Cu-ni alloy with gradient nanocrystalline structure and preparation method and application thereof
By constructing a Cu-Ni alloy with a gradient nanocrystalline structure, the problem of uneven corrosion film in chlorine-containing media of traditional alloys was solved, forming a dense oxide film and improving the corrosion resistance and service stability of the alloy.
Patent Information
- Application Number
- CN202611297977.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional coarse-grained Cu-Ni alloys tend to form loose, multi-layered corrosion product films in chlorine-containing media, making it difficult to stably obtain a dense nickel-rich passivation film, thus limiting their corrosion resistance.
By constructing a Cu-Ni alloy with a gradient nanocrystalline structure, a gradient grain refinement layer is formed on the alloy surface through surface strong plastic deformation treatment, and a single-layer, ultrathin, and nickel-rich dense oxide film is formed in a chlorine-containing corrosion environment, thereby improving the self-passivation capability.
It significantly improves the corrosion resistance of the alloy, reduces the corrosion current density, and enhances its service stability and self-passivation ability in chlorine-containing environments.
Smart Images

Figure CN123108356A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of surface engineering and corrosion resistance technology of metallic materials, specifically to a Cu-Ni alloy with a gradient nanocrystalline structure, its preparation method, and its application. Background Technology
[0002] Cu-Ni alloys are widely used in shipbuilding, marine engineering, and chemical equipment due to their excellent mechanical properties and resistance to marine corrosion. However, traditional coarse-grained Cu-Ni alloys tend to form loose, thick, and multi-layered corrosion product films in chlorine-containing media. These films have an inhomogeneous structure and numerous ion transport channels, making it difficult to effectively prevent the continuous corrosion reaction and thus limiting their service life in harsh corrosive environments. Existing research has shown that grain refinement can improve material properties to some extent, but how to stably form a highly dense, high-nickel-content, and ultra-thin oxide film structure remains a key problem that urgently needs to be solved in current technology. Summary of the Invention
[0003] This invention addresses the problem that existing Cu-Ni alloys easily form loose, multi-layered corrosion product films and are difficult to stably obtain dense, nickel-rich passivation films in chloride-containing corrosive environments, thus limiting their corrosion resistance. It provides a Cu-Ni alloy with a gradient nanocrystalline structure, its preparation method, and its applications. By constructing a Cu-Ni alloy with a gradient nanocrystalline structure through strong plastic deformation of the surface, the gradient nanocrystalline structure is used to regulate the oxidation behavior of the alloy surface, promoting the spontaneous formation of a single-layer, ultrathin, and nickel-rich dense oxide film in natural oxidation or corrosive environments. This significantly improves the self-passivation capability and corrosion resistance of the Cu-Ni alloy.
[0004] In a first aspect, the present invention provides a Cu-Ni alloy having a gradient nanostructure, the Cu-Ni alloy comprising an alloy matrix and a gradient grain refinement layer located on the surface of the alloy matrix; wherein, The mass fraction of Ni in the Cu-Ni alloy is 20 wt.%~40 wt.%. The gradient grain refinement layer includes, from the outside to the inside, a nanocrystalline region, an ultrafine crystalline region, and a dislocation structure region. Each region transitions continuously, and the grain size gradually increases from the outside to the inside along the thickness direction. The average grain size of the nanocrystalline region is 50 nm to 100 nm.
[0005] Furthermore, the total thickness of the gradient grain refinement layer is 50 μm to 120 μm.
[0006] Furthermore, the proportion of high-angle grain boundaries >15° in the nanocrystalline region is 70%~85%.
[0007] Furthermore, the Cu-Ni alloy is exposed to air or a chlorine-containing corrosive medium and subjected to polarization treatment at a voltage 50 mV to 100 mV above its open-circuit potential to form an oxide film with a thickness of 1 nm to 5 nm on the surface. The oxide film contains more than 40% nickel atomic content and nickel mainly exists in the form of NiO.
[0008] A second aspect of the present invention provides a method for preparing the above-described Cu-Ni alloy, comprising the following steps: Step 1: Perform surface strong plastic deformation treatment on a Cu-Ni alloy matrix with a Ni mass fraction of 20 wt.%~40 wt.% to construct a gradient grain refinement layer on the alloy surface. The gradient grain refinement layer consists of a nanocrystalline region, an ultrafine grain region, and a dislocation structure region from the outside to the inside, with continuous transitions between each region and the grain size gradually increasing from the outside to the inside along the thickness direction; control the average grain size of the nanocrystalline region to be 50 nm~100 nm. Step 2: Remove the surface deformation layer from the alloy treated in Step 1.
[0009] Furthermore, in step 1, the surface strong plastic deformation treatment is performed by surface mechanical rolling and / or surface mechanical grinding.
[0010] Furthermore, in step 2, the surface deformation layer removal process is performed by mechanical polishing and / or ion beam treatment.
[0011] Furthermore, the surface deformation layer removal process removes a layer with a thickness of 300 nm to 500 nm.
[0012] A third aspect of the present invention provides the application of the above-described Cu-Ni alloy in marine engineering structural components, ship equipment structural components, structural components for chlorine-containing corrosive environments, or heat exchange equipment.
[0013] Furthermore, the Cu-Ni alloy forms an oxide film on its surface in a chlorine-containing corrosive environment, and the corrosion resistance of the oxide film is superior to that of a surface film formed by a coarse-grained Cu-Ni alloy of the same composition under the same conditions.
[0014] Compared with the prior art, the present invention has at least the following beneficial effects: (1) By constructing a gradient nanostructure and removing the surface deformation damage layer, the Cu-Ni alloy can be promoted to form a nickel-rich, dense, ultrathin oxide film mainly composed of NiO in a chlorine-containing corrosive medium, which significantly improves the corrosion resistance of the alloy.
[0015] (2) Within a range of 50 mV to 100 mV above its open-circuit potential, the nanocrystalline alloy exhibits a significant passivation region, with a passivation current density reaching 10 mV. -8 A / cm2 The corrosion current density of nanocrystalline alloys is close to that of typical passive materials such as stainless steel and titanium alloys. Compared with coarse-grained alloys, nanocrystalline alloys have a lower corrosion current density, and the passivation current density, which reflects the film protection capability, is reduced by about 20 times. The alloy of this invention exhibits superior self-passivation capability and long-term service stability in chlorine-containing environments.
[0016] (3) The oxide film formed by the nanocrystalline structure is more uniform and dense, thus significantly improving the long-term service stability.
[0017] (4) The preparation method of the present invention is simple and highly controllable, and is suitable for engineering application. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments recorded in the embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings.
[0019] Figure 1 This is a microstructure diagram of the surface layer of a Cu-Ni alloy with a gradient nanocrystalline structure provided in Embodiment 1 of the present invention.
[0020] Figure 2 The image shown is a TKD image of Example 1 of the present invention, displaying the grain size and grain boundary type of the Cu-30Ni alloy of Example 1.
[0021] Figure 3 The images shown are TEM characterization composite images of the nickel-rich ultrathin oxide film formed on the surface of the Cu-Ni alloy with a gradient nanocrystalline structure provided in Example 1 of the present invention; wherein, a is a high-resolution HAADF-STEM image; b is an EDS elemental surface distribution map; and c is an EDS line scan elemental composition distribution map.
[0022] Figure 4 This is a schematic diagram comparing the corrosion resistance of the gradient nanocrystalline Cu-Ni alloy and the coarse-grained Cu-Ni alloy provided in Embodiment 1 of the present invention; wherein, a is a potentiodynamic polarization curve; b is a constant potential polarization curve; c is a Bode plot; and d is a Nernquist plot.
[0023] Figure 5 The X-ray photoelectron spectroscopy (XPS) of the passivation film formed by the gradient nanocrystalline Cu-Ni alloy provided in Example 1 of this invention in a 3.5 wt.% NaCl electrolyte at -150 mV / SCE is shown. Here, a is the Cu LMM spectrum; b is the Ni 2p3 / 2 spectrum; and c is the O 1s spectrum. This indicates that the Ni content in the film is mainly in the form of NiO, accounting for approximately 66%.
[0024] Figure 6 The potentiodynamic polarization curves are for nanocrystals (green line), ultrafine grains (blue line), and coarse grains (red line) of Cu-10Ni alloy in Comparative Example 1 in 3.5 wt.% NaCl.
[0025] Figure 7 The potentiostatic polarization curves of Cu-10Ni alloy nanocrystals (green line) and coarse grains (red line) of Comparative Example 1 are shown under the condition of constant potential -100mV / SCE in 3.5 wt.% NaCl.
[0026] Figure 8 The TKD image for Comparative Example 2 of this invention shows the grain size and grain boundary type of the Cu-30Ni alloy in Comparative Example 2.
[0027] Figure 9 The high-magnification HAADF-STEM image of Comparative Example 2 of this invention shows that under constant potential of -150mV / SCE in 3.5 wt.% NaCl, the passivation film of the Cu-30Ni alloy ultrafine grains in Comparative Example 2 is about 5 nm, and there is no Ni enrichment in the film.
[0028] Figure 10 The TKD image for Comparative Example 3 of this invention shows the grain size and grain boundary type of the Cu-30Ni alloy in Comparative Example 3.
[0029] Figure 11 The high-magnification HAADF-STEM image of Comparative Example 3 of this invention shows the corrosion product particles of the fine grains of Cu-30Ni alloy in Comparative Example 3 under constant potential -150mV / SCE conditions in 3.5 wt.% NaCl.
[0030] Figure 12 This is a high-magnification HAADF-STEM image of Comparative Example 4 of the present invention, showing the surface damage layer structure of the Cu-30Ni alloy in Comparative Example 4.
[0031] Figure 13 The high-magnification HAADF-STEM image of Comparative Example 4 of this invention shows the compositional distribution of the damage layer structure on the surface of the Cu-30Ni alloy in Comparative Example 4.
[0032] Figure 14 The present invention provides potentiodynamic polarization curves for the nanocrystals (green line) of Cu-30Ni alloy with deformation layer damage removed in Example 1, the nanocrystals (blue line) of Comparative Example 4 without deformation layer damage removed, and the coarse grains (red line) in 3.5 wt.% NaCl. Detailed Implementation
[0033] To better understand the above technical solutions, the technical solutions of the embodiments of this application will be described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the embodiments of this application and the specific features in the embodiments are detailed descriptions of the technical solutions of the embodiments of this application, rather than limitations on the technical solutions of this application. In the absence of conflict, the embodiments of this application and the technical features in the embodiments can be combined with each other.
[0034] A first aspect of the present invention provides a Cu-Ni alloy with a gradient nanostructure, comprising an alloy matrix and a gradient grain refinement layer located on the surface of the alloy matrix; wherein, The mass fraction of Ni in the Cu-Ni alloy is 20 wt.%~40 wt.%; The gradient grain refinement layer consists of a nanocrystalline region, an ultrafine crystalline region, and a dislocation structure region from the outside to the inside. Each region transitions continuously, and the grain size gradually increases from the outside to the inside along the thickness direction. The average grain size of the nanocrystalline region is 50 nm to 100 nm.
[0035] The Cu-Ni alloy with a gradient nanostructure in this invention exhibits higher film impedance and charge transfer resistance compared to traditional coarse-grained Cu-Ni alloys, significantly reducing corrosion current density and demonstrating excellent self-passivation capability and corrosion resistance. Using a fully automated micro Vickers hardness tester, the outermost surface hardness of the Cu-Ni alloy is characterized to be greater than 3 GPa, showing a continuous gradient decrease along the thickness direction. This higher surface hardness allows for rapid characterization of the surface grain refinement effect.
[0036] In some embodiments, the total thickness of the gradient grain refinement layer is 50 μm to 120 μm, wherein the thickness of the nanocrystalline region is 5 μm to 20 μm.
[0037] Specifically, the total thickness of the gradient grain refinement layer is controlled to be 50 μm to 120 μm, and the thickness of the nanocrystalline region is 5 μm to 20 μm. On the one hand, this ensures the refinement effect of the surface grains, and on the other hand, a sufficiently thick nanocrystalline region can still be retained after the surface deformation layer is removed.
[0038] In some embodiments, the proportion of high-angle grain boundaries >15° in the nanocrystalline region is 70%~85%, which makes the outermost surface of the gradient grain refinement layer have high-density high-angle grain boundary exposure characteristics. A higher proportion of high-angle grain boundary exposure is beneficial to the formation of nickel-rich passivation film.
[0039] In some embodiments, the Cu-Ni alloy is exposed to air or a chlorine-containing corrosive medium and subjected to polarization treatment at a voltage 50 mV to 100 mV above its open circuit potential to form a crystalline oxide film with a thickness of 1 nm to 5 nm on the surface. The oxide film contains more than 40% nickel atomic content, and the nickel exists mainly in the form of NiO, supplemented by Cu2O and / or Cu(OH)2.
[0040] A second aspect of the present invention provides a method for preparing the above-described Cu-Ni alloy with a gradient nanostructure, comprising the following steps: Step 1: Perform surface strong plastic deformation treatment on Cu-Ni alloy matrix with Ni mass fraction of 20 wt.%~40 wt.% to construct a gradient grain refinement layer on the alloy surface. The gradient grain refinement layer consists of nanocrystalline region, ultrafine grain region and dislocation structure region from the outside to the inside. The transition between each region is continuous, and the grain size gradually increases from the outside to the inside along the thickness direction. The average grain size of the nanocrystalline region is 50 nm~100 nm. Step 2: The alloy treated in Step 1 is subjected to surface deformation layer removal treatment to eliminate the surface roughness and non-uniform deformation damage layer introduced by strong plastic deformation, and to expose the nanocrystalline region on the alloy surface.
[0041] The method for preparing Cu-Ni alloy with gradient nanostructure in this invention promotes the formation of a nickel-rich, dense, ultrathin oxide film mainly composed of NiO in a chlorine-containing corrosive medium by constructing a gradient nanostructure and removing the surface deformation and damage layer, thereby significantly improving the corrosion resistance of the alloy.
[0042] In some embodiments, in step 1, the surface undergoes strong plastic deformation treatment, which includes surface mechanical rolling and / or surface mechanical grinding.
[0043] Specifically, surface mechanical rolling and / or surface mechanical grinding can significantly improve surface hardness and wear resistance, and also obtain deeper gradient nanostructure layers.
[0044] In some embodiments, step 2 involves removing the surface deformation layer, which includes mechanical polishing and / or ion beam treatment to prevent the non-uniform strain layer from introducing structural defects. Optionally, mechanical polishing can be performed using a 0.1 μm SiO2 polishing slurry, or the surface deformation layer can be treated using an ion polishing instrument.
[0045] In some embodiments, the surface deformation layer is removed, with a thickness of 300 nm to 500 nm.
[0046] Understandably, experiments have shown that the depth of the surface deformation layer is generally less than 300 nm. Therefore, the thickness of the removal layer is controlled to be 300 nm to 500 nm so that the alloy surface exposes nanocrystalline regions with a high-angle grain boundary ratio of 70% to 85%.
[0047] A third aspect of this invention provides the application of the above-described Cu-Ni alloy with a gradient nanostructure in marine engineering components, ship equipment, structural components in chlorine-corrosion environments, or heat exchange equipment. The Cu-Ni alloy with the gradient nanostructure forms an oxide film on its surface in a chlorine-corrosion environment, and the corrosion resistance of this oxide film is superior to that of a surface film formed by a coarse-grained Cu-Ni alloy of the same composition under the same conditions.
[0048] Specifically, compared with traditional coarse-grained Cu-Ni alloys, Cu-Ni alloys with gradient nanostructures exhibit higher film impedance and charge transfer resistance, significantly reduce corrosion current density, and possess excellent self-passivation ability and corrosion resistance, making them suitable for marine engineering and structural components in chlorine-containing corrosive environments.
[0049] Example 1: Preparation and characterization of Cu-Ni alloy with gradient nanocrystalline structure 1. Preparation method The preparation method of this embodiment includes, in sequence, surface strong plastic deformation treatment and surface deformation layer removal treatment.
[0050] A Cu-Ni alloy is selected as the base material, with a nickel content of 30 wt.%. The alloy material can be in the form of plates or bars, and its surface is subjected to routine degreasing and cleaning treatment before implementation.
[0051] Step 1: Surface Strong Plastic Deformation Treatment First, the Cu-Ni alloy surface undergoes a surface hardening and plastic deformation treatment. The treatment method can be one of surface mechanical rolling, surface mechanical grinding, or a combination thereof. This embodiment uses a surface mechanical rolling process with the following specific parameters: the Cu-Ni alloy rod sample is placed in liquid nitrogen and rotated at 400 rpm; an 8 mm diameter WC / Co hemispherical needle tip is inserted into the sample surface and slid along the length of the Cu-Ni alloy rod sample at a feed speed of 8 mm / min, with each indentation depth of 20 μm. The same surface is subjected to 10 repeated rolling treatments.
[0052] Step 2: Remove the surface deformation layer The Cu-Ni alloy subjected to the above-mentioned strong plastic deformation treatment is then subjected to surface treatment to remove the deformation damage layer on its surface. The removal method can be mechanical polishing, ion beam treatment, or a combination of both. In this embodiment, mechanical polishing is used to perform a light polishing treatment on the alloy surface, removing a surface material with a thickness of 300 nm to 500 nm to eliminate the surface roughness and non-uniform deformation damage layer introduced by the strong plastic deformation.
[0053] 2. Characterization (1) Gradient nanocrystalline structure Through the aforementioned strong plastic deformation treatment, a gradient nanostructure refinement layer is formed on the surface of the Cu-Ni alloy, consisting of nanocrystalline regions, ultrafine crystalline regions, and dislocation structure regions distributed sequentially from the outside in. For example... Figure 1 and Figure 2 As shown, microstructural analysis reveals that the average grain size of the outermost nanocrystalline region of the alloy is 50 nm to 100 nm, the region thickness is 5 μm to 20 μm, the proportion of high-angle grain boundaries in the nanocrystalline region is 70% to 85%, and the grain boundary density is significantly higher than that in the coarse-grained region of the alloy. The grain size gradually increases inward along the thickness direction, and the total thickness of the gradient nanocrystalline refinement layer is 50 μm to 120 μm.
[0054] (2) Characteristics of surface oxide film The gradient nanocrystalline Cu-Ni alloy treated in step 2 was exposed to a chloride-containing corrosive medium and subjected to constant potential polarization for 2 h at a voltage 50 mV–100 mV above its open-circuit potential to form an oxide film. Subsequently, the microstructure was observed using HAADF-STEM, and its elemental distribution was analyzed using energy dispersive spectroscopy. Figure 3 As shown, a continuous, dense, and uniform ultrathin oxide film was formed on the alloy surface, with a thickness of approximately 1 nm to 5 nm, exhibiting a monolayer structure or being predominantly monolayer. Energy dispersive spectroscopy (EDS) analysis revealed that the atomic percentage of Ni in the oxide film exceeded 40%, significantly higher than the Ni content in the substrate; simultaneously, the Cu content decreased significantly, to only about 30%, indicating that Ni preferentially enriched in the film during oxidation, while Cu was selectively repelled. Further X-ray photoelectron spectroscopy (XPS) analysis of the oxide film, such as... Figure 5 As shown, Ni in the film mainly exists in the form of NiO, accounting for about 66% of the total Ni species; while Cu mainly exists in the form of Cu(OH)2.
[0055] (3) Corrosion resistance test The gradient nanocrystalline Cu-Ni alloy obtained in this embodiment was compared with a coarse-grained Cu-Ni alloy of the same composition, and its electrochemical corrosion performance was tested in a chlorine-containing electrolyte environment. Figure 4As shown in Figure a, the potentiodynamic polarization curves indicate that the passivation film formed by the Cu-Ni alloy of this invention in a chlorine-containing corrosive medium exhibits higher corrosion resistance. Its corrosion current density is significantly lower than that of the coarse-grained Cu-Ni alloy, demonstrating superior corrosion resistance. Its passivation current density can reach 10... -8 A / cm 2 Magnitude. For example... Figure 4 As shown in b, the current-time curves after constant potential polarization indicate that the current in the gradient nanocrystalline alloy rapidly decays and remains at an extremely low level during polarization, exhibiting more stable passivation behavior. Figure 4 As shown in c-4d, the electrochemical impedance spectroscopy indicates that, compared with traditional coarse-grained Cu-Ni alloys, Cu-Ni alloys with gradient nanostructures exhibit higher film impedance and charge transfer resistance, significantly reduce corrosion current density, and possess excellent self-passivation ability and corrosion resistance, making them suitable for marine engineering and structural components in chlorine-containing corrosive environments.
[0056] Comparative Example 1 1. Preparation method The difference from Example 1 is that the Ni mass fraction in the Cu-Ni alloy is 10 wt.%.
[0057] 2. Characterization like Figure 6 As shown, there is no significant difference in the potentiodynamic polarization curves of nanocrystals, ultrafine grains, and coarse grains in the Cu-Ni alloy with gradient nanocrystal structure obtained in Comparative Example 1.
[0058] like Figure 7 As shown, when a constant potential polarization of -100mV / SCE is selected, the current density of nanocrystals is even higher than that of coarse crystals, and the corrosion resistance obviously decreases significantly.
[0059] Comparative Example 2 1. Preparation method The difference from Example 1 is that in step 1, the same surface is subjected to six repeated rolling processes.
[0060] 2. Characterization like Figure 8 As shown, the Cu-Ni alloy of Comparative Example 2 was refined to 300 nm~500 nm after surface strong plastic deformation treatment.
[0061] like Figure 9 As shown, the Cu-Ni alloy prepared in Comparative Example 2 was placed in a 3.5 wt.% NaCl solution and polarized at a constant potential of -150 mV / SCE. The results showed that a passivation film with a thickness of approximately 5 nm was formed on the surface of the Cu-Ni alloy in Comparative Example 2, and no enrichment of Ni element was observed in the film.
[0062] Comparative Example 3 1. Preparation method The difference from Example 1 is that in step 1, the same surface is subjected to repeated rolling treatment three times.
[0063] 2. Characterization like Figure 10 As shown, the Cu-Ni alloy in Comparative Example 3, after surface strong plastic deformation treatment, had its grains refined to the micrometer level.
[0064] like Figure 11 As shown, the Cu-Ni alloy prepared in Comparative Example 3 was placed in a 3.5 wt.% NaCl solution and polarized at a constant potential of -150 mV / SCE. The results showed that a passivation film no longer formed on the surface of the Cu-Ni alloy in Comparative Example 3; instead, a thicker layer of corrosion product particles was formed, and such a film did not possess corrosion resistance.
[0065] Comparative Example 4 1. Preparation method The difference from Example 1 is that the "removal of the surface deformation layer" was not performed.
[0066] 2. Characterization After surface hard plastic deformation treatment, a surface deformation layer is inevitably introduced into the outermost layer of the alloy. If this deformation layer is removed (as in Example 1), a stable nanocrystalline structure dominated by high-angle grain boundaries is exposed; if it is not removed (as in Comparative Example 4), a large number of defect structures are retained in the outermost layer, such as... Figure 12 and Figure 13 As shown, these defect sites are not only unfavorable for the formation of nickel-rich passivation films, but also tend to become preferred sites for corrosion initiation.
[0067] Figure 14 The potentiodynamic polarization curves of Cu-30Ni alloys in different states in 3.5 wt.% NaCl solution are shown. The results show that the open circuit potential of the nanocrystals (blue line) without the removal of the surface deformation layer is basically the same as that of the coarse grains (red line), and they do not show a significant passivation zone similar to that of the nanocrystals with the surface deformation layer removed (green line), indicating that their corrosion resistance has not been substantially improved.
[0068] It will be readily understood by those skilled in the art that the above-described advantageous methods can be freely combined and superimposed without conflict. The above are merely preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application. The above are merely preferred embodiments of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of this application, and these improvements and modifications should also be considered within the protection scope of this application.
Claims
1. A Cu-Ni alloy with a gradient nanostructure, characterized in that, The Cu-Ni alloy consists of an alloy matrix and a gradient grain refinement layer located on the surface of the alloy matrix; wherein... The mass fraction of Ni in the Cu-Ni alloy is 20 wt.%~40 wt.%. The gradient grain refinement layer includes, from the outside to the inside, a nanocrystalline region, an ultrafine crystalline region, and a dislocation structure region. Each region transitions continuously, and the grain size gradually increases from the outside to the inside along the thickness direction. The average grain size of the nanocrystalline region is 50 nm to 100 nm.
2. The Cu-Ni alloy according to claim 1, characterized in that, The total thickness of the gradient grain refinement layer is 50 μm to 120 μm.
3. The Cu-Ni alloy according to claim 1, characterized in that, The proportion of high-angle grain boundaries >15° in the nanocrystalline region is 70%~85%.
4. The Cu-Ni alloy according to claim 1, characterized in that, The Cu-Ni alloy is exposed to air or a chlorine-containing corrosive medium and subjected to polarization treatment at a voltage 50 mV to 100 mV above its open circuit potential to form an oxide film with a thickness of 1 nm to 5 nm on its surface. The oxide film contains more than 40% nickel atomic content and nickel mainly exists in the form of NiO.
5. A method for preparing a Cu-Ni alloy with a gradient nanostructure, characterized in that, Includes the following steps: Step 1: Perform surface strong plastic deformation treatment on a Cu-Ni alloy matrix with a Ni mass fraction of 20 wt.%~40 wt.% to construct a gradient grain refinement layer on the alloy surface. The gradient grain refinement layer consists of a nanocrystalline region, an ultrafine grain region, and a dislocation structure region from the outside to the inside, with continuous transitions between each region and the grain size gradually increasing from the outside to the inside along the thickness direction; control the average grain size of the nanocrystalline region to be 50 nm~100 nm. Step 2: Remove the surface deformation layer from the alloy treated in Step 1.
6. The preparation method according to claim 5, characterized in that, In step 1, the surface strong plastic deformation treatment is performed by surface mechanical rolling and / or surface mechanical grinding.
7. The preparation method according to claim 5, characterized in that, In step 2, the surface deformation layer removal process is carried out by mechanical polishing and / or ion beam treatment.
8. The method for preparing Cu-Ni alloy according to claim 7, characterized in that, The surface deformation layer removal process removes a layer with a thickness of 300 nm to 500 nm.
9. The application of the Cu-Ni alloy according to any one of claims 1-4 in marine engineering structural components, ship equipment structural components, structural components in chlorine-containing corrosive environments, or heat exchange equipment.
10. The application of the Cu-Ni alloy with a gradient nanostructure according to claim 9, characterized in that, The Cu-Ni alloy forms an oxide film on its surface in a chlorine-containing corrosive environment, and the corrosion resistance of the oxide film is superior to that of a surface film formed by a coarse-grained Cu-Ni alloy of the same composition under the same conditions.