A method for smelting high-alloy steel with low burn-off

By segmented atmosphere control and electrical parameter optimization, low burn-loss smelting of high alloy steel is achieved, solving the problems of high alloy burn-loss and inaccurate impurity control in alloy steel smelting, and realizing stable production with high quality and low cost.

CN123108399APending Publication Date: 2026-11-17武汉重工铸锻有限责任公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202611540510.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high-alloy steel smelting processes suffer from high alloy burn-off, low carbon and phosphorus control precision, and unstable operating conditions, making it impossible to achieve stable mass production with high quality and low cost.

Method used

The method employs segmented atmosphere control, dual-stage electrical system, time-sequential slag stabilization, and constant-rate precise impurity removal, including induction melting, oxygen-free heating, intermittent carbon powder blowing to create foamed slag, and low-pressure constant-rate oxygen blowing, to form a closed foamed slag layer and a weak oxidation mode on the slag surface, thereby achieving the unity of alloy protection and impurity removal.

Benefits of technology

It significantly reduces the loss of alloying elements by burning, improves the recovery rate, and stably controls carbon and phosphorus impurities at extremely low levels, enabling high-quality and low-cost production of high-alloy steel, and improving metallurgical efficiency and product consistency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a low-burn-loss smelting method for high-alloy steel, belonging to the field of special alloy steel metallurgical smelting technology. Addressing the problems of high alloy element burn-off, low carbon and phosphorus removal precision, coarse process parameters, and poor batch stability in existing dual-process smelting methods using induction furnaces and electric arc furnaces, this invention proposes a process involving segmented atmosphere control, dual-stage electrical control, time-sequential foamed slag, constant-rate controllable oxidation for decarburization and dephosphorization, and multi-element quantitative recovery rate control. The process includes: induction furnace pre-melting and return of material; pre-deoxidation and slag control; electric arc furnace slag retention and steel mixing; oxygen-free operation and pure electric heating up to 1560℃; fixed-sequential pulse carbon injection to create foamed slag; high-temperature, low-pressure, constant-rate, precise blowing for decarburization and dephosphorization; endpoint deoxidation and alloying; and multi-element graded quantitative recovery rate control. This invention overcomes the technical problems of excessive impurities due to alloy preservation and severe alloy burn-off due to thorough impurity removal, achieving a chromium recovery rate of ≥95% and deep carbon and phosphorus removal, suitable for large-scale stable production of high-end alloy steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of alloy steel metallurgical smelting technology, and more specifically, to a smelting method for high alloy steel with low burn-off. Background Technology

[0002] High-chromium, niobium, boron, and manganese alloy steels are widely used in high-end equipment, power rotors, pressure vessels, molds, and high-strength structural components. These steels have high alloy value and are extremely sensitive to impurities, requiring stringent control over carbon and phosphorus content and alloy recovery rates.

[0003] In the prior art, the dual-smelting process combining induction furnace pre-melting and electric arc furnace refining for processing high-alloy steel return materials is a known method. For example, Chinese patent document CN108823348B discloses various dual-smelting routes using induction furnaces and electric arc furnaces. Chinese patent document CN104178596A discloses a process for smelting stainless steel using an electric arc furnace return oxygen blowing method, which employs a high-temperature, high-pressure (oxygen supply pressure up to 8MPa) dual-pipe continuous oxygen blowing method for decarburization and alloy preservation within the electric arc furnace. CN121109689A discloses an electric arc furnace smelting method that uses a furnace wall oxygen lance for weak oxygen supply in the later stages of smelting, combined with carbon powder injection, to control the decarburization rate. CN102634634A discloses the use of an electric arc furnace to produce high-alloy steel for boiler tubes. A method for producing low-phosphorus steel involves dephosphorizing by slag formation with lime and iron oxide; CN111809017A discloses a method for improving Cr yield in electric arc furnaces, which involves retaining steel and slag and adding lime to treat scrap steel alloy materials; CN1233851C discloses a method for controlling foamed slag in electric arc furnaces for steelmaking, which involves closed-loop dynamic control of foamed slag by adjusting the amount of oxygen blown and carbon powder injected; CN104131134A discloses a general process for producing foamed slag in the molten pool of an electric arc furnace, which requires the coordination of oxygen blowing.

[0004] However, the existing technologies still have the following drawbacks: The existing processes lack strict oxygen-free control during the heating stage; in the low-temperature stage (below 1560℃), easily oxidized elements such as Cr, Mn, B, and Nb have a strong affinity for oxygen and are preferentially oxidized, resulting in high alloy burn-off rates and high production costs. For example, the return oxygen blowing method in CN104178596A involves oxygen blowing during the heating stage, highlighting the alloy burn-off problem in the low-temperature section. The existing electric arc furnace smelting electrical parameters are crude (voltage 340V or 319V; current 16000A~22000A), lacking segmented fixed voltage and current systems, leading to uneven heating, unstable arcs, and large fluctuations in furnace conditions. Existing foam slag forming methods often require oxygen blowing (such as CN104131134A) and lack standardized timing control (carbon powder spraying at the furnace door). (≥1 minute), foam slag has poor stability and limited shielding oxidation effect. Although CN1233851C discloses a foam slag control method, it adopts a closed-loop dynamic adjustment method, which requires real-time monitoring and adjustment of oxygen blowing volume, making control complex and unable to be used under full oxygen-free conditions. Existing blowing processes are mostly extensive strong oxidation blowing, which cannot achieve uniform and controllable decarburization and dephosphorization, and are very likely to cause steel over-oxidation and aggravated alloy loss. Although CN121109689A proposes to control the decarburization rate with weak oxygen supply in the later stage, its blowing system is still substantially different from the low-pressure constant-rate selective oxidation system of this invention. Existing technologies only qualitatively describe improving the recovery rate (such as CN111809017B), without quantitative grading control standards, resulting in poor process reproducibility and insufficient batch consistency of products.

[0005] In view of this, the present invention is proposed. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing duplex smelting processes, such as coarse parameters, high alloy burn-off, low carbon and phosphorus control precision, and unstable operating conditions. It provides a high-alloy steel low-burn-off precision smelting method with segmented atmosphere control, dual-stage electrical system, time-sequential slag stabilization, constant-rate precise impurity removal, and multi-element quantitative control of recovery rate, so as to achieve high-quality, low-cost, and stable mass production of high-end alloy steel.

[0007] This invention is implemented as follows: In a first aspect, the present invention provides a method for smelting high-alloy steel with low burn-off, comprising the following steps: (1) An induction melting furnace is used to melt scrap recycled raw materials containing chromium, niobium, boron and manganese alloy steel; (2) After the molten steel is completely melted, fluorite ore is added, and the temperature is raised and samples are taken to confirm that the alloy element composition is stable; the temperature is raised further, silicon carbide is added for pre-deoxidation, and the slag is removed after tapping the steel. (3) Empty the residual molten steel inside the electric arc furnace, retain the oxidized slag from the furnace, add lime to make slag, and pour the pre-melted molten steel into the electric arc furnace; (4) After the steel is poured, the entire process is carried out using oxygen-free pure electric energy to raise the temperature until the temperature of the molten steel is stable at ≥1560℃; (5) Use carbon powder intermittent blowing to make foam slag; the blowing system is: blow for 40-50 seconds at a time, and then let it stand at intervals for a cycle of blowing, and do not blow oxygen throughout the process; (6) After the foamy slag forms and stably covers the molten steel surface, the temperature is raised to 1620℃~1680℃; single-pipe oxygen blowing is adopted, and the oxygen supply pressure is kept constant at 0.4~0.6MPa, and smelting is carried out in the weak oxidation mode of slag surface; the decarburization rate is controlled at 0.005~0.015% / minute. (7) After smelting, stop oxygen blowing, adjust the slag reducing properties, add trace amounts of alloy to fine-tune the steel composition, and control the tapping temperature to ≥1630℃.

[0008] In an optional implementation, in step (2), fluorite ore is added at 1.5 to 2.5 kg / t of molten steel, and the temperature is raised to 1600 to 1620°C to take samples to confirm that the alloy element composition is stable; the temperature is further raised to 1670 to 1680°C, and silicon carbide is added at 0.3 to 0.5 kg / t for pre-deoxidation.

[0009] In an optional implementation, in step (3), lime is added at a rate of 10-15 kg / t of molten steel to form slag.

[0010] In an optional implementation, in step (4), the heating is performed using an electrical system with a voltage of 319V, a current of 22000A, and a smelting power of 5-6MW.

[0011] In an optional implementation, in step (5), after each spraying, the mixture is left to stand for 1 minute, and the spraying is repeated 3 times in a continuous cycle; the spraying flow rate of the carbon powder is 10 kg / min; the carbon powder is coke powder with a C content ≥ 90%.

[0012] In an optional implementation, in step (6), the smelting electrical parameters are a voltage of 300V and a current of 19000A; the carbon content of the molten steel is smelted to less than 0.04% and the phosphorus content is smelted to less than 0.003%.

[0013] In an optional implementation, in step (6), the decarbonization rate is controlled to be 0.01% / minute.

[0014] In an optional implementation, in step (7), oxygen blowing is stopped when the degree of smelting oxidation reaches 1 / 2 of the theoretical total oxidation.

[0015] In an optional implementation, in step (6), the temperature is raised to 1620℃~1630℃, and the oxygen supply pressure is kept constant at 0.4~0.5MPa.

[0016] In an optional implementation, the alloy recovery rate is controlled as follows throughout the smelting process: chromium recovery rate ≥95%, niobium recovery rate 60%~70%, boron recovery rate 20%~30%, manganese recovery rate 40%~50%, and recovery rate of other alloying elements ≥98%.

[0017] The present invention has the following beneficial effects: This invention achieves a balance between high alloy recovery and ultra-low carbon and phosphorus impurities through a three-stage atmosphere synergistic control system: "oxygen-free heating—time-sequential slag stabilization—low-pressure constant-speed blowing." Compared with traditional processes, the loss of alloying elements (Cr, Nb, B, Mn, etc.) is significantly reduced, and the recovery rate is greatly improved. Simultaneously, the decarburization rate is stable and controllable (0.005%–0.015% / minute), dephosphorization is thorough, and carbon and phosphorus impurities can be stably controlled at extremely low levels. This fundamentally solves the contradiction in traditional processes where "preserving the alloy results in excessive impurities, while thorough impurity removal leads to severe alloy loss," achieving a comprehensive effect of high metallurgical efficiency, superior product quality, and low production costs. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0019] This invention provides a method for smelting high-alloy steel with low burn-off, comprising the following steps: (1) An induction melting furnace is used to melt scrap recycled raw materials containing chromium, niobium, boron and manganese alloy steel; (2) After the molten steel is completely melted, fluorite ore is added, and the temperature is raised and samples are taken to confirm that the alloy element composition is stable; the temperature is raised further, silicon carbide is added for pre-deoxidation, and the slag is removed after tapping the steel. (3) Empty the residual molten steel inside the electric arc furnace, retain the oxidized slag from the furnace, add lime to make slag, and pour the pre-melted molten steel into the electric arc furnace; (4) After the steel is poured, the entire process is carried out using oxygen-free pure electric energy to raise the temperature until the temperature of the molten steel is stable at ≥1560℃; (5) Use carbon powder intermittent blowing to make foam slag; the blowing system is: blow for 40-50 seconds at a time, and let stand at intervals for cyclic blowing, and do not blow oxygen throughout the process; (6) After the foamy slag forms and stably covers the molten steel surface, the temperature is raised to 1620℃~1680℃; single-pipe oxygen blowing is adopted, and the oxygen supply pressure is kept constant at 0.4~0.6MPa, and smelting is carried out in the weak oxidation mode of slag surface; the decarburization rate is controlled at 0.005%~0.015% / minute. (7) After smelting, stop oxygen blowing, adjust the slag reducing properties, add alloys to adjust the steel composition, and control the tapping temperature to ≥1630℃.

[0020] In the above technical solution of the present invention, each step cooperates with each other and is linked together to form a complete low-burn-loss, high-purity smelting process chain: Steps (1) and (2) transform high alloy return material into low-oxygen, stable pre-melted steel through induction furnace pre-melting and pre-deoxidation treatment, laying the basis for composition and oxygen potential for subsequent smelting; Step (3) uses slag retention and steel mixing to construct an alkaline oxidation slag system, creating slag phase conditions for dephosphorization; Step (4) uses oxygen-free and pure electric heating below 1560℃ throughout the process, cutting off the oxidation path of easily oxidized elements such as chromium, niobium, boron, and manganese in the low-temperature stage from the source, which is the first barrier to protect the alloy; Step (5) (6) Pulsed sequential carbon injection forms a closed foam slag layer under non-oxygen blowing conditions, shielding the air and stabilizing the electric arc, thus achieving slag stabilization and alloy protection. This is the second barrier to protect the alloy. In step (6), the alloy is blown in a low-pressure, constant-speed weak oxidation mode in the high-temperature zone of 1620℃~1680℃. The selective removal of carbon and phosphorus and the inhibition of alloy element oxidation are achieved by utilizing the thermodynamic principle of high-temperature carbon removal and chromium preservation. Alloy preservation and impurity removal are achieved in the same smelting stage. In step (7), the endpoint is controlled by reducing slag adjustment and alloy addition. The multi-element graded quantitative recovery rate is used as the whole process assessment indicator to ensure the replicability and batch consistency of the process.

[0021] Through the aforementioned segmented atmosphere control and parameter coupling, this invention achieves a three-stage synergy of oxygen-free heating to protect the alloy, sequential slag stabilization to protect the working condition, and low-pressure constant-rate oxidation to remove impurities, resulting in the following comprehensive technical effects: Firstly, in terms of alloy protection, the full-process oxygen-free heating and sealed foam slag layer prevent easily oxidized elements such as chromium, niobium, boron, and manganese from excessive oxidation throughout the smelting process. The chromium recovery rate is stably maintained at over 95%, while the recovery rates of niobium, boron, and manganese are controlled at 60%–70%, 20%–30%, and 40%–50%, respectively, and the recovery rate of other alloying elements is not less than 98%. Firstly, the consumption of precious alloys is significantly reduced. Secondly, in terms of impurity removal, high-temperature and low-pressure constant-speed blowing removes the carbon and phosphorus content of molten steel to below the lower limit of the target steel product standard, while avoiding over-oxidation of molten steel. The purity of the product meets the stringent requirements of high-end alloy steels such as P91 and P92. Thirdly, in terms of process stability, the parameters of each step are fixed, the timing is standardized, and the assessability is strong. The process is replicable, and the consistency of batch steel composition is significantly improved. This overcomes the industry's technical bias that traditional dual-process alloy preservation results in excessive carbon and phosphorus content, while thorough impurity removal results in severe alloy burn-off.

[0022] In an optional embodiment, in step (1), the induction furnace lining is made of refractory material with an alumina content of 86% to 88% and a magnesium oxide content of 8% to 10%, and the refractoriness is not less than 1800℃.

[0023] The furnace lining composition balances erosion resistance and thermal stability, allowing it to withstand the erosion of high-chromium, niobium-containing, and boron-containing alloy return materials during prolonged melting, thus preventing lining material from entering the molten steel and causing compositional contamination. The alumina content of 86%–88% ensures sufficient refractoriness and slag erosion resistance of the furnace lining, while the magnesium oxide content of 8%–10% enhances the thermal shock resistance of the furnace lining. Together, these two components ensure that the furnace lining maintains structural integrity under high-temperature smelting conditions above 1600℃, extending the service life of the furnace lining and preventing lining debris from entering the molten steel and affecting the accuracy of the alloy composition.

[0024] In an optional implementation, in step (2), fluorite ore is added at 1.5 to 2.5 kg / t of molten steel, and the temperature is raised to 1600 to 1620°C to take samples to confirm that the alloy element composition is stable; the temperature is further raised to 1670 to 1680°C, and silicon carbide is added at 0.3 to 0.5 kg / t for pre-deoxidation.

[0025] Insufficient fluorite addition results in insufficient slag fluidity and incomplete removal of inclusions, while excessive addition exacerbates furnace lining erosion. An addition of 1.5–2.5 kg / t ensures both slag fluidity and furnace lining life. Adding silicon carbide for pre-deoxidation at a high temperature of 1670–1680℃ ensures a sufficient deoxidation reaction, reducing the oxygen content of the molten steel to a low level and preventing high-oxygen molten steel from reacting with easily oxidized elements and causing burn-off during subsequent steelmaking and heating processes. Sampling confirms stable alloy element composition, preventing compositional fluctuations from affecting the control precision of subsequent steelmaking and blowing processes, and providing pre-melted steel with a clearly defined composition for electric arc furnace steelmaking.

[0026] In an optional implementation, in step (3), lime is added at a rate of 10-15 kg / t of molten steel to form slag.

[0027] The amount of lime added ensures that the slag basicity meets the dephosphorization requirements, while avoiding excessive slag volume that would lead to increased power consumption and slag-steel mixing. The retained oxidized slag from the furnace, together with the added lime, forms a high-basicity oxidizing slag system, providing sufficient slag phase capacity and oxidation conditions for the dephosphorization reaction in the subsequent blowing stage, thus ensuring dephosphorization efficiency. The lime slag formation also synergizes with the subsequent carbon injection to form foamed slag, providing a stable slag base for the formation of foamed slag.

[0028] In an optional implementation, in step (4), the heating adopts an electrical system with a voltage of 319V, a current of 22000A, and a smelting power of 5-6MW; the entire heating range of 1560℃ prohibits any form of oxygen blowing, oxygen spraying, or oxygen supply operation, and relies solely on electric energy for heating and submerged arc slag stabilization to achieve non-oxidative heating of alloying elements.

[0029] The high-current, low-voltage electrical system, combined with submerged arc operation, ensures concentrated and uniform heat input and stable arc, avoiding alloy oxidation and furnace lining erosion caused by exposed arc and localized high temperatures. The fixed electrical parameters of 319V, 22000A, and 5-6MW make the heating process stable and controllable. Combined with submerged arc slag stabilization, it achieves oxidation-free heating, physically eliminating alloy burn-off at low temperatures. If high-voltage, low-current or open operation is used, the arc will penetrate the slag layer to form a localized high-temperature zone, significantly aggravating the oxidation loss of alloy elements on the surface of molten steel. This is precisely the defect of the existing technology.

[0030] In an optional implementation, in step (5), after each spraying, the mixture is left to stand for 1 minute, and the spraying is repeated 3 times in a continuous cycle; the spraying flow rate of the carbon powder is 10 kg / min; the carbon powder is coke powder with a C content ≥ 90%.

[0031] Intermittent static setting allows bubbles to stabilize and coalesce into a film. Continuous cycling three times allows the foamed slag to gradually accumulate and thicken, forming a uniform and structurally stable closed foamed slag layer. The injection flow rate of 10 kg / min and the high carbon content of coke powder (≥90%) ensure that each injection generates sufficient CO gas in a short time and disperses it evenly in the slag layer, resulting in a thorough slag-forming reaction. This closed foamed slag layer, on the one hand, shields the air from direct contact with the molten steel, preventing secondary oxidation of the steel, and on the other hand, absorbs arc radiation, stabilizes the arc, and reduces furnace lining erosion. At the same time, it provides a stable slag phase basis for the weak oxidation mode of the slag surface in the subsequent blowing stage.

[0032] In an optional implementation, in step (6), the smelting electrical parameters are: voltage 300V, current 19000A; temperature rise to 1620℃~1630℃, oxygen supply pressure is constant at 0.4~0.5MPa; carbon content of molten steel is smelted to below 0.04%, and phosphorus content is smelted to below 0.003%.

[0033] Lowering electrical parameters and oxygen supply pressure results in gentle stirring of the molten pool and controlled oxygen mass transfer, which, combined with constant-rate decarburization, achieves uniform and controllable refining. The electrical parameters of 300V and 19000A are matched with the oxygen supply pressure of 0.4 to 0.5MPa, allowing the blowing process to proceed gently in a weak oxidation mode on the slag surface, avoiding splashing of molten steel and over-oxidation of alloys caused by strong stirring. The carbon content is smelted to below 0.04% and the phosphorus content to below 0.003%, meeting the ultra-purity requirements of high-end alloy steels such as P91 and P92. At the same time, the preferred temperature range of 1620℃ to 1630℃ takes into account the thermodynamic balance between decarburization kinetics and alloy protection.

[0034] In an optional implementation, in step (6), the decarbonization rate is controlled to be 0.01% / minute.

[0035] A decarburization rate of 0.01% / minute strikes a balance between decarburization efficiency and alloy protection. It ensures the smelting rhythm while avoiding alloy over-oxidation caused by concentrated oxygen potential. Too fast a decarburization rate will lead to a sudden increase in local oxygen potential and the oxidation of elements such as chromium and manganese. Too slow a rate will prolong smelting time and increase power consumption. A rate of 0.01% / minute can achieve selective removal of carbon and phosphorus while ensuring uniform decarburization. It works in conjunction with the low-pressure oxygen supply system to form a constant-rate precise impurity removal mode.

[0036] In an optional implementation, in step (7), oxygen blowing is stopped when the degree of smelting oxidation reaches 1 / 2 of the theoretical total oxidation.

[0037] The theoretical total oxidation amount is calculated based on the amount of carbon and phosphorus to be removed during smelting using stoichiometry: the amount of oxygen required is calculated and summed according to the stoichiometry of carbon oxidation to carbon monoxide and phosphorus oxidation to phosphorus pentoxide, respectively, based on the difference between the initial carbon content and the target carbon content and the difference between the initial phosphorus content and the target phosphorus content of the molten steel. The degree of oxidation is determined by the proportion of the cumulative oxygen supply to the theoretical total oxidation amount, and the blowing process is judged in real time by the cumulative measurement of the oxygen flow meter. When the cumulative oxygen supply reaches 1 / 2 of the theoretical total oxidation amount, the oxygen blowing is stopped. At this time, carbon and phosphorus have not been removed to the required extent. The remaining oxygen demand is supplemented by the oxidation slag retained in step (3): the ferrous oxide in the slag releases oxygen slowly into the molten steel under the weak oxidation mode on the slag surface, and reacts continuously with carbon and phosphorus in the steel, so that decarburization and dephosphorization continue to proceed to the target content after the oxygen is stopped. The gas phase oxygen supply and the slag phase oxygen supply each undertake half of the oxidation task. The molten steel will not experience a sudden increase in local oxygen potential due to the concentrated blowing of oxygen, leaving an operating window for the reducing slag adjustment in step (7). If oxygen blowing exceeds 1 / 2 of the theoretical total oxidation, the excess oxygen will directly oxidize alloying elements such as chromium, manganese, niobium, and boron, or cause excessive enrichment of iron oxide in the slag. After oxygen is stopped, the re-oxidation of alloying elements will intensify, and the consumption of reducing agent and smelting costs will increase. Using 1 / 2 oxidation degree as the endpoint criterion, the oxygen supply task is shared by the gas phase and slag phase in a determined ratio. The endpoint control is measurable and repeatable, ensuring batch process consistency.

[0038] In an optional implementation, in step (1), the waste return material is high-chromium, niobium-containing, boron-containing alloy steel cut heads, tails, steel chips, forging heads, and production line return waste.

[0039] This type of recycled alloy has high value, and low-cost, high-quality recycling smelting can be achieved by pre-melting in an induction furnace. Cut-off heads, tails, steel chips, forging heads, and recycled waste from the production line have the characteristics of known composition and low impurity content. After pre-melting, they can be directly used as raw materials for refining in an electric arc furnace, which greatly reduces the raw material cost of alloy steel smelting, while reducing the waste of metal resources, and has significant environmental and economic benefits.

[0040] In an optional implementation, a three-stage differentiated atmosphere control system is adopted, consisting of segmented non-oxidizing heating, slag stabilization and alloy protection, and controllable and precise oxidation.

[0041] The three-stage atmosphere control corresponds to three technical objectives: alloy preservation, stable operating conditions, and precise impurity removal. The non-oxidizing heating stage protects alloy elements through a completely oxygen-free process. The slag stabilization and alloy protection stage stabilizes the smelting conditions and isolates air through sealed foam slag. The controllable and precise oxidation stage achieves selective removal of carbon and phosphorus through low-pressure constant-speed blowing. The three stages are interconnected and work synergistically to overcome the technical defects of traditional dual-stage processes that cannot simultaneously achieve high alloy recovery rates and ultra-low impurity content.

[0042] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0043] Example 1 (1) An induction furnace with Al2O3 87% and MgO 9% refractory materials was used to charge high-chromium niobium-boron steel return material (analytical composition wt%: C=0.13, P=0.014, Cr=8.63, Nb=0.043, B=0.0023, Mn=0.48, the remainder being Fe and unavoidable impurities) and completely melted it; (2) Add 2 kg / t fluorite, heat to 1610℃ and take a sample to confirm that the alloy element composition is stable; heat to 1675℃, add 0.4 kg / t silicon carbide for pre-deoxidation, and remove the lumpy slag after tapping the steel. (3) Empty the residual steel from the electric arc furnace, retain the oxide slag, add 12 kg / t of lime, and slowly add the pre-melted steel. (4) No oxygen is blown throughout the process. Power is supplied at 319V, 22000A, and 5.5MW to raise the temperature to 1570℃. (5) Use 10kg / min carbon powder (coke powder, C content ≥90%), each injection lasts 45s, with a 1min interval, for 3 consecutive injections to create stable foam slag; (6) Heat to 1630℃, switch to 300V and 19000A, oxygen supply pressure 0.5MPa, control decarbonization rate 0.01% / min, smelt carbon content to below 0.04% and phosphorus content to below 0.003%; (7) When the oxidation degree reaches 1 / 2 of the theoretical total oxidation, stop the oxidation, add 5 kg / t of Si-Mn alloy to fine-tune the composition of the molten steel, and tap the steel at 1640℃; (8) Actual alloy recovery rate: Cr=96%, Nb=65%, B=24%, Mn=47%, and other elements ≥98%.

[0044] Example 2 (1) An induction furnace containing 86% Al2O3 and 10% MgO refractory materials was used to charge high-chromium niobium-boron steel recycled material (analytical composition wt%: C=0.14, P=0.015, Cr=8.56, Nb=0.046, B=0.0029, Mn=0.52, the remainder being Fe and unavoidable impurities) and it was completely melted; (2) Add 1.5 kg / t fluorite, heat to 1600℃ and take a sample to confirm that the alloy element composition is stable; heat to 1680℃, add 0.3 kg / t silicon carbide for pre-deoxidation, and remove the lumpy slag after tapping the steel. (3) Empty the residual steel from the electric arc furnace, retain the oxide slag, add 10 kg / t of lime, and slowly add the pre-melted steel. (4) No oxygen is blown throughout the process. Power is supplied at 319V, 22000A, and 5.5MW to raise the temperature to 1560℃. (5) Use 10kg / min carbon powder (coke powder, C content ≥90%), spray for 40s each time, with a 1min interval, for 3 consecutive times to create stable foam slag; (6) Heat to 1620℃, switch to 300V and 19000A, oxygen supply pressure 0.4MPa, control decarbonization rate 0.01% / min, smelt carbon content to below 0.04% and phosphorus content to below 0.003%; (7) When the oxidation degree reaches 1 / 2 of the theoretical total oxidation, stop the oxidation, add 5 kg / t of Si-Mn alloy to fine-tune the composition of the molten steel, and tap the steel at 1635℃; (8) Actual alloy recovery rate: Cr=97%, Nb=66%, B=28%, Mn=43%, and other elements ≥98%.

[0045] Example 3 (1) An induction furnace with Al2O3 88% and MgO 8% refractory materials was used to charge high-chromium niobium-boron steel return material (analytical composition wt%: C=0.16, P=0.016, Cr=8.72, Nb=0.047, B=0.0016, Mn=0.47, the remainder being Fe and unavoidable impurities) and completely melted it; (2) Add 2.5 kg / t fluorite, heat to 1620℃ and take a sample to confirm that the alloy element composition is stable; heat to 1670℃, add 0.3 kg / t silicon carbide for pre-deoxidation, and remove the lumpy slag after tapping the steel. (3) Empty the residual steel from the electric arc furnace, retain the oxide slag, add 11 kg / t of lime, and slowly add the pre-melted steel. (4) No oxygen is blown throughout the process. Power is supplied at 319V, 22000A, and 5.5MW to raise the temperature to 1580℃. (5) Use 10kg / min carbon powder (coke powder, C content ≥90%), spray for 40s each time, with a 1min interval, for 3 consecutive times to create stable foam slag; (6) Heat to 1620℃, switch to 300V and 19000A, oxygen supply pressure 0.4MPa, control decarbonization rate 0.01% / min, smelt carbon content to below 0.04% and phosphorus content to below 0.003%; (7) When the oxidation degree reaches 1 / 2 of the theoretical total oxidation, stop the oxidation, add 5 kg / t of Si-Mn alloy to fine-tune the composition of the molten steel, and tap the steel at 1650℃; (8) Actual alloy recovery rate: Cr=96.5%, Nb=64%, B=26%, Mn=45%, and other elements ≥98%.

[0046] Example 4 (1) An induction furnace with Al2O3 87% and MgO 9% refractory materials was used to charge high-chromium niobium-boron steel return material (analytical composition wt%: C=0.11, P=0.017, Cr=8.83, Nb=0.049, B=0.0035, Mn=0.55, the remainder being Fe and unavoidable impurities) and completely melted it; (2) Add 1.8 kg / t fluorite, heat to 1610℃ and take a sample to confirm that the alloy element composition is stable; heat to 1675℃, add 0.5 kg / t silicon carbide for pre-deoxidation, and remove the lumpy slag after tapping the steel. (3) Empty the residual steel from the electric arc furnace, retain the oxide slag, add 10 kg / t of lime, and slowly add the pre-melted steel. (4) No oxygen is blown throughout the process. Power is supplied at 319V, 22000A, and 5.5MW to raise the temperature to 1565℃. (5) Use 10kg / min carbon powder (coke powder, C content ≥90%), each injection lasts 45s, with a 1min interval, for 3 consecutive injections to create stable foam slag; (6) Heat up to 1620℃, switch to 300V and 19000A, oxygen supply pressure 0.4MPa, control decarbonization rate 0.005% / min, smelt carbon content to below 0.04% and phosphorus content to below 0.003%; (7) When the oxidation degree reaches 1 / 2 of the theoretical total oxidation, stop the oxidation, add 5 kg / t of Si-Mn alloy to fine-tune the composition of the molten steel, and tap the steel at 1630℃; (8) Actual alloy recovery rate: Cr=97.5%, Nb=67%, B=26%, Mn=47%, and other elements ≥98%.

[0047] Example 5 (1) An induction furnace with Al2O3 88% and MgO 8% refractory materials was used to charge high-chromium niobium-boron steel return material (analytical composition wt%: C=0.15, P=0.016, Cr=8.72, Nb=0.054, B=0.003, Mn=0.55, the remainder being Fe and unavoidable impurities) and completely melted it; (2) Add 2.2 kg / t fluorite, heat to 1620℃ and take a sample to confirm that the alloy element composition is stable; heat to 1680℃, add 0.5 kg / t silicon carbide for pre-deoxidation, and remove the lumpy slag after tapping the steel. (3) Empty the residual steel from the electric arc furnace, retain the oxide slag, add 15 kg / t of lime, and slowly add the pre-melted steel. (4) No oxygen is blown throughout the process. Power is supplied at 319V, 22000A, and 5.5MW to raise the temperature to 1590℃. (5) Use 10kg / min carbon powder (coke powder, C content ≥90%), spray for 50s each time, with a 1min interval, for 3 consecutive times to create stable foam slag; (6) Heat to 1680℃, switch to 300V and 19000A, oxygen supply pressure 0.6MPa, control decarbonization rate 0.015% / min, smelt carbon content to below 0.04% and phosphorus content to below 0.003%; (7) When the oxidation degree reaches 1 / 2 of the theoretical total oxidation, stop the oxidation, add 5 kg / t of Si-Mn alloy to fine-tune the composition of the molten steel, and tap the steel at 1660℃; (8) Actual alloy recovery rate: Cr=95%, Nb=61%, B=22%, Mn=41%, and other elements ≥98%.

[0048] Comparative Example 1 The process parameters are the same as in Example 1, except that the oxygen supply pressure in step (6) is increased from 0.5MPa to 8MPa, and a high-pressure strong oxidation blowing mode is adopted.

[0049] Results: During the blowing process, the molten steel was violently stirred and splashed significantly, and the decarburization rate fluctuated greatly (measured from 0.02% / min to 0.04% / min), making it impossible to achieve uniform and controllable decarburization; measured alloy recovery rates: Cr=51%, Nb=15%, B=8%, Mn=10%.

[0050] Compared with Example 1, although high-pressure strong oxidation blowing can complete decarburization and dephosphorization, the molten steel is severely over-oxidized, the burning loss of chromium, manganese, niobium and boron is aggravated, and the alloy loss is significantly increased, making it impossible to achieve both low burning loss and ultra-purity.

[0051] Comparative Example 2 The process parameters are the same as in Example 1, except that step (4) is changed to oxygen blowing and heating immediately after steel is added, and oxygen is not prohibited throughout the process.

[0052] Results: In the low-temperature range (below 1560℃), alloying elements are preferentially oxidized. The measured alloy recovery rates are: Cr=32%, Nb=7%, B=0%, Mn=8%.

[0053] Compared with Example 1, when oxygen-free heating was not used throughout the process, chromium, niobium, boron, manganese and boron all suffered significant burn-off in the low-temperature section, proving that oxygen-free pure electric heating plays a key role in protecting easily oxidized alloying elements.

[0054] Comparative Example 3 The process parameters are the same as in Example 1, except that the blowing system in step (5) is changed to continuous blowing, without interval static circulation.

[0055] Results: Continuous carbon injection can cause local carbon powder accumulation in the slag layer, damaging the slag surface and making it impossible to form a stable and uniform closed foam slag, resulting in incomplete coverage and alloy burn-off. The measured alloy recovery rates were: Cr=58%, Nb=13%, B=9%, Mn=12%.

[0056] Compared with Example 1, continuous carbon injection cannot form a stable and uniform closed foam slag layer, resulting in deterioration of smelting conditions and increased alloy burn-off. This proves that fixed-sequence pulse injection plays an irreplaceable role in the stability of foam slag and alloy protection.

[0057] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for smelting high-alloy steel with low burn-off, characterized in that, Includes the following steps: (1) An induction melting furnace is used to melt scrap recycled raw materials containing chromium, niobium, boron and manganese alloy steel; (2) After the molten steel is completely melted, fluorite ore is added, and the temperature is raised and samples are taken to confirm that the alloy element composition is stable; the temperature is raised further, silicon carbide is added for pre-deoxidation, and the slag is removed after tapping the steel. (3) Empty the residual molten steel inside the electric arc furnace, retain the oxidized slag from the furnace, add lime to make slag, and pour the pre-melted molten steel into the electric arc furnace; (4) After the steel is poured, the entire process is carried out using oxygen-free pure electric energy to raise the temperature until the temperature of the molten steel is stable at ≥1560℃; (5) Use carbon powder intermittent blowing to make foam slag; the blowing system is: blow for 40-50 seconds at a time, and then let it stand at intervals for a cycle of blowing, and do not blow oxygen throughout the process; (6) After the foamy slag forms and stably covers the molten steel surface, the temperature is raised to 1620℃~1680℃; single-pipe oxygen blowing is adopted, and the oxygen supply pressure is kept constant at 0.4~0.6MPa, and smelting is carried out in the weak oxidation mode of slag surface; the decarburization rate is controlled at 0.005~0.015% / minute. (7) After smelting, stop oxygen blowing, adjust the slag reducing properties, add alloys to adjust the steel composition, and control the tapping temperature to ≥1630℃.

2. The smelting method according to claim 1, characterized in that: In step (2), fluorite ore is added at 1.5 to 2.5 kg / t of molten steel, and the temperature is raised to 1600 to 1620℃. Samples are taken to confirm that the alloy element composition is stable. The temperature is then raised to 1670 to 1680℃, and silicon carbide is added at 0.3 to 0.5 kg / t for pre-deoxidation.

3. The smelting method according to claim 1, characterized in that: In step (3), lime is added at a rate of 10-15 kg / t of molten steel to form slag.

4. The smelting method according to claim 1, characterized in that: In step (4), the heating is carried out using an electrical system with a voltage of 319V, a current of 22000A, and a smelting power of 5-6MW.

5. The smelting method according to claim 1, characterized in that: In step (5), after each spraying, the mixture is left to stand for 1 minute, and the spraying is repeated 3 times in a continuous cycle; the spraying flow rate of the carbon powder is 10 kg / min; the carbon powder is coke powder with a C content ≥ 90%.

6. The smelting method according to claim 1, characterized in that: In step (6), the smelting electrical parameters are voltage 300V and current 19000A; the carbon content of the molten steel is smelted to below 0.04% and the phosphorus content is smelted to below 0.003%.

7. The smelting method according to claim 1, characterized in that: In step (6), the decarbonization rate is controlled at 0.01% / minute.

8. The smelting method according to claim 1, characterized in that: In step (7), oxygen blowing is stopped when the smelting oxidation degree reaches 1 / 2 of the theoretical total oxidation.

9. The smelting method according to claim 1, characterized in that: In step (6), the temperature is raised to 1620℃~1630℃, and the oxygen supply pressure is kept constant at 0.4~0.5MPa.

10. The smelting method according to claim 1, characterized in that: The alloy recovery rate is controlled throughout the smelting process as follows: chromium recovery rate ≥95%, niobium recovery rate 60%~70%, boron recovery rate 20%~30%, manganese recovery rate 40%~50%, and recovery rate of other alloying elements ≥98%.

Citation Information

Patent Citations

  • Method for producing high-alloy low-phosphorous steel used for boiler tube by adopting electric-arc furnace

    CN102634634A

  • Technology for fabricating foaming slag in arc furnace molten pool

    CN104131134A

  • Process of smelting stainless steel in electric arc furnace with back blowing method

    CN104178596A

  • A process for smelting ultra-high-grade duplex stainless steel of CD3MWN material

    CN108823348B

  • Method for improving Cr yield of electric furnace

    CN111809017A