Carbide suitable for CNC cutting tools and its preparation method
By using a combination of WC, CoCrFeNiAl high-entropy alloy and carbon nanotube-SiC composite powder, the problem of decreased toughness when increasing the hardness of cemented carbide was solved, and a cemented carbide with high hardness, high toughness and wear resistance suitable for CNC cutting tools was prepared to meet the requirements of high-speed cutting and interrupted cutting.
Patent Information
- Application Number
- CN202611614371.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cemented carbide materials exhibit a decrease in toughness when increasing hardness, or a decrease in hardness when increasing toughness, making it difficult to achieve both high hardness and high toughness in CNC cutting tools.
Hard alloys were prepared by ball milling and spark plasma sintering using WC powder, CoCrFeNiAl high-entropy alloy powder, carbon nanotube-SiC composite powder and VC powder as raw materials. CoCrFeNiAl high-entropy alloy was used as the binder phase to replace traditional Co, and carbon nanotube-SiC composite powder was used as the reinforcing phase to inhibit WC grain growth and improve toughness and wear resistance.
The prepared cemented carbide possesses high hardness, high toughness, and wear resistance, and can maintain excellent cutting performance and long service life under harsh cutting conditions, making it suitable for CNC cutting tools.
Smart Images

Figure CN123108385A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of cemented carbide technology, and in particular to a cemented carbide suitable for CNC cutting tools and its preparation method. Background Technology
[0002] CNC cutting tools, as key consumables in the automotive, aerospace, and energy equipment industries, must possess high hardness and good toughness. High hardness is fundamental for resisting wear and maintaining dimensional accuracy, while good toughness is crucial to preventing tool chipping failure under intermittent cutting and vibration conditions. Cemented carbide, a composite material composed of hard phases such as tungsten carbide (WC) and metallic binder phases such as cobalt, is widely used in CNC cutting tools due to its high hardness and wear resistance. However, there is an inherent contradiction between hardness and toughness—increasing hardness often sacrifices toughness, while increasing toughness leads to a decrease in hardness. To alleviate this contradiction, existing technologies attempt to add toughening and reinforcing phases to cemented carbide or develop novel binder phases.
[0003] In terms of reinforcing phases, silicon carbide possesses high hardness, high thermal stability, and good oxidation resistance, making it suitable as a reinforcing phase for cemented carbides to further improve the material's wear resistance and high-temperature performance. However, the significant difference in thermal expansion coefficients between silicon carbide and the WC-Co matrix easily leads to thermal stress during sintering and cooling. Furthermore, the addition of silicon carbide reduces the fracture toughness of cemented carbides, resulting in a decrease in the material's impact resistance.
[0004] Regarding the binder phase, although replacing the Co binder phase with intermetallic compounds such as Ni3Al is an attempt to improve high-temperature performance, its inherent brittleness and poor plastic deformation ability make it difficult to effectively absorb crack propagation energy, resulting in insufficient impact toughness of the tool. Summary of the Invention
[0005] The present invention was made in view of the above-mentioned problems, and its purpose is to provide a cemented carbide suitable for CNC cutting tools and a method for preparing the same, so as to maintain the high hardness of the cemented carbide while improving its toughness and wear resistance.
[0006] Specifically, the first aspect of the present invention provides a cemented carbide comprising the following raw materials by weight percentage: WC powder: 87%–89.7%, CoCrFeNiAl high-entropy alloy powder: 10%–12%, carbon nanotube-SiC composite powder: 0.1%–0.5%, and VC powder: 0.2%–0.5%; wherein the molar ratio of Co:Cr:Fe:Ni:Al in the CoCrFeNiAl high-entropy alloy powder is (2–2.5):1:1:(3–5.5):(0.1–0.25); the preparation method of the carbon nanotube-SiC composite powder is as follows: carbon nanotubes, ammonium persulfate, and a first solvent are mixed and dried, then mixed with silicon powder and a second solvent and dried, and then subjected to composite heat treatment under a protective atmosphere.
[0007] Optionally, the mass ratio of the carbon nanotubes to the ammonium persulfate is 1:20 to 50.
[0008] Optionally, the first solvent is water.
[0009] Optionally, the second solvent is ethanol.
[0010] Optionally, the molar ratio of the carbon nanotubes to the silicon powder is 2 to 4:1.
[0011] Optionally, the temperature of the composite heat treatment is 1200℃~1300℃.
[0012] Optionally, the heat treatment holding time is 2h to 4h.
[0013] The second aspect of the present invention provides a method for preparing the above-mentioned cemented carbide, comprising the following steps: S1: mixing carbon nanotube-SiC composite powder and a third solvent, and then adding WC powder, CoCrFeNiAl high-entropy alloy powder and VC powder; S2: ball milling under a protective atmosphere to obtain cemented carbide powder; S3: obtaining the cemented carbide powder by spark plasma sintering under a protective atmosphere.
[0014] Optionally, in step S1, the third solvent is an ethanol solution of polyvinylpyrrolidone.
[0015] Optionally, in step S2, the ball milling speed is 200 r / min to 300 r / min.
[0016] Optionally, in step S3, the temperature of the spark plasma sintering is 1230℃~1280℃.
[0017] Optionally, in step S3, the holding time for discharge plasma sintering is 3 min to 15 min.
[0018] Optionally, after step S3, the product after sintering is further subjected to vacuum heat treatment.
[0019] Optionally, the preparation method of the CoCrFeNiAl high-entropy alloy powder is as follows: cobalt salt, chromium salt, iron salt, nickel salt, aluminum salt and a first solvent are mixed to obtain a mixed metal salt solution; a complexing agent is added, and after heating and reaction, the solution is freeze-dried to obtain a dry gel; the dry gel is then subjected to alloying heat treatment in a hydrogen atmosphere to obtain the powder.
[0020] Optionally, the alloying heat treatment includes a first-stage alloying heat treatment and a second-stage alloying heat treatment; the temperature of the first-stage alloying heat treatment is 450℃~550℃, and the holding time is 1h~2h; the temperature of the second-stage alloying heat treatment is 900℃~1000℃, and the holding time is 2h~4h.
[0021] Optionally, the heating rate of the first stage alloying heat treatment is 3℃ / min to 5℃ / min.
[0022] Optionally, the heating rate of the second stage alloying heat treatment is 5℃ / min to 10℃ / min.
[0023] Optionally, the concentration of the mixed metal salt solution is 0.5 mol / L to 1.5 mol / L.
[0024] Optionally, the complexing agent is citric acid.
[0025] Optionally, the temperature of the heating reaction is 70°C to 90°C.
[0026] Optionally, the vacuum degree of the freeze-drying is 10 Pa to 50 Pa.
[0027] Optionally, the freeze-drying temperature is -50℃ to -60℃.
[0028] Optionally, the freeze-drying time is 24h to 72h.
[0029] Optionally, the molar ratio of the citric acid to the total metal ions in the mixed metal salt solution is 1.2 to 1.5:1.
[0030] A third aspect of the present invention provides an application of the aforementioned cemented carbide in CNC cutting tools.
[0031] Compared with the prior art, the present invention has the following beneficial effects: This invention employs ultrafine silicon carbide (WC) as the hard phase, combined with a VC grain inhibitor to suppress WC grain growth during sintering. By in-situ compositing carbon nanotubes with silicon carbide, and using carbon nanotube-SiC composite powder as the reinforcing phase, the high hardness of silicon carbide enhances the matrix's resistance to abrasive cutting, while the high specific strength and toughness of carbon nanotubes, together with the silicon carbide, synergistically strengthen and toughen the matrix. Furthermore, a high-entropy alloy (CoCrFeNiAl) is used as the binder phase to replace traditional Co. The solid solution strengthening effect of the high-entropy alloy makes its strength higher than pure Co. As a binder phase, it provides stronger support for the WC hard phase, resisting plastic deformation and abrasive cutting on the friction surface, thus improving toughness and wear resistance while maintaining hardness.
[0032] The cemented carbide provided by this invention has high hardness, high toughness and wear resistance, which can meet the stringent requirements of hardened steel, mold steel and other high-hardness materials under continuous and intermittent cutting conditions, and is suitable for the use of CNC cutting tools. Attached Figure Description
[0033] To more clearly illustrate the technical solutions in the embodiments of this drawing or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this drawing. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0034] Figure 1 This is a SEM image of the cemented carbide powder prepared in Example 1. Detailed Implementation
[0035] To make the objectives, technical solutions, and advantages of this application clearer, the following description and illustration are provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application. All other embodiments obtained by those skilled in the art based on the embodiments provided in this application without inventive effort are within the scope of protection of this application.
[0036] Obviously, the following description is merely some examples or embodiments of this application. Those skilled in the art can apply this application to other similar scenarios without any inventive effort. Furthermore, it is understood that although the effort involved in such development may be complex and lengthy, for those skilled in the art related to the content disclosed in this application, any changes to design, manufacturing, or production based on the technical content disclosed in this application are merely conventional technical means and should not be construed as insufficient disclosure of the content of this application.
[0037] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0038] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0039] On one hand, this application provides a cemented carbide comprising the following raw materials by weight percentage: WC powder: 87%–89.7%, CoCrFeNiAl high-entropy alloy powder: 10%–12%, carbon nanotube-SiC composite powder: 0.1%–0.5%, and VC powder: 0.2%–0.5%; the molar ratio of Co:Cr:Fe:Ni:Al in the CoCrFeNiAl high-entropy alloy powder is (2–2.5):1:1:(3–5.5):(0.1–0.25); the preparation method of the carbon nanotube-SiC composite powder is as follows: carbon nanotubes, ammonium persulfate and a first solvent are mixed and dried, then mixed with silicon powder and a second solvent and dried, and then subjected to composite heat treatment under a protective atmosphere.
[0040] WC powder: provides a hard phase framework, ensuring high hardness and wear resistance of cemented carbide.
[0041] CoCrFeNiAl high-entropy alloy: As a binder phase to replace traditional Co, when subjected to cutting impact, this binder phase can absorb a large amount of fracture energy through strong dislocation slip, effectively blunting the crack tip, thereby giving the tool excellent anti-chipping toughness; at the same time, its solid solution strengthening effect ensures the high hardness and compressive strength of the binder phase itself, which can provide stronger support for the WC hard phase, resist plastic deformation of the friction surface and abrasive cutting, thereby improving wear resistance.
[0042] Carbon nanotube-SiC composite powder: As a synergistic reinforcing and toughening phase, carbon nanotubes and silicon powder form SiC in situ. The carbon nanotubes act as a physical barrier, preventing direct contact between SiC and the matrix, avoiding the formation of harmful η phase, ensuring interfacial bonding strength, and consuming fracture energy through bridging, pull-out, and crack deflection mechanisms, achieving toughening without reducing hardness. Silicon carbide itself has high hardness, which can improve the matrix's resistance to abrasive cutting, while carbon nanotubes have high specific strength and toughness. The combination of the two has a synergistic reinforcing and toughening effect on the matrix.
[0043] VC: As a grain inhibitor, it helps to obtain a uniform grain size distribution by suppressing abnormal growth of WC grains during sintering.
[0044] By controlling the molar ratio of each component in the CoCrFeNiAl high-entropy alloy powder within the range of Co:Cr:Fe:Ni:Al (2–2.5):1:1:(3–5.5):(0.1–0.25), the alloy system tends to form a face-centered cubic solid solution structure, exhibiting both high plasticity and solid solution strengthening effects. The high Co content provides good wettability and adhesion, Ni and Fe enhance toughness and corrosion resistance, Cr improves oxidation resistance, and a small amount of Al promotes oxide formation and increases high-temperature hardness. The solid solution strengthening effect gives the high-entropy alloy binder phase high hardness and strength, providing stronger support for the WC hard phase (compared to pure Co), resisting plastic deformation and abrasive cutting on the friction surface.
[0045] In some embodiments of this application, the mass ratio of the carbon nanotubes to the ammonium persulfate is 1:20 to 50.
[0046] By controlling the mass ratio of carbon nanotubes to ammonium persulfate to 1:20-50, ammonium persulfate can carboxylate the surface of carbon nanotubes in the aqueous phase, introduce oxygen-containing functional groups, and enhance the polarity of the carbon nanotube surface.
[0047] In some embodiments of this application, the first solvent is water.
[0048] In some embodiments of this application, the second solvent is ethanol.
[0049] In some embodiments of this application, the molar ratio of carbon nanotubes to silicon powder is 2 to 4:1.
[0050] The molar ratio of carbon nanotubes to silicon powder is controlled at 2 to 4:1 to ensure that there is sufficient silicon source on the surface of carbon nanotubes, and that excess carbon nanotubes can retain the flexible bridge structure.
[0051] In some embodiments of this application, the temperature of the composite heat treatment is 1200℃~1300℃.
[0052] In some embodiments of this application, the heat treatment holding time is 2h to 4h.
[0053] By controlling the composite heat treatment temperature and holding time, silicon powder reacts with carbon nanotubes in situ to form SiC before melting, while avoiding excessive temperature that could damage the carbon nanotube structure. The carbon nanotubes act as a physical barrier to effectively prevent SiC from reacting directly with the matrix, thereby avoiding the formation of brittle η phase, ensuring interfacial bonding strength, and maintaining the toughening effect.
[0054] On the other hand, this application provides a method for preparing cemented carbide, comprising the following steps: S1: mixing carbon nanotube-SiC composite powder and a third solvent, and then adding WC powder, CoCrFeNiAl high-entropy alloy powder, and VC powder; S2: ball milling under a protective atmosphere to obtain cemented carbide powder; S3: subjecting the cemented carbide powder to spark plasma sintering under a protective atmosphere.
[0055] Ball milling thoroughly mixes the raw materials, providing a foundation for the uniformity of the microstructure after sintering. Spark plasma sintering utilizes Joule heating and plasma effects generated by pulsed current to achieve densification at lower temperatures and in a shorter time, significantly suppressing WC grain growth and avoiding grain coarsening caused by prolonged holding in traditional hot pressing sintering. Simultaneously, the rapid heating of spark plasma sintering helps preserve the metastable structure of the high-entropy alloy and the integrity of the carbon nanotube-SiC composite toughening phase.
[0056] In some embodiments of this application, in step S1, the third solvent is an ethanol solution of polyvinylpyrrolidone.
[0057] In some embodiments of this application, in step S2, the ball milling speed is 200 r / min to 300 r / min.
[0058] By controlling the ball mill speed between 200 r / min and 300 r / min, the powder can be fully mixed while avoiding damage to the carbon nanotube structure caused by excessively high speed.
[0059] In some embodiments of this application, in step S3, the temperature of the spark plasma sintering is 1230℃~1280℃.
[0060] In some embodiments of this application, the holding time for discharge plasma sintering in step S3 is 3 min to 15 min.
[0061] Controlling the temperature of spark plasma sintering (SPS) to 1230℃–1280℃ and the time to 3 min–15 min can promote the full melting and spreading of the high-entropy alloy binder phase and improve densification while inhibiting abnormal growth of WC grains. If the temperature is too low (or the time too short), the high-entropy alloy binder phase will not have fully melted or will lack sufficient fluidity, failing to effectively wet the WC powder and carbon nanotube-SiC composite powder. If the temperature is too high (or the time too long), the liquid-phase sintering process will intensify, and the WC grains may grow abnormally, leading to a decrease in hardness.
[0062] In some embodiments of this application, after step S3, the product after sintering is further subjected to vacuum heat treatment.
[0063] Vacuum heat treatment after sintering can release the thermal stress generated during sintering and improve the uniformity of the alloy's microstructure.
[0064] In some embodiments of this application, the preparation method of the CoCrFeNiAl high-entropy alloy powder is as follows: cobalt salt, chromium salt, iron salt, nickel salt, aluminum salt and a first solvent are mixed to obtain a mixed metal salt solution; a complexing agent is added, and after heating and reaction, the solution is freeze-dried to obtain a dry gel; the dry gel is then subjected to alloying heat treatment in a hydrogen atmosphere to obtain the powder.
[0065] High-entropy alloy powder was prepared using a sol-gel method combined with hydrogen reduction. A complexing agent (citric acid) was used to uniformly mix the metal ions at the molecular level, followed by freeze-drying to obtain a fluffy, porous precursor dry gel, avoiding the problem of uneven element distribution in conventional mechanical alloying methods. Alloying heat treatment in a hydrogen atmosphere reduced the metal oxides to an alloyed state, obtaining alloyed high-entropy alloy powder, which is beneficial for good bonding with WC during subsequent sintering.
[0066] In some embodiments of this application, the alloying heat treatment includes a first-stage alloying heat treatment and a second-stage alloying heat treatment; the temperature of the first-stage alloying heat treatment is 450℃~550℃, and the holding time is 1h~2h; in some embodiments of this application, the temperature of the second-stage alloying heat treatment is 900℃~1000℃, and the holding time is 2h~4h.
[0067] In some embodiments of this application, the heating rate of the first stage alloying heat treatment is 3°C / min to 5°C / min.
[0068] The first stage of alloying heat treatment decomposes the citric acid and nitrates in the dry gel, generating a mixture of metal oxides. The temperature is increased slowly to avoid the decomposition reaction being too violent and causing powder to splatter.
[0069] In some embodiments of this application, the heating rate of the second-stage alloying heat treatment is 5°C / min to 10°C / min.
[0070] The second-stage alloying heat treatment reduces the metal oxide to an alloy state in a hydrogen-containing atmosphere. The higher heating rate shortens the high-temperature period and inhibits excessive grain growth.
[0071] In some embodiments of this application, the concentration of the mixed metal salt solution is 0.5 mol / L to 1.5 mol / L.
[0072] Controlling the concentration of the mixed metal salt solution ensures a uniform distribution of metal ions during the sol-gel process.
[0073] In some embodiments of this application, the complexing agent is citric acid.
[0074] In some embodiments of this application, the temperature of the heating reaction is 70°C to 90°C.
[0075] In some embodiments of this application, the vacuum degree of the freeze-drying is 10 Pa to 50 Pa.
[0076] In some embodiments of this application, the freeze-drying temperature is -50°C to -60°C.
[0077] In some embodiments of this application, the freeze-drying time is 24h to 72h.
[0078] By controlling the freeze-drying process under low temperature and low vacuum conditions, the collapse of the gel skeleton caused by rapid solvent evaporation during conventional drying is avoided, resulting in a fluffy and porous dry gel precursor. This facilitates gas diffusion during subsequent hydrogen reduction, leading to the production of high-entropy alloy powder with fine particle size and uniform distribution.
[0079] In some embodiments of this application, the molar ratio of the citric acid to the total metal ions in the mixed metal salt solution is 1.2 to 1.5:1.
[0080] Controlling the amount of citric acid ensures that all metal ions are fully complexed, preventing uneven precipitation of free metal ions in subsequent processing and promoting thorough mixing of metal ions at the molecular level.
[0081] A third aspect of this application provides an application of cemented carbide in CNC cutting tools.
[0082] The cemented carbide of this application combines high hardness, high toughness, and high wear resistance, exhibiting excellent comprehensive mechanical properties. It is suitable for the manufacture of CNC cutting tools and can maintain excellent cutting performance and long service life under harsh working conditions such as high-speed cutting, heavy cutting, and intermittent cutting.
[0083] Example The following embodiments describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on weight, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0084] In the embodiments and comparative examples of the present invention: The average particle size of the WC powder used was 0.4 μm; The carbon nanotubes used are multi-walled carbon nanotubes with a diameter of 10 nm to 15 nm and a length of 10 μm to 15 μm. The average particle size of the silicon powder and VC powder used is 1 μm; The polyvinylpyrrolidone used has a K value of 27-30 and an average molecular weight of approximately 58,000 g / mol.
[0085] Example 1 The cemented carbide provided in this embodiment includes the following raw materials by weight percentage: WC powder: 88.4%, CoCrFeNiAl high-entropy alloy powder: 11%, carbon nanotube-SiC composite powder: 0.3%, and VC powder: 0.3%.
[0086] The preparation method of CoCrFeNiAl high-entropy alloy powder provided in this embodiment is as follows: Cobalt nitrate, chromium nitrate, ferric nitrate, nickel nitrate, aluminum nitrate, and water were mixed to obtain a mixed metal salt solution. Citric acid was added, and the mixture was stirred at 80°C to obtain a wet gel. Liquid nitrogen was added to the wet gel, and the mixture was freeze-dried at -55°C under a vacuum of 40 Pa for 40 hours to obtain a dry gel. The dry gel was then heat-treated in a mixed atmosphere of hydrogen and argon (H2:Ar=1:4). The first stage of heat treatment involved heating to 500°C at a rate of 4°C / min and holding for 1.5 hours. The second stage of heat treatment involved heating to 950°C at a rate of 8°C / min and holding for 3 hours, followed by furnace cooling to 25°C.
[0087] The total concentration of metal ions in the mixed metal salt solution is 1 mol / L. The molar ratio of Co:Cr:Fe:Ni:Al in the mixed metal salt solution is 2.2:1:1:4.5:0.15; The molar ratio of total metal ions in citric acid and mixed metal salt solutions is 1.4:1.
[0088] The preparation method of carbon nanotube-SiC composite powder provided in this embodiment is as follows: Carbon nanotubes and water were mixed and sonicated for 15 minutes. Ammonium persulfate was added and sonicated for 25 minutes. After being filtered, washed, and dried, the mixture was then mixed with silicon powder and anhydrous ethanol. After vacuum drying at 60°C, the mixture was heated to 1260°C at a rate of 8°C / min under argon protection and held for 3 hours. The mixture was then cooled to 25°C in the furnace.
[0089] The mass ratio of carbon nanotubes to ammonium persulfate is 1:40. The mass ratio of carbon nanotubes to silicon powder is 2:1.
[0090] The method for preparing cemented carbide provided in this embodiment includes the following steps: S1: Carbon nanotube-SiC composite powder and polyvinylpyrrolidone ethanol solution were mixed and ultrasonically dispersed for 50 min. The mass-to-volume ratio of polyvinylpyrrolidone to anhydrous ethanol in the polyvinylpyrrolidone ethanol solution was 0.12 g: 10 mL. WC powder, CoCrFeNiAl high-entropy alloy powder, and VC powder were then added. The mixture was ball-milled under argon protection with anhydrous ethanol as the ball milling medium and a ball-to-material ratio of 10:1. The mixture was ball-milled at 250 r / min for 26 h. The resulting ball-milled slurry was vacuum-dried at 60 °C, crushed, and passed through a 400-mesh sieve to obtain cemented carbide powder.
[0091] Figure 1 This is a SEM image of the cemented carbide powder prepared in Example 1. The image shows that the cemented carbide powder exhibits an irregular polygonal structure, with the binder and reinforcing phase components well dispersed and attached to the surface of the WC hard phase particles.
[0092] S2: The cemented carbide powder was subjected to spark plasma sintering under argon protection. The parameters were: heating rate of 100℃ / min, sintering temperature of 1250℃, sintering pressure of 35MPa, holding temperature for 4min, and furnace cooling to 25℃. Then, it underwent heat treatment with the following parameters: vacuum degree of 10Pa, heating rate of 5℃ / min to 600℃, holding temperature for 2h, and furnace cooling to 25℃.
[0093] Example 2 The difference between the cemented carbide provided in this embodiment and that in Embodiment 1 is as follows: The raw materials include the following weight percentages: WC powder: 89.6%, CoCrFeNiAl high-entropy alloy powder: 10%, carbon nanotube-SiC composite powder: 0.1%, and VC powder: 0.3%.
[0094] The preparation method was carried out in accordance with Example 1.
[0095] Example 3 The difference between the cemented carbide provided in this embodiment and that in Embodiment 1 is as follows: The raw materials include the following weight percentages: WC powder: 87.2%, CoCrFeNiAl high-entropy alloy powder: 12%, carbon nanotube-SiC composite powder: 0.5%, and VC powder: 0.3%.
[0096] The preparation method was carried out in accordance with Example 1.
[0097] Example 4 The difference between the cemented carbide provided in this embodiment and that in Embodiment 1 is as follows: In the preparation method of CoCrFeNiAl high-entropy alloy powder, the molar ratio of Co:Cr:Fe:Ni:Al in the mixed metal salt solution is 2:1:1:3:0.1.
[0098] The preparation method was carried out in accordance with Example 1.
[0099] Example 5 The difference between the cemented carbide provided in this embodiment and that in Embodiment 1 is as follows: In the preparation method of CoCrFeNiAl high-entropy alloy powder, the molar ratio of Co:Cr:Fe:Ni:Al in the mixed metal salt solution is 2.5:1:1:5.5:0.25.
[0100] The preparation method was carried out in accordance with Example 1.
[0101] Comparative Example 1 The cemented carbide provided in this comparative example differs from that in Example 1 in that: The raw materials include the following weight percentages: WC powder: 88.4%, CoCrFeNiAl high-entropy alloy powder: 11%, SiC: 0.3%, and VC powder: 0.3%.
[0102] The preparation method was carried out in accordance with Example 1.
[0103] Comparative Example 2 The cemented carbide provided in this comparative example differs from that in Example 1 in that: The raw materials include the following weight percentages: WC powder: 88.4%, CoCrFeNiAl high-entropy alloy powder: 11%, carbon nanotubes: 0.2%, SiC: 0.1%, and VC powder: 0.3%.
[0104] The preparation method was carried out in accordance with Example 1.
[0105] Comparative Example 3 The cemented carbide provided in this comparative example differs from that in Example 1 in that: The raw materials include the following weight percentages: WC powder: 88.4%, Co powder: 11%, carbon nanotube-SiC composite powder: 0.3%, and VC powder: 0.3%.
[0106] The preparation method was carried out in accordance with Example 1.
[0107] The performance of the cemented carbides prepared in Examples 1-5 and Comparative Examples 1-3 was tested: (1) Hardness test: Vickers hardness test was performed in accordance with GB / T 4340.1-2024 "Metallic materials Vickers hardness test - Part 1: Test method" with a test force of 30 kgf and a holding time of 15 s.
[0108] (2) Fracture toughness test: The fracture toughness test was carried out in accordance with JB / T 12616-2016 "Method for testing fracture toughness of matrix material of cemented carbide cutting tool".
[0109] (3) Transverse fracture strength test: The bending strength was tested in accordance with GB / T 3851-2015 "Method for Determination of Transverse Fracture Strength of Hard Alloy". The three-point bending method was adopted, the sample size was 5mm×5mm×35mm, the span was 30mm, and the loading rate was 2mm / min.
[0110] (4) Volume loss test: The wear amount test was carried out in accordance with GB / T 34501-2017 "Test Method for Wear Resistance of Hard Alloy". The sample area was 50mm×20mm, 30-mesh alumina abrasive was used, the load was 130N, the rotation speed was 1m / s, the abrasive flow rate through the contact surface was 150g / min, and the test time was 20min.
[0111] The test results are shown in Table 1.
[0112] Table 1. Performance test results of cemented carbides prepared in Examples 1-5 and Comparative Examples 1-3
[0113] According to Table 1, the Vickers hardness of the cemented carbide provided in this application is 1945 HV. 30 ~2120HV 30 The fracture toughness is 11.0 MN / m. 3 / 2 ~14.1MN / m 3 / 2 The transverse tensile strength is 3656 MPa to 4207 MPa, and the volume loss is 7.9 mm. 3 ~12.7mm 3 .
[0114] Compared to Example 1, Comparative Example 1 exhibits significantly lower fracture toughness, transverse fracture strength, and wear resistance. This may be because SiC, being in direct contact with the matrix, is prone to interfacial reactions that generate brittle phases, and the mismatch in thermal expansion coefficients leads to interfacial stress concentration, weakening the bond strength. During wear, SiC easily detaches, becoming a source of abrasive particles and exacerbating wear. In Example 1, carbon nanotubes act as a physical barrier, preventing direct contact between SiC and the matrix, and enhance toughness and strength through bridging, pull-out, and crack deflection mechanisms.
[0115] Compared with Example 1 and Comparative Example 1, Comparative Example 2 exhibits better fracture toughness, transverse fracture strength, and wear resistance than Comparative Example 1, but is still significantly lower than Example 1. This may be because carbon nanotubes and SiC are independently dispersed, lacking structural coupling. Carbon nanotubes tend to agglomerate, becoming defect sources, while SiC still partially undergoes interfacial reactions. The two cannot form a synergistic toughening effect, and during wear, agglomerates and weak interfacial areas preferentially peel off, transforming into abrasive particles. In Example 1, carbon nanotubes and SiC are in-situ composited, resulting in a unified structure and uniform dispersion, achieving a synergistic effect of bridging toughening and dispersion strengthening.
[0116] Compared to Example 1, Comparative Example 3 exhibits lower hardness, fracture toughness, transverse fracture strength, and wear resistance. This is because the pure Co binder phase has lower intrinsic hardness and strength, limited work hardening ability, and cannot effectively passivate crack tips, resulting in insufficient holding force for WC particles. During wear, the binder phase is prone to plastic deformation and adhesion, while the hard phase particles lack support and detach, exacerbating wear. In Example 1, the CoCrFeNiAl high-entropy alloy binder phase, through lattice distortion solid solution strengthening and slow diffusion effects, improves its own hardness, interface stability, and deformation resistance, ensuring that the hard phase is not easily detached, thus simultaneously improving overall performance.
[0117] The cemented carbide provided by this invention combines high hardness, high toughness, and wear resistance, which can meet the stringent requirements of high-hardness materials such as hardened steel and die steel under continuous and intermittent cutting conditions, providing a material basis for improving tool life and machining reliability.
[0118] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A cemented carbide, characterized in that, The raw materials include the following weight percentages: WC powder: 87%–89.7%, CoCrFeNiAl high-entropy alloy powder: 10%–12%, carbon nanotube-SiC composite powder: 0.1%–0.5%, and VC powder: 0.2%–0.5%. The molar ratio of Co:Cr:Fe:Ni:Al in the CoCrFeNiAl high-entropy alloy powder is (2~2.5):1:1:(3~5.5):(0.1~0.25). The preparation method of the carbon nanotube-SiC composite powder is as follows: The mixture of carbon nanotubes, ammonium persulfate, and a first solvent is dried, then mixed with silicon powder and a second solvent and dried. The mixture is then subjected to composite heat treatment under a protective atmosphere to obtain the final product.
2. The cemented carbide according to claim 1, characterized in that, The mass ratio of the carbon nanotubes to the ammonium persulfate is 1:20-50; And / or, the first solvent is water; And / or, the second solvent is ethanol; And / or, the molar ratio of the carbon nanotubes to the silicon powder is 2 to 4:1; And / or, the temperature of the composite heat treatment is 1200℃~1300℃; And / or, the heat treatment holding time for the composite heat treatment is 2h to 4h.
3. A method for preparing a cemented carbide as described in claim 1 or 2, characterized in that, Includes the following steps: S1: After mixing carbon nanotube-SiC composite powder and a third solvent, add WC powder, CoCrFeNiAl high-entropy alloy powder, and VC powder; S2: Ball milling is performed under a protective atmosphere to obtain cemented carbide powder; S3: Prepared by spark plasma sintering of cemented carbide powder under a protective atmosphere.
4. The method for preparing cemented carbide according to claim 3, characterized in that, In step S1, the third solvent is an ethanol solution of polyvinylpyrrolidone. And / or, in step S2, the ball milling speed is 200 r / min to 300 r / min; And / or, in step S3, the temperature of the discharge plasma sintering is 1230℃~1280℃; And / or, in step S3, the holding time for discharge plasma sintering is 3 min to 15 min; And / or, after step S3, the product after sintering is further subjected to vacuum heat treatment.
5. The method for preparing cemented carbide according to claim 3, characterized in that, The preparation method of the CoCrFeNiAl high-entropy alloy powder is as follows: Cobalt salt, chromium salt, iron salt, nickel salt, aluminum salt and a first solvent are mixed to obtain a mixed metal salt solution; a complexing agent is added, the mixture is heated to react and then freeze-dried to obtain a dry gel; The dry gel was prepared by alloying heat treatment in a hydrogen-containing atmosphere.
6. The method for preparing cemented carbide according to claim 5, characterized in that, The alloying heat treatment includes a first-stage alloying heat treatment and a second-stage alloying heat treatment; the temperature of the first-stage alloying heat treatment is 450℃~550℃, and the holding time is 1h~2h; the temperature of the second-stage alloying heat treatment is 900℃~1000℃, and the holding time is 2h~4h.
7. The method for preparing cemented carbide according to claim 6, characterized in that, The heating rate of the first stage alloying heat treatment is 3℃ / min to 5℃ / min; And / or, the heating rate of the second stage alloying heat treatment is 5℃ / min to 10℃ / min.
8. The method for preparing cemented carbide according to claim 5, characterized in that, The complexing agent is citric acid; And / or, the concentration of the mixed metal salt solution is 0.5 mol / L to 1.5 mol / L; And / or, the temperature of the heating reaction is 70°C to 90°C; And / or, the vacuum degree of the freeze-drying is 10 Pa to 50 Pa; And / or, the freeze-drying temperature is -50℃ to -60℃; And / or, the freeze-drying time is 24h to 72h.
9. The method for preparing cemented carbide according to claim 8, characterized in that, The molar ratio of the citric acid to the total metal ions in the mixed metal salt solution is 1.2 to 1.5:
1.
10. An application of cemented carbide as described in claim 1 or 2 in CNC cutting tools.