A titanium-based cermet with a multilayer micro / nano gradient structure and its preparation method

By constructing a multi-layered micro-nano gradient core-ring structure inside hard phase particles, the problem of insufficient strength and toughness of Ti(C,N)-based cermets was solved, and the efficient preparation and application of high-hardness materials were realized.

CN123108384APending Publication Date: 2026-11-17SHIZUISHAN VOCATIONAL & TECH COLLEGE OF IND & TRADE (NINGXIA IND SCHOOL SHIZUISHAN VOCATIONAL EDUCATION CENT NORTHWEST COAL MINING MASCH MFG ADVANCED TECH COLLEGE)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611369260.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing Ti(C,N)-based cermets mostly have single-layer or non-gradient core-ring structures. The number of ring phase layers is limited, and the lack of compositional gradient control results in low material strength and toughness, which restricts their widespread application.

Method used

A multi-layered micro-nano gradient core-ring structure with two or more layers is constructed inside the hard phase particles. The compositional gradient distribution of the ring phase is controlled by graded ball milling and gradient sintering processes. Multiple elements such as Mo, W, Ta, and Nb are dissolved in Ti (C, N), and the nitrogen partial pressure of the atmosphere is controlled during the sintering process to achieve the gradient distribution of the multi-layered ring phase.

Benefits of technology

It significantly improves the bending strength and fracture toughness of Ti(C,N)-based cermets by more than 30%, while maintaining high hardness and facilitating mass production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention proposes a titanium-based cermet with a multi-layered micro-nano gradient structure and its preparation method. The cermet comprises a hard phase and a binder phase. The hard phase particles contain two or more annular phases, each annular phase exhibiting a compositional gradient distribution from the inside to the outside. The number of annular phase layers is 2 to 5. This invention effectively alleviates the internal stress between the core and ring structures by constructing two or more multi-layered micro-nano gradient core-ring structures within the hard phase particles, enabling each annular phase to exhibit a compositional gradient distribution from the inside to the outside. Through a graded ball milling combined with gradient sintering, the preparation process is highly compatible with existing powder metallurgy production lines, requiring no additional expensive equipment and facilitating large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal ceramic materials technology, and in particular to a titanium-based metal ceramic with a multilayer micro-nano gradient structure and its preparation method. Background Technology

[0002] Ti(C,N)-based cermets are a type of composite material produced by powder metallurgy. Using TiC, TiN, or Ti(C,N) as the hard phase matrix, transition metals (such as Ni and Co) are added as the binder phase, along with secondary carbides such as Mo₂C, WC, TaC, and NbC. The mixture is then pressed and sintered. Ti(C,N)-based cermets possess advantages such as high hot hardness, good wear resistance, low coefficient of friction, and good chemical stability, and are considered an important alternative to WC-Co cemented carbides. Their microstructure mainly consists of a binder phase and a hard phase. The edges of the hard phase particles typically form a coating layer composed of elements such as Mo, W, Ta, and Nb dissolved in Ti(C,N), known as a ring phase or core-ring structure.

[0003] The core-ring structure of Ti(C,N)-based cermets has a decisive influence on their mechanical properties. During high-temperature sintering, the core-ring structure formed through the Ostwald dissolution-precipitation mechanism can prevent crack propagation and achieve a toughening effect. However, in traditional Ti(C,N)-based cermets, the core-ring structure is mostly a simple single-layer or non-gradient structure, and the composition, thickness, and number of ring phases are difficult to precisely control. While existing technologies exist for preparing submicron-scale core-ring structure cermets by controlling the particle size of raw material powders and sintering processes, and for forming mixed-crystal structures by combining two different particle sizes of Ti(C,N), the core-ring structures obtained by these methods are still mainly single-layer or bilayer, with a limited number of ring phase layers and a lack of effective control over the compositional gradient within the ring phase. Furthermore, while gradient Ti(C,N)-based cermet materials have been reported, their gradient is mainly reflected in the change in the mass percentage of the binder phase from the outside to the inside, rather than the multi-layer gradient construction of the core-ring structure within the hard phase grains.

[0004] Ti(C,N)-based cermets generally exhibit lower strength and toughness than WC-Co cemented carbides. This lower strength and toughness makes the material prone to microcracks during processing, thus reducing its service life and severely hindering its widespread application. The internal stress between the core and ring structures is one of the important reasons for the poor strength and toughness of Ti(C,N)-based cermets. Therefore, how to significantly improve the fracture toughness and bending strength of materials while maintaining high hardness through the refined design and control of the core-ring structure is a technical challenge that urgently needs to be solved in this field. Summary of the Invention

[0005] This invention proposes a titanium-based cermet with a multilayer micro-nano gradient structure and its preparation method. The cermet comprises a hard phase and a binder phase. The hard phase particles have two or more annular phases inside, and each annular phase has a compositional gradient distribution from the inside to the outside. The number of annular phase layers is 2 to 5.

[0006] Furthermore, the annular phase is formed by solid dissolving one or more elements selected from Mo, W, Ta, and Nb in Ti(C,N); from the inside out, the content of W and / or Mo elements in each layer of the annular phase shows a gradient increasing or decreasing distribution, while the content of N element shows the opposite gradient change.

[0007] Furthermore, the particle size of the hard phase particles is 0.2~2.0μm; the binder phase is one or both of Ni and Co, and the mass percentage of the binder phase is 8%~25%.

[0008] The present invention also provides a method for preparing the above-mentioned Ti(C,N)-based cermet with a multilayer micro / nano gradient core-ring structure, comprising the following steps: (1) Raw material preparation: Weigh Ti(C,N) powder, carbide additive phase powder and metal binder phase powder; the carbide additive phase powder is selected from one or more of Mo2C, WC, TaC and NbC; (2) Graded ball milling: The raw material powder from step (1) is subjected to graded ball milling. First, it is coarsely ground with the first ball milling parameters, and then finely ground with the second ball milling parameters to obtain a mixed slurry. (3) Drying and granulation: The mixed slurry from step (2) is vacuum dried, sieved and granulated to obtain mixed powder; (4) Press molding: The mixed powder from step (3) is pressed into a mold to obtain a shaped blank; (5) Gradient sintering: The formed blank from step (4) is subjected to gradient sintering under atmosphere protection. The gradient sintering includes a heating stage, a holding stage and a cooling stage. During the holding stage and / or cooling stage, the nitrogen partial pressure of the atmosphere is controlled to be 0.5~2.0 kPa, the holding temperature is 1350~1500℃, and the holding time is 0.5~3 hours. (6) After cooling, Ti(C,N)-based metal ceramics with multi-layer micro-nano gradient core-ring structure are obtained.

[0009] Further, the particle size of the Ti(C,N) powder in step (1) is 0.2~1.0μm, the particle size of the carbide additive phase powder is 0.1~0.8μm, and the particle size of the metal binder phase powder is 0.5~2.0μm.

[0010] Further, the graded ball milling in step (2) is as follows: first, ball milling at a speed of 200~400 r / min for 2~6 hours, and then ball milling at a speed of 100~200 r / min for 8~24 hours.

[0011] Furthermore, the heating rate in step (5) is 5~15℃ / min during the heating stage, and the cooling rate in the cooling stage is 3~10℃ / min.

[0012] Further, the atmosphere described in step (5) is nitrogen, argon, or a mixture of nitrogen and argon.

[0013] The present invention also provides the application of Ti(C,N)-based cermets with multilayer micro-nano gradient core-ring structures prepared by the above preparation method in cutting tools, molds or wear-resistant parts.

[0014] This invention constructs a multi-layered micro-nano gradient core-ring structure with two or more layers inside hard phase particles, so that the ring phases in each layer are distributed in a compositional gradient from the inside to the outside, which effectively relieves the internal stress between the core-ring structures. By using a graded ball milling combined with gradient sintering process, the preparation process is highly compatible with existing powder metallurgy production lines, does not require additional expensive equipment, and is easy to achieve large-scale production.

[0015] The Ti(C,N)-based cermet prepared by this invention maintains high hardness (≥92 HRA) while improving bending strength and fracture toughness by more than 30% compared with traditional single-layer core-ring structure materials. Detailed Implementation

[0016] Example 1 Raw material ratio (mass percentage): Ti(C,N) powder (particle size 0.5μm) 50%, WC powder (particle size 0.3μm) 15%, Mo2C powder (particle size 0.3μm) 10%, Ni powder (particle size 1.0μm) 20%, Co powder (particle size 1.0μm) 5%.

[0017] Preparation method: (1) Weigh the above raw material powder according to the ratio and put it into the ball mill jar. Add anhydrous ethanol as the ball milling medium. The ball-to-material ratio is 8:1. (2) Classification ball milling: First, ball mill at a speed of 300 r / min for 4 hours, and then ball mill at a speed of 150 r / min for 16 hours to obtain a mixed slurry; (3) The mixed slurry was vacuum dried at 80°C for 12 hours and granulated through a 200-mesh sieve to obtain mixed powder; (4) The mixed powder is unidirectionally cold-pressed in a mold at a pressure of 200 MPa and held for 30 seconds to obtain a shaped blank; (5) The formed blank is placed in a vacuum sintering furnace and heated to 1420°C at a heating rate of 10°C / min. It is then held at 1420°C for 1.5 hours. During the holding period, nitrogen gas is introduced to control the nitrogen partial pressure to 1.0 kPa. Then, it is cooled to room temperature at a cooling rate of 5°C / min to obtain Ti(C,N)-based metal ceramics with a three-layer micro-nano gradient core-ring structure.

[0018] The product obtained in this embodiment was subjected to microstructural observation and mechanical property testing. Scanning electron microscopy (SEM) observation showed that the hard phase particles had a clear three-layer ring-shaped phase structure. From the innermost to the outermost ring-shaped phases, the content of W and Mo elements increased in a gradient, while the content of N element decreased in a gradient. The Ti(C,N)-based cermet obtained in this embodiment was tested to have a hardness of 93.2 HRA, a flexural strength of 1850 MPa, and a fracture toughness of 12.8 MPa·m. 1 / 2 .

[0019] Example 2 Raw material ratio (mass percentage): Ti(C,N) powder (particle size 0.3μm) 45%, WC powder (particle size 0.2μm) 18%, Mo2C powder (particle size 0.2μm) 12%, TaC powder (particle size 0.2μm) 5%, Ni powder (particle size 0.8μm) 15%, Co powder (particle size 0.8μm) 5%.

[0020] Preparation method: (1) Weigh the above raw material powder according to the ratio and put it into the ball mill jar. Add anhydrous ethanol as the ball milling medium. The ball-to-material ratio is 10:1. (2) Classification ball milling: First, ball mill at a speed of 350 r / min for 3 hours, and then ball mill at a speed of 120 r / min for 20 hours to obtain a mixed slurry; (3) The mixed slurry was vacuum dried at 80°C for 12 hours and granulated through a 200-mesh sieve to obtain mixed powder; (4) The mixed powder is unidirectionally cold-pressed in a mold at a pressure of 250 MPa and held for 30 seconds to obtain a shaped blank; (5) The formed blank is placed in a vacuum sintering furnace and heated to 1450°C at a heating rate of 8°C / min. It is then held at 1450°C for 2 hours. During the holding period, nitrogen gas is introduced to control the nitrogen partial pressure to 1.5 kPa. Then, it is cooled to room temperature at a cooling rate of 4°C / min to obtain Ti(C,N)-based metal ceramic with a four-layer micro-nano gradient core-ring structure.

[0021] The product obtained in this embodiment was subjected to microstructural observation and mechanical property testing. The results showed that the hard phase particles had a clear four-layer ring phase structure, and the ring phases in each layer were distributed with a compositional gradient. The Ti(C,N)-based cermet obtained in this embodiment was tested to have a hardness of 93.8 HRA, a flexural strength of 1780 MPa, and a fracture toughness of 13.5 MPa·m.

[0022] Example 3 Raw material ratio (mass percentage): Ti(C,N) powder (particle size 0.8μm) 55%, WC powder (particle size 0.5μm) 12%, Mo2C powder (particle size 0.5μm) 8%, NbC powder (particle size 0.4μm) 5%, Ni powder (particle size 1.5μm) 20%.

[0023] Preparation method: (1) Weigh the above raw material powder according to the ratio and put it into the ball mill jar. Add anhydrous ethanol as the ball milling medium. The ball-to-material ratio is 6:1. (2) Classification ball milling: First, ball mill at a speed of 250 r / min for 5 hours, and then ball mill at a speed of 180 r / min for 12 hours to obtain a mixed slurry; (3) The mixed slurry was vacuum dried at 80°C for 12 hours and granulated through a 200-mesh sieve to obtain mixed powder; (4) The mixed powder is unidirectionally cold-pressed in a mold at a pressure of 180MPa and held for 30 seconds to obtain a shaped blank; (5) The formed blank is placed in a vacuum sintering furnace and heated to 1380°C at a heating rate of 12°C / min. It is held at 1380°C for 1 hour. During the holding period, nitrogen gas is introduced to control the nitrogen partial pressure to 0.8 kPa. Then, it is cooled to room temperature at a cooling rate of 6°C / min to obtain Ti(C,N)-based metal ceramics with a two-layer micro-nano gradient core-ring structure.

[0024] The product obtained in this embodiment was subjected to microstructural observation and mechanical property testing. The results showed that the hard phase particles had a clear two-layer ring-shaped phase structure. The Ti(C,N)-based cermet obtained in this embodiment was tested to have a hardness of 92.5 HRA, a flexural strength of 1920 MPa, and a fracture toughness of 11.5 MPa·m.

Claims

1. A titanium-based cermet having a multilayer micro-nano gradient structure, characterized in that, The titanium-based metal ceramic with a multilayer micro-nano gradient structure comprises a hard phase and a binder phase. The hard phase particles have two or more annular phases inside, and each annular phase has a compositional gradient distribution from the inside to the outside. The number of annular phase layers is 2 to 5. The annular phase is formed by solid dissolving one or more elements of Mo, W, Ta, and Nb in Ti(C,N). From the inside to the outside, the content of W and / or Mo elements in each annular phase layer shows a gradient increase or a gradient decrease, while the content of N element shows the opposite gradient change.

2. The titanium-based cermets with multi-layered micro-nano gradient structure according to claim 1, characterized in that, The particle size of the hard phase particles is 0.2~2.0μm.

3. A method for preparing a titanium-based cermet having a multilayer micro-nano gradient structure, characterized in that Includes the following steps: (1) Raw material preparation: Weigh Ti(C,N) powder, carbide additive phase powder and metal binder phase powder; the carbide additive phase powder is selected from one or more of Mo2C, WC, TaC and NbC; (2) Graded ball milling: The raw material powder from step (1) is subjected to graded ball milling. First, it is coarsely ground with the first ball milling parameters, and then finely ground with the second ball milling parameters to obtain a mixed slurry. (3) Drying and granulation: The mixed slurry from step (2) is vacuum dried, sieved and granulated to obtain mixed powder; (4) Press molding: The mixed powder from step (3) is pressed into a mold to obtain a shaped blank; (5) Gradient sintering: The formed blank from step (4) is subjected to gradient sintering under atmosphere protection. The gradient sintering includes a heating stage, a holding stage and a cooling stage. During the holding stage and / or cooling stage, the nitrogen partial pressure of the atmosphere is controlled to be 0.5~2.0 kPa, the holding temperature is 1350~1500℃, and the holding time is 0.5~3 hours. (6) After cooling, a Ti(C,N)-based metal ceramic with a multilayer micro-nano gradient core-ring structure is obtained. Further, the particle size of the Ti(C,N) powder in step (1) is 0.2~1.0μm, the particle size of the carbide additive phase powder is 0.1~0.8μm, and the particle size of the metal binder phase powder is 0.5~2.0μm.

4. The method for preparing titanium-based cermets with multilayer micro / nano gradient structures as described in claim 3, characterized in that: The graded ball milling in step (2) is as follows: first, ball mill at a speed of 200~400 r / min for 2~6 hours, and then ball mill at a speed of 100~200 r / min for 8~24 hours.

5. The method for preparing titanium-based cermets with multilayer micro / nano gradient structures as described in claim 3, characterized in that: The heating rate in step (5) is 5~15℃ / min, and the cooling rate in the cooling stage is 3~10℃ / min.

6. The method for preparing titanium-based cermets with multilayer micro / nano gradient structures as described in claim 3, characterized in that: The atmosphere described in step (5) is nitrogen, argon, or a mixture of nitrogen and argon.