr 1-x Cr 0.1 V 0.8 Fe 0.1 The high-entropy alloy is polished to remove the oxide scale and then cut into small pieces.

6. The application of a Zr-Ti high-entropy alloy as described in claim 2 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, In step S1, the specific smelting process is as follows: the temperature is increased to 790℃~800℃ at a rate of 15℃ / min, held for 40~50 min, the stirring rate is 200 r / min, and the stirring time is 3~5 min.

7. The application of a Zr-Ti high-entropy alloy as described in claim 2 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, In step S2, the preheating process of the graphite mold is as follows: preheat to 200 ℃, with a heating rate of 5 ℃ / min.

8. The application of a Zr-Ti high-entropy alloy as described in claim 2 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, In step S2, the graphite mold has dimensions of 110 mm × 30 mm × 20 mm.

9. The application of a Zr-Ti high-entropy alloy as described in claim 2 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, In step S2, the mass fractions of each element in the recycled aluminum ingot are: Si 0.212%~0.277%, Fe 0.664%~0.699%, Cu 0.02%~0.07%, Mn 1.025%~1.07%, Cr 0.033%~0.052%, Ti 0.032%~0.071%, with Al as the balance.

10. The application of a Zr-Ti high-entropy alloy as described in claim 2 in grain refinement and anti-poisoning of aluminum alloys, characterized in that, In step S3, the number of alloy grains in the 3003 recycled aluminum alloy material refined by high entropy alloy is 98~305, and the average grain size is 19.53 μm~48.25 μm.