A method for preparing boron nitride-reinforced copper-graphite composite materials

By employing wet dispersion, ball milling, drying, and spark plasma sintering processes, combined with ultrasonic cleaning and dispersants, the problem of insufficient bonding between hexagonal boron nitride and the copper matrix was solved, resulting in the preparation of a Cu-graphite-h-BN composite material with excellent tribological properties.

CN123108348APending Publication Date: 2026-11-17HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611587679.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, the wettability between hexagonal boron nitride and copper matrix is ​​poor, resulting in limited interfacial bonding ability. This easily leads to uneven dispersion of the reinforcing phase, insufficient interfacial bonding, and porosity defects, which affect the mechanical properties and tribological properties of the composite material.

Method used

Cu-graphite-h-BN composite materials were prepared by using wet dispersion, ball milling, drying, reduction and spark plasma sintering processes, combined with ultrasonic cleaning and sodium dodecylbenzoate dispersant. The heat was transferred in the form of suspension to improve powder dispersibility, and spark plasma sintering technology was used to refine the grains and enhance interfacial bonding.

Benefits of technology

The mechanical and tribological properties of Cu-graphite-h-BN composite materials were significantly improved, and the uniform distribution and good bonding of the reinforcing phase were achieved, resulting in the preparation of dense, high-performance copper-based materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure AOT9STAREOHE2OEPV3VLY5ELE6XUFP64KP3TYHOB
    Figure AOT9STAREOHE2OEPV3VLY5ELE6XUFP64KP3TYHOB
  • Figure PV243KO7OPYMDDC6SMRCBYX3RIIP0IAWOJPR234E
    Figure PV243KO7OPYMDDC6SMRCBYX3RIIP0IAWOJPR234E
  • Figure YJ3EIACBKTB8UJYOPC2DFUL5IRXEODYVJCXIUEWZ
    Figure YJ3EIACBKTB8UJYOPC2DFUL5IRXEODYVJCXIUEWZ
Patent Text Reader

Abstract

This invention discloses a method for preparing a boron nitride-reinforced copper-graphite composite material, specifically including the following steps: (1) powder pretreatment; (2) high-temperature reduction; and (3) spark plasma sintering. This invention incorporates h-BN, which, due to its graphite-like layered crystal structure, low coefficient of friction, good high-temperature stability, and excellent chemical inertness, enhances the tribological properties of the copper-based alloy. This invention uses a suspension instead of powder, transferring the heat generated during ball milling by adding ethanol and isolating it from air. Sodium dodecylbenzoate is used as a dispersant, and an ultrasonic cleaner is employed to reduce the powder's agglomeration ability and accelerate the ball milling process. Spark plasma sintering technology refines the grain size of the alloy through the combined effects of plasma activation and sintering densification, ultimately producing a dense Cu / GF-h-BN composite material with superior mechanical properties and wider applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal matrix composite materials and friction materials technology, specifically relating to a method for preparing boron nitride-reinforced copper-graphite composite materials. By regulating the reinforcing phase and optimizing the composite structure, the mechanical properties and tribological properties of copper-graphite materials are improved, and it can be applied to electrical contact materials, friction pair materials, and high wear-resistant copper-based engineering materials. Background Technology

[0002] Copper-based alloys are widely used in various electronic components due to their excellent electrical properties, but their poor mechanical properties limit their application in many emerging fields. In order to meet the high-performance requirements brought about by the progress of the times, it is necessary to further improve the comprehensive mechanical properties of copper alloys.

[0003] To improve the overall performance of copper-based composites, existing technologies typically employ methods such as introducing ceramic particles, carbon materials, or other reinforcing phases to strengthen the copper matrix. Among these, hexagonal boron nitride (h-BN) is considered a promising reinforcing phase for copper-based composites due to its graphite-like layered crystal structure, low coefficient of friction, good high-temperature stability, and excellent chemical inertness. The weak interlayer bonding in the layered structure of h-BN provides a certain degree of solid lubrication, forming a lubrication transfer film during friction and reducing the shear resistance at the friction interface. Simultaneously, its high hardness and good thermal stability can reinforce the copper matrix, improving the service stability of the composite material under high-temperature and high-load conditions.

[0004] However, due to the poor wettability between hexagonal boron nitride and the copper matrix, their interfacial bonding ability is limited. In traditional mixed sintering processes, problems such as uneven dispersion of the reinforcing phase, insufficient interfacial bonding, and porosity defects easily occur, making it difficult to fully realize the reinforcing effect of hexagonal boron nitride. Furthermore, the hexagonal boron nitride lamellar structure is prone to agglomeration during composite material preparation, leading to reduced internal microstructure uniformity and potentially affecting the mechanical and tribological properties of the composite material. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing boron nitride-reinforced copper-graphite composite materials, which significantly improves the mechanical properties of the prepared Cu-graphite-h-BN composite materials.

[0006] The technical solution of this invention: A method for preparing boron nitride-reinforced copper-graphite composite material specifically includes the following steps: (1) Powder pretreatment High-purity Cu powder and flake graphite were weighed separately and added to a beaker in sequence. Anhydrous ethanol was added until the powder was completely submerged. Then, a dispersant was added. The beaker was placed in a magnetic stirrer and heated and stirred until fully mixed. Anhydrous ethanol was added again until the powder was submerged. The slurry was loaded into a ball mill jar, and cemented carbide balls were added. After assembly, the ball mill jar was fixed in a planetary ball mill for ball milling. After ball milling, the slurry was poured into a beaker. Hexagonal boron nitride powder was added to the beaker and the beaker was placed in an ultrasonic cleaner to fully disperse the agglomerated boron nitride powder, thus obtaining a Cu / GF-h-BN mixed slurry. (2) High-temperature reduction Take out the slurry after ball milling in step (1) and place it in a beaker. Place the beaker in a drying oven to dry it. Grind the dried powder evenly and spread it on a ceramic firing boat. Then place it in a tube furnace. Set the program and carry out reduction treatment in a hydrogen atmosphere to finally obtain Cu / GF-h-BN composite powder. (3) Spark plasma sintering The Cu / GF-h-BN composite powder that has been reduced in step (2) is ground and added to a graphite mold. The graphite mold is placed in the furnace cavity of a spark plasma sintering furnace for pre-compactment. After setting the program, the furnace cavity is vacuum treated and then sintered. After sintering, Cu / GF-h-BN composite material is obtained.

[0007] In step (1), the mass fraction of h-BN powder is 0.5-1.5%, the mass fraction of flake graphite is 8%, and the remainder is high-purity Cu powder. The Cu powder is high-purity electrolytic Cu powder, which is grape-like in shape, with a purity of 99.999% and a particle size of 1-3 μm. The purity of h-BN powder is 99.8% and the particle size is 10,000 mesh. The purity of flake graphite is 99.5% and the particle size is 50 mesh.

[0008] In step (1), the magnetic stirrer is a DF-101S type heat-collecting magnetic stirrer with a stirring temperature of 25-35℃ and a stirring time of 6-8 h. In addition to an appropriate amount of anhydrous ethanol, sodium dodecyl benzoate is added to the beaker as a dispersant. The amount added depends on the dispersion of the mixed powder to promote more uniform powder dispersion.

[0009] In step (1), the planetary ball mill is the Nanjing University Instruments QM-QX4 omnidirectional planetary ball mill with a ball milling speed (rotation speed) of 300 rpm, a ball-to-material ratio of 5:1, a ball milling time of 16 h, and the ball tank and the ball milling media balls are all made of hard alloy.

[0010] In step (1), the ultrasonic cleaner is model FUYANG-F-030, and the ultrasonic time is 20 minutes.

[0011] In step (2), the slurry after ball milling is taken out and placed in a beaker. The slurry residue on the ball milling tank wall and the surface of the alloy balls is repeatedly rinsed with anhydrous ethanol and then placed in a drying oven. The model of the drying oven is DHG-9000-9005, the drying temperature is 50-60 ℃, and the drying time is 12 h.

[0012] In step (2), the tubular furnace model is GSL-1200X, and the program is set as follows: the temperature is increased from room temperature to 200℃ at 5℃ / min, then increased from 200℃ to 400℃ at 10℃ / min, held for 2 h, and then decreased to 300℃ at 10℃ / min. After that, the furnace is cooled to room temperature, and finally Cu / GF-h-BN composite powder is obtained.

[0013] The gas introduced in step (2) is hydrogen, and the introduction rate is 300-350 ml / min.

[0014] In step (3), the graphite mold has an inner diameter of 20 mm, an outer diameter of 60 mm, and a height of 70 mm. Carbon paper is used to separate the Cu / GF-BN composite powder from the graphite mold to facilitate sampling and demolding after sintering.

[0015] In step (3), the discharge plasma sintering furnace is model LaboxTM-300, and thermocouple temperature measurement is used. The front end of the thermocouple is inserted into the temperature measuring hole of the graphite mold.

[0016] The discharge plasma sintering program in step (3) is as follows: the temperature is raised from room temperature to 600 ℃ and held for 5 min, then the temperature is raised to 920 ℃ and held for 5 min. The heating rate is 80-100 ℃ / min, the pre-pressure is 10 MPa, the pressure is raised to 50 MPa during the second heating process, and the temperature is held for 5 min before cooling with the furnace.

[0017] The innovation of this invention lies in: In terms of material design: by mixing Cu powder and h-BN powder in a certain proportion, the graphite-like layered crystal structure, low coefficient of friction, good high-temperature stability and excellent chemical inertness of h-BN are fully utilized to achieve the reinforcement effect on the copper matrix.

[0018] Regarding the preparation method: The preparation method of this invention consists of wet dispersion, ball milling, drying, reduction, and spark plasma sintering processes, which gives the material a specific crystal structure and phase composition, thereby improving the material's performance. Furthermore, by utilizing the ultrasonic cavitation and vibration effects of an ultrasonic cleaner, the ball-milled powder is dispersed, de-agglomerated, surface deposits are removed, and the uniformity of subsequent sintering is improved. This preparation method makes it possible to mass-produce this high wear-resistant copper-based engineering material.

[0019] In terms of performance optimization: by reinforcing copper-based composite materials with h-BN, the tribological and wear properties of copper-based alloys are further improved, exhibiting excellent overall performance.

[0020] Compared with existing technologies, the present invention has at least the following advantages: This invention incorporates h-BN, leveraging its graphite-like layered crystal structure, low coefficient of friction, good high-temperature stability, and excellent chemical inertness to enhance the tribological properties of copper-based alloys. Traditional ball milling easily generates significant heat, and the softness of copper leads to powder agglomeration, resulting in large particle sizes. This invention replaces powder with a suspension, using ethanol to transfer the heat generated during ball milling while isolating it from air. Sodium dodecylbenzoate is used as a dispersant, and an ultrasonic cleaner is employed to reduce powder agglomeration and accelerate the ball milling process. Spark plasma sintering technology refines the alloy's grain size through the combined effects of plasma activation and sintering densification, ultimately producing a dense Cu / GF-h-BN composite material with superior mechanical properties and wider applications. Attached Figure Description

[0021] Figure 1 This is a surface morphology diagram of the raw material, high-purity copper powder. Figure 2 High-magnification morphology image of the surface of Cu / GF-h-BN composite material; Among them: (a) Cu / GF-0.5%h-BN, (b) Cu / GF-1%h-BN, (c) Cu / GF-1.5%h-BN; Figure 3 The image shows the XRD pattern of the Cu / GF-h-BN composite material. Detailed Implementation

[0022] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0023] Example 1

[0024] The Cu / GF-h-BN composite material in this embodiment is processed by wet dispersion, ball milling, drying, reduction, and spark plasma sintering. The mass fraction of h-BN is 0.5%, the mass fraction of flake graphite is 8%, and the remainder is high-purity electrolytic Cu powder in the form of grape bunches with a purity of 99.999% and a particle size of 1-3 μm. The purity of h-BN powder is 99.8% with a particle size of 10,000 mesh, and the purity of flake graphite is 99.5% with a mesh size of 50 mesh.

[0025] The preparation method of Cu / GF-h-BN composite material in this embodiment is as follows: (1) Powder pretreatment Weigh 45.75g of high-purity Cu powder and 4g of flake graphite into a beaker, add anhydrous ethanol until the powder is completely submerged, then add 0.06g of sodium dodecylbenzoate. Place the beaker in a magnetic stirrer and stir at 25-35 ℃ for 6-8 hours. After thorough mixing, add anhydrous ethanol again until the powder is submerged. Load the slurry into a ball mill jar, add cemented carbide balls at a ball-to-powder ratio of 5:1. After assembly, fix the ball mill jar in a planetary ball mill and ball mill for 16 hours. After ball milling, add 0.25gh-BN powder and ultrasonically treat for 20 minutes. (2) High-temperature reduction The slurry after ball milling was taken out and placed in a beaker. The slurry residue on the ball mill jar wall and the surface of the alloy balls was repeatedly rinsed with anhydrous ethanol. The beaker was then placed in a drying oven for drying at 50-60 ℃ for 12 h. After drying, the obtained powder was ground and evenly spread on a ceramic sintering boat and placed in a tube furnace. Hydrogen was introduced at a flow rate of 300-350 ml / min to create a reducing atmosphere. The program was set to increase the temperature from room temperature to 200 ℃ at 5 ℃ / min, then increase it from 200 ℃ to 400 ℃ at 10 ℃ / min, hold it for 2 h, and then decrease it to 300 ℃ at 10 ℃ / min. The furnace was then cooled to room temperature to obtain Cu / GF-h-BN composite powder. (3) Spark plasma sintering The reduced Cu / GF-h-BN composite powder was ground and added to a graphite mold (the graphite mold has an inner diameter of 20 mm, an outer diameter of 60 mm, and a height of 70 mm, with carbon paper separating the Cu / GF-h-BN composite powder from the graphite mold for easy sampling and demolding after sintering) wrapped in carbon paper. The graphite mold was then placed in the furnace cavity of a spark plasma sintering furnace and pre-compacted at a pressure of 10 MPa. The tip of a thermocouple was inserted into the temperature measuring hole of the graphite mold. The furnace door was closed for vacuum treatment. After the furnace cavity reached the vacuum level, sintering was carried out according to the set program, which is as follows: the temperature was raised from room temperature to 600 ℃ and held for 5 min, then raised to 920 ℃ and held for 5 min, with a heating rate of 80-100 ℃ / min and a pre-compression pressure of 10 MPa. During the second stage of heating, the pressure was raised to 50 MPa and held for 5 min before cooling with the furnace. After sintering, Cu / GF-h-BN composite material was obtained.

[0026] Example 2

[0027] The Cu / GF-h-BN composite material in this embodiment is processed by wet dispersion, ball milling, drying, reduction, and spark plasma sintering. The mass fraction of h-BN is 1%, the mass fraction of flake graphite is 8%, and the remainder is high-purity electrolytic Cu powder in the form of grape bunches with a purity of 99.999% and a particle size of 1-3 μm. The purity of h-BN powder is 99.8% with a particle size of 10,000 mesh, and the purity of flake graphite is 99.5% with a mesh size of 50 mesh.

[0028] The preparation method of Cu / GF-h-BN composite material in this embodiment is as follows: (1) Powder pretreatment Weigh out 45.5g of high-purity Cu powder and 4g of flake graphite, add them to a beaker, add anhydrous ethanol until the powder is completely submerged, then add 0.06g of sodium dodecylbenzoate. Place the beaker in a magnetic stirrer and stir at 25-35 ℃ for 6-8 hours. After stirring thoroughly, add anhydrous ethanol again until the powder is submerged. Load the slurry into a ball mill jar, add cemented carbide balls at a ball-to-powder ratio of 5:1. After assembly, fix the ball mill jar in a planetary ball mill and ball mill for 16 hours. After ball milling, add 0.5g of h-BN powder and ultrasonically treat for 20 minutes. (2) High-temperature reduction The slurry after ball milling was taken out and placed in a beaker. The slurry residue on the ball mill jar wall and the surface of the alloy balls was repeatedly rinsed with anhydrous ethanol. The beaker was then placed in a drying oven for drying at 50-60 ℃ for 12 h. After drying, the obtained powder was ground and evenly spread on a ceramic sintering boat and placed in a tube furnace. Hydrogen gas was introduced at a flow rate of 300-350 ml / min to create a reducing atmosphere. The program was set to increase the temperature from room temperature to 200 ℃ at 5 ℃ / min, then increase it from 200 ℃ to 400 ℃ at 10 ℃ / min, hold it for 2 h, and then decrease it to 300 ℃ at 10 ℃ / min. The furnace was then cooled to room temperature to obtain Cu / GF-h-BN composite powder. (3) Spark plasma sintering The reduced Cu / GF-h-BN composite powder was ground and then added to a graphite mold (20 mm inner diameter, 60 mm outer diameter, and 70 mm height) wrapped in carbon paper. The Cu / GF-BN composite powder and the graphite mold were separated by carbon paper for easy sampling and demolding after sintering. The graphite mold was placed in the furnace cavity of a spark plasma sintering furnace and pre-compacted at 10 MPa. The tip of a thermocouple was inserted into the temperature measuring hole of the graphite mold. The furnace door was closed for vacuum treatment. After the furnace cavity reached the vacuum level, sintering was performed according to the set program as follows: the temperature was raised from room temperature to 600 °C and held for 5 min, then raised to 920 °C and held for 5 min, with a heating rate of 80-100 °C / min and a pre-compression pressure of 10 MPa. During the second stage of heating, the pressure was increased to 50 MPa and held for 5 min before cooling with the furnace. After sintering, the Cu / GF-h-BN composite material was obtained.

[0029] Example 3

[0030] The Cu / GF-h-BN composite material in this embodiment is processed by wet dispersion, ball milling, drying, reduction, and spark plasma sintering. The mass fraction of h-BN is 1.5%, the mass fraction of flake graphite is 8%, and the remainder is high-purity electrolytic Cu powder in the form of grape bunches with a purity of 99.999% and a particle size of 1-3 μm. The purity of h-BN powder is 99.8% with a particle size of 10,000 mesh, and the purity of flake graphite is 99.5% with a mesh size of 50 mesh.

[0031] The preparation method of Cu / GF-h-BN composite material in this embodiment is as follows: (1) Powder pretreatment Weigh out 45.25g of high-purity Cu powder and 4g of flake graphite, add them to a beaker, add anhydrous ethanol until the powder is completely submerged, then add 0.06g of sodium dodecyl benzoate. Place the beaker in a magnetic stirrer and stir at 25-35 ℃ for 6-8 hours. After thorough mixing, add anhydrous ethanol again until the powder is submerged. Load the slurry into a ball mill jar, add cemented carbide balls at a ball-to-powder ratio of 5:1. After assembly, fix the ball mill jar in a planetary ball mill and ball mill for 16 hours. After ball milling, add 0.75gh-BN powder and ultrasonically treat for 20 minutes. (2) High-temperature reduction The slurry after ball milling was taken out and placed in a beaker. The slurry residue on the ball mill jar wall and the surface of the alloy balls was repeatedly rinsed with anhydrous ethanol. The beaker was then placed in a drying oven for drying at 50-60 ℃ for 12 h. After drying, the obtained powder was ground and evenly spread on a ceramic sintering boat and placed in a tube furnace. Hydrogen gas was introduced at a flow rate of 300-350 ml / min to create a reducing atmosphere. The program was set to increase the temperature from room temperature to 200 ℃ at 5 ℃ / min, then increase it from 200 ℃ to 400 ℃ at 10 ℃ / min, hold it for 2 h, and then decrease it to 300 ℃ at 10 ℃ / min. The furnace was then cooled to room temperature to obtain Cu / GF-h-BN composite powder. (3) Spark plasma sintering The reduced Cu / GF-h-BN composite powder was ground and added to a graphite mold (the graphite mold has an inner diameter of 20 mm, an outer diameter of 60 mm, and a height of 70 mm, with carbon paper separating the Cu / GF-h-BN composite powder from the graphite mold for easy sampling and demolding after sintering) wrapped in carbon paper. The graphite mold was then placed in the furnace cavity of a spark plasma sintering furnace and pre-compacted at a pressure of 10 MPa. The tip of a thermocouple was inserted into the temperature measuring hole of the graphite mold. The furnace door was closed for vacuum treatment. After the furnace cavity reached the vacuum level, sintering was carried out according to the set program, which is as follows: the temperature was raised from room temperature to 600 ℃ and held for 5 min, then raised to 920 ℃ and held for 5 min, with a heating rate of 80-100 ℃ / min and a pre-compression pressure of 10 MPa. During the second stage of heating, the pressure was raised to 50 MPa and held for 5 min before cooling with the furnace. After sintering, Cu / GF-h-BN composite material was obtained.

[0032] Table 1 below shows Cu, Cu / GF-0.5% h-BN , Table of bulk friction coefficients for Cu / GF-1%h-BN and Cu / GF-1.5%h-BN. Formed by spark plasma sintering, these materials exhibit significantly improved tribological properties compared to pure copper. Furthermore, the lowest friction coefficient and optimal performance are achieved when the boron nitride mass fraction is 1%.

[0033] Table 1. Friction coefficient of the sample block

[0034] from Figure 1 It can be seen that the copper powder is spherical with a particle size of 1-3μm. The powder agglomerates into grape-like clusters and has a smooth surface.

[0035] from Figure 2As shown in the surface morphology images, the graphite reinforcing phase exhibits a distinct layered orientation within the copper matrix. The lamellar structure extends parallel along a specific direction, demonstrating good orientation, which is beneficial for constructing a directional reinforcing phase distribution structure and provides a microstructural basis for optimizing the composite material's performance. Simultaneously, high-magnification SEM observation reveals that the h-BN reinforcing phase is relatively uniformly distributed within the composite material without significant agglomeration, forming a multi-scale reinforcing structure together with the graphite lamellars. Furthermore, the interface continuity between graphite and the copper matrix is ​​good, with no obvious through-cracks or large-area interface debonding regions observed, indicating good bonding performance between the reinforcing phase and the copper matrix. These microstructures demonstrate that the copper-graphite-h-BN composite material prepared in this invention possesses good reinforcing phase orientation control, interfacial bonding performance, and microstructure uniformity, which is beneficial for obtaining copper-based materials with high tribological properties and high stability.

[0036] from Figure 3 As can be seen from the X-ray diffraction analysis diagram, diffraction peaks of various components can be found.

[0037] This invention incorporates h-BN, whose graphite-like layered crystal structure, low coefficient of friction, good high-temperature stability, and excellent chemical inertness enhance the tribological properties of copper-based alloys. Traditional ball milling easily generates a large amount of heat, and due to the softness of copper, copper powder tends to agglomerate, resulting in large particle sizes. This invention replaces powder with a suspension, using ethanol to transfer the heat generated during ball milling and isolating it from air. Sodium dodecylbenzoate is used as a dispersant, and an ultrasonic cleaner is employed to reduce powder agglomeration and accelerate the ball milling process. Spark plasma sintering technology refines the alloy's grain size through the combined effects of plasma activation and sintering densification, ultimately producing a dense Cu / GF-h-BN composite material with superior mechanical properties and wider applications.

[0038] The above embodiments are merely illustrative of specific implementations of this disclosure, but the implementations of this disclosure are not limited to the above content. Any changes, modifications, substitutions, combinations, or simplifications made without substantially departing from the spirit and principle of the inventive concept of this disclosure shall be considered equivalent substitutions and included within the scope of protection defined by the claims.

Claims

1. A method of making a boron nitride reinforced copper graphite composite material, characterized by: Specifically, the following steps are included: (1) Powder pretreatment High-purity Cu powder and flake graphite were weighed separately and added to a beaker in sequence. Anhydrous ethanol was added until the powder was completely submerged. Then, a dispersant was added. The beaker was placed in a magnetic stirrer and heated and stirred until fully mixed. Anhydrous ethanol was added again until the powder was submerged. The slurry was loaded into a ball mill jar, and cemented carbide balls were added. After assembly, the ball mill jar was fixed in a planetary ball mill for ball milling. After ball milling, the slurry was poured into a beaker. Hexagonal boron nitride powder was added to the beaker and the beaker was placed in an ultrasonic cleaner to fully disperse the agglomerated boron nitride powder, thus obtaining a Cu / GF-h-BN mixed slurry. (2) High-temperature reduction Take out the slurry after ball milling in step (1) and place it in a beaker. Place the beaker in a drying oven to dry it. Grind the dried powder evenly and spread it on a ceramic firing boat. Then place it in a tube furnace. After setting the program, perform reduction treatment in a hydrogen atmosphere. The tube furnace model is GSL-1200X. The program is set as follows: heat from room temperature to 200 ℃ at 5 ℃ / min, then heat from 200 ℃ to 400 ℃ at 10 ℃ / min, hold for 2 h, then reduce to 300 ℃ at 10 ℃ / min, and then cool to room temperature with the furnace to finally obtain Cu / GF-h-BN composite powder. (3) Spark plasma sintering The Cu / GF-h-BN composite powder reduced in step (2) was ground and added to a graphite mold. The graphite mold was placed in the furnace cavity of a spark plasma sintering furnace for pre-compactment. After setting the program, the furnace cavity was vacuum-treated and then sintered. After sintering, Cu / GF-h-BN composite material was obtained. The spark plasma sintering furnace was a LaboxTM-300 model. Thermocouple temperature measurement was used. The front end of the thermocouple was inserted into the temperature measuring hole of the graphite mold. The spark plasma sintering program was set as follows: the temperature was raised from room temperature to 600 ℃ and held for 5 min. Then the temperature was raised to 920 ℃ and held for 5 min. The heating rate was 80-100 ℃ / min. The pre-compression pressure was 10 MPa. During the second heating process, the pressure was raised to 50 MPa and held for 5 min before being cooled with the furnace.

2. The method of claim 1, wherein the boron nitride reinforced copper graphite composite is prepared by the steps of: In step (1), the mass fraction of h-BN powder is 0.5-1.5%, the mass fraction of flake graphite is 8%, and the remainder is high-purity Cu powder. The Cu powder is high-purity electrolytic Cu powder, which is grape-like in shape, with a purity of 99.999% and a particle size of 1-3 μm. The purity of h-BN powder is 99.8% and the particle size is 10,000 mesh. The purity of flake graphite is 99.5% and the particle size is 50 mesh. ​ 3. The preparation method of boron nitride-reinforced copper-graphite composite material as described in claim 1, characterized in that: In step (1), the magnetic stirrer is a DF-101S type heat-collecting magnetic stirrer with a stirring temperature of 25-35 ℃ and a stirring time of 6-8 h. In addition to an appropriate amount of anhydrous ethanol, sodium dodecyl benzoate is added to the beaker as a dispersant. The amount added depends on the dispersion of the mixed powder to promote more uniform powder dispersion.

4. The preparation method of boron nitride-reinforced copper-graphite composite material as described in claim 1, characterized in that: In step (1), the planetary ball mill is the Nanjing University Instruments QM-QX4 omnidirectional planetary ball mill with a ball milling speed (rotation speed) of 300 rpm, a ball-to-material ratio of 5:1, a ball milling time of 16 h, and the ball tank and the ball milling media balls are all made of hard alloy.

5. The preparation method of boron nitride-reinforced copper-graphite composite material as described in claim 1, characterized in that: In step (1), the ultrasonic cleaner is model FUYANG-F-030, and the ultrasonic time is 20 minutes.

6. The preparation method of boron nitride-reinforced copper-graphite composite material as described in claim 1, characterized in that: In step (2), the slurry after ball milling is taken out and placed in a beaker. The slurry residue on the ball milling tank wall and the surface of the alloy balls is repeatedly rinsed with anhydrous ethanol and then placed in a drying oven. The model of the drying oven is DHG-9000-9005, the drying temperature is 50-60 ℃, and the drying time is 12 h.

7. The preparation method of boron nitride-reinforced copper-graphite composite material as described in claim 1, characterized in that: The gas introduced in step (2) is hydrogen, and the introduction rate is 300-350 ml / min.

8. The preparation method of boron nitride-reinforced copper-graphite composite material as described in claim 1, characterized in that: In step (3), the graphite mold has an inner diameter of 20 mm, an outer diameter of 60 mm, and a height of 70 mm. Carbon paper is used to separate the Cu / GF-BN composite powder from the graphite mold to facilitate sampling and demolding after sintering.