A method for efficiently increasing nitrogen content and achieving high purity in the smelting of high-nitrogen steel
By combining hydrogen-containing plasma arc and nitrogen plasma in a smelting method, the technical challenges of efficient nitrogen increase and high cleanliness have been solved, enabling the efficient production of high-nitrogen steel and meeting the needs of large-scale production.
Patent Information
- Application Number
- CN202611618844.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot achieve efficient and uniform nitrogen increase while maintaining stable control of molten steel cleanliness, making it difficult to achieve large-scale production of high-nitrogen steel.
A hydrogen-containing plasma arc is used in conjunction with refining slag for deep deoxidation and desulfurization. Combined with nitrogen plasma and nitrogen bottom blowing stirring, alloying and pressurized casting are carried out simultaneously to improve nitrogen solubility and cleanliness.
The nitrogen content in high-nitrogen steel is 0.1%~0.5%, oxygen content ≤15ppm, and sulfur content ≤30ppm, meeting the composition and cleanliness requirements of high-nitrogen steel.
Smart Images

Figure CN123108401A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of iron and steel smelting technology, and more specifically to a method for smelting high-nitrogen steel with high efficiency and high purity. Background Technology
[0002] High-nitrogen steel is a special type of steel in which nitrogen, as the core alloying element, is dissolved in the steel matrix. Nitrogen can partially or completely replace the expensive nickel element in steel, significantly improving the material's strength, hardness, wear resistance, and corrosion resistance. It has broad application prospects in aerospace, marine engineering, medical devices, energy conservation and environmental protection, and high-end equipment manufacturing. However, nitrogen has extremely low solubility in molten steel at normal pressure, and nitrogen will precipitate during the solidification process of molten steel, forming porosity defects. Therefore, how to achieve efficient and uniform nitrogen addition while stably controlling the cleanliness of molten steel is the core technical bottleneck restricting the large-scale industrial production of high-nitrogen steel.
[0003] Nitrogen enrichment technologies for high-nitrogen steel are mainly divided into three categories: alloy enrichment, gas enrichment, and pressure smelting. Among them, alloy enrichment achieves nitrogen enrichment by adding nitride alloys such as chromium nitride and manganese nitride, but it has drawbacks such as high cost of alloy raw materials, large fluctuations in nitrogen yield, and easy introduction of non-metallic inclusions that reduce the cleanliness of molten steel. Atmospheric pressure gas enrichment increases nitrogen through bottom blowing, but it suffers from slow enrichment rate and low enrichment efficiency, resulting in generally low nitrogen content in the steel, which cannot meet the composition requirements of high-nitrogen steel. Pressure smelting methods such as pressure induction furnaces and pressure electroslag remelting can significantly improve nitrogen solubility, but the output per furnace is low and the equipment investment is high, making it difficult to adapt to the needs of large-scale industrial production.
[0004] Patent document CN122327072A discloses a low-cost nitrogen-enhancing smelting method for non-quenched and tempered steel for crankshafts. This method increases the nitrogen content of the steel by staged control of the intensity of top-blown oxygen and bottom-blown nitrogen in the converter, and achieves a balance between inclusion removal and nitrogen enhancement through staged control in the RH process. While this method ensures the cleanliness of the steel, the final nitrogen content is only 0.013%~0.016 wt.%, far below the composition requirements for high-nitrogen steel.
[0005] Patent document CN122279365A discloses a smelting method for high-purity nitrogen- and sulfur-containing steel. Nitrogen is increased through bottom blowing nitrogen in the entire process of converter tapping, LF refining, and RH vacuum treatment. However, the nitrogen content in the final steel is only 0.016%~0.019wt.%, which still falls into the category of low-nitrogen steel and cannot meet the performance requirements of high-nitrogen steel.
[0006] Therefore, a high-purity, high-efficiency nitrogen-enrichment smelting method for high-nitrogen steel is needed. Summary of the Invention
[0007] In view of the technical problems in the preparation technology of high nitrogen steel, such as low nitrogen increase efficiency, difficulty in increasing nitrogen content, difficulty in controlling the cleanliness of molten steel, and inability to adapt to large-scale production, the purpose of this invention is to provide a method for smelting high nitrogen steel with high efficiency in nitrogen increase and high cleanliness, which has both high cleanliness and high efficiency in nitrogen increase.
[0008] The technical solution of the present invention is as follows: A method for smelting high-nitrogen steel includes the following steps: (1) The raw materials are smelted in an electric arc furnace. A hydrogen-containing mixed gas is blown into the electric arc zone to form a hydrogen-containing plasma electric arc for heating and melting. When the furnace charge is completely melted and the temperature of the initial molten steel rises to above 1600°C, the molten steel is tapped into the ladle. (2) Perform LF refining, add refining slag, blow hydrogen into the arc zone to form a hydrogen plasma arc, and simultaneously stir by blowing nitrogen from the bottom of the ladle; (3) Nitrogen gas is blown into the arc region to form nitrogen plasma, and alloying is carried out simultaneously; (4) The casting is completed under nitrogen pressure atmosphere, with a casting pressure of 0.3~1.0MPa and a casting superheat of 50~100℃. The nitrogen pressure atmosphere is maintained until the molten steel is completely cooled and formed to obtain high nitrogen steel ingot.
[0009] In the above smelting method, the hydrogen-containing mixed gas includes hydrogen and an inert gas, wherein the inert gas includes argon or nitrogen.
[0010] In the above smelting method, the hydrogen content in the hydrogen-containing mixed gas is 10% to 50% by volume percentage.
[0011] In the above smelting method, in step (1), the injection flow rate is 10~50NL / (min·t).
[0012] In the above smelting method, the refining slag, by mass fraction, includes 50-60 parts CaO, 5-10 parts SiO2, 20-30 parts Al2O3, 5-10 parts MgO, and <1 part FeO and MnO. The amount of refining slag added is 1-3% of the mass of molten steel.
[0013] In the above smelting method, in step (2), the hydrogen injection flow rate is 10~30NL / (min·t) and the injection pressure is 0.4~0.7MPa.
[0014] In the above smelting method, in step (2), the refining time is 5~25min and the molten steel temperature is 1550~1620℃.
[0015] In the above smelting method, in step (2), the flow rate of nitrogen is 5~25NL / (min·t), and the injection pressure is 0.7~1.0MPa.
[0016] In the above smelting method, in step (3), the nitrogen injection flow rate is 10~50NL / (min·t) and the injection pressure is 0.4~0.7MPa.
[0017] In the above smelting method, in step (3), the time for adding nitrogen and alloying molten steel is 10~30 min.
[0018] The beneficial effects of this invention are as follows: The smelting method of this invention achieves high-purity steel smelting through hydrogen-containing plasma refining combined with refining slag production; and achieves efficient nitrogen enrichment of the molten steel through nitrogen plasma, nitrogen bottom blowing, and nitrogen pressurized casting. The high-nitrogen steel ingots obtained according to this method have a nitrogen mass fraction of 0.1%~0.5%, an oxygen mass fraction ≤15ppm, and a sulfur mass fraction ≤30ppm. Attached Figure Description
[0019] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope of the present invention.
[0020] Figure 1 This is a flowchart of the smelting method for high-nitrogen steel in Example 1. Detailed Implementation
[0021] The embodiments of the present invention will be described in detail below with reference to examples, and are intended to explain the present invention, but should not be construed as limiting the present invention. Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods.
[0022] A method for smelting high-nitrogen steel includes the following steps: (1) The smelting raw materials can be one or more of scrap steel, direct reduced iron, and recycled materials. The smelting raw materials are smelted in an electric arc furnace. A hydrogen-containing mixed gas is blown into the electric arc zone to form a hydrogen-containing plasma arc for heating and melting. When the furnace charge is completely melted and the temperature of the primary molten steel rises to above 1600℃, this condition is conducive to the subsequent deep deoxidation and desulfurization steps. The molten steel is then tapped into the ladle. The entire tapping process adopts a slag-blocking tapping process, which can reduce the amount of slag.
[0023] Hydrogen-containing plasma arcs have shorter arc lengths and higher heat transfer efficiency, making it easier to transfer heat to the molten pool during smelting and enabling rapid melting of the furnace charge. Hydrogen-containing plasma arcs also have higher temperatures and a stronger impact on the molten pool than traditional air arcs. The introduction of hydrogen gas creates a strongly reducing atmosphere above the molten pool, preventing oxidation of the molten steel caused by contact with air.
[0024] The hydrogen-containing gas mixture may include hydrogen and an inert gas, preferably argon or nitrogen. The hydrogen content in the gas mixture is 10%–50% by volume. The injection flow rate is 10–50 NL / (min·t).
[0025] (2) LF refining is carried out, and refining slag is added. By mass fraction, the refining slag includes 50-60 parts CaO, 5-10 parts SiO2, 20-30 parts Al2O3, 5-10 parts MgO, and <1 part FeO and MnO. The amount of refining slag added is 1-3% of the mass of the molten steel. Hydrogen gas is blown into the arc zone to form a highly active hydrogen plasma arc. The refining time is preferably 5-25 minutes, and the temperature of the molten steel is controlled at 1550-1620℃. While heating, the reduction reaction of the molten pool is strengthened. This process deeply deoxidizes and desulfurizes, reducing oxygen and sulfur to extremely low levels. The deoxidation and desulfurization efficiency is significantly improved, ensuring the high cleanliness of high-nitrogen steel. At the same time, nitrogen is blown from the bottom of the ladle for stirring to promote the slag-metal reaction and the floating of inclusions, thus completing the deep deoxidation, desulfurization and inclusion removal of the molten steel.
[0026] The hydrogen injection flow rate is 10~30 NL / (min·t), and the injection pressure is 0.4~0.7 MPa. The nitrogen flow rate is 5~25 NL / (min·t), and the injection pressure is 0.7~1.0 MPa. In this step, the bottom-blown nitrogen is mainly used for stirring; excessive flow rate should be avoided to prevent large fluctuations in nitrogen content.
[0027] The above steps use a hydrogen-containing plasma arc as a heat source, which utilizes the high temperature and high thermal conductivity of the plasma to achieve rapid melting of the furnace charge, and removes impurity elements from the steel through the reduction effect of highly active hydrogen plasma. At the same time, a strong reducing atmosphere is created in the furnace to avoid oxidation of the molten steel in the initial refining process, thereby reducing the load for subsequent refining.
[0028] (3) After deep purification, maintain a stable steel temperature. Blow nitrogen into the arc zone to form nitrogen plasma, achieving efficient nitrogen enrichment of the molten steel. Maintain a constant bottom-blown nitrogen flow rate and simultaneously carry out alloying, further improving the solubility of nitrogen. During the nitrogen enrichment process, add alloying elements such as chromium, manganese, molybdenum, and nickel according to the composition requirements of the target steel grade to complete the steel composition adjustment. This step has a high alloy yield, and the optimal time for nitrogen enrichment and alloying of the molten steel is 10-30 minutes. If the time is shorter than this range, the nitrogen content of the ingot may not reach the expected level.
[0029] The nitrogen injection flow rate is 10~50 NL / (min·t), and the injection pressure is 0.4~0.7 MPa.
[0030] (4) Nitrogen gas can be introduced into the equipment for 1 to 3 minutes to purge the air in the equipment to avoid oxidation and contamination of the molten steel. Then, the casting is completed under nitrogen pressure atmosphere, with a casting pressure of 0.3 to 1.0 MPa and a casting superheat of 50 to 100°C. The nitrogen pressure atmosphere is maintained until the molten steel is completely cooled and formed to obtain a high-nitrogen steel ingot.
[0031] This step increases the nitrogen partial pressure during solidification by pressurizing the nitrogen during casting, which significantly improves the solidification solubility of nitrogen in steel, effectively inhibits the precipitation of nitrogen and the formation of porosity defects, and ensures that the nitrogen content of the ingot meets the standard stably.
[0032] The smelting method of the present invention first uses hydrogen plasma in conjunction with refining slag to achieve deep deoxidation, desulfurization and inclusion removal of molten steel to obtain high-purity molten steel; then it switches to nitrogen plasma in conjunction with bottom blowing nitrogen, using highly active nitrogen plasma to greatly improve the nitrogen enrichment rate and efficiency, so as to achieve simultaneous homogenization of composition and efficient nitrogen enrichment.
[0033] Example 1 This embodiment is used to prepare 10 tons of high-purity austenitic stainless steel with a nitrogen content of 0.2 wt%.
[0034] A method for smelting high-nitrogen steel, such as Figure 1 As shown, it includes the following steps: (1) Rapid smelting in electric arc furnace Six tons of scrap steel and four tons of direct reduced iron are charged. After energizing and arc ignition, a hydrogen-argon mixture is blown in through hollow graphite electrodes to form a hydrogen-containing plasma arc. The hydrogen-containing gas mixture accounts for 20% of the volume, and the total gas flow rate is 200 NL / min. When the furnace charge is completely melted and the temperature of the initial molten steel reaches 1620℃, the molten steel is transferred to the ladle using a slag-blocking tapping process.
[0035] (2) LF furnace refining and deep purification The ladle is hoisted to the LF refining station, where 200 kg of refining slag is added. The slag composition is: CaO 56%, SiO 29%, Al2O3 25.1%, MgO 9.3%, FeO + MnO 0.6%. Hydrogen gas is blown into the arc zone through hollow electrodes to form hydrogen plasma at a flow rate of 160 NL / min and a pressure of 0.5 MPa. Simultaneously, nitrogen is blown into the ladle from the bottom for stirring at a flow rate of 60 NL / min and a pressure of 0.8 MPa. The refining time is 20 min, and the molten steel temperature is controlled at 1580~1600℃.
[0036] (3) LF furnace alloying and molten steel nitrogen addition After deep purification, the molten steel temperature is maintained at a stable 1590℃. Nitrogen gas is blown into the arc zone through hollow graphite electrodes to form nitrogen plasma, with a blowing flow rate of 250 NL / min and a blowing pressure of 0.6 MPa. The bottom-blowing nitrogen flow rate is maintained at 60 NL / min. During the nitrogen addition process, metallic chromium, metallic nickel, and electrolytic manganese are added to adjust the composition of the molten steel. The time for nitrogen addition and alloying of the molten steel is 15 minutes.
[0037] (4) Pressure casting The ladle is hoisted to the pressure casting equipment, and nitrogen gas is first introduced to purge the equipment cavity for 2 minutes to remove all air. Then, casting is completed under a nitrogen pressure atmosphere of 0.6 MPa, with a casting superheat of 70°C. The nitrogen pressure atmosphere is maintained until the molten steel completely cools and solidifies, resulting in a high-nitrogen steel ingot.
[0038] Testing revealed that the average nitrogen content of the ingots obtained in this embodiment was 0.21 wt%, the oxygen content was 14 ppm, and the sulfur content was 26 ppm, thus achieving the preparation of high-nitrogen austenitic stainless steel.
[0039] Example 2 This embodiment is used to prepare 10 tons of high-purity austenitic stainless steel with a nitrogen content of 0.45wt%.
[0040] A method for smelting high-nitrogen steel includes the following steps: (1) Rapid smelting in electric arc furnace 7 tons of high-nitrogen steel return material and 3 tons of scrap steel are loaded. After energizing and arc ignition, a hydrogen-nitrogen mixture is blown in through hollow graphite electrodes to form a hydrogen-containing plasma arc. The hydrogen-containing gas mixture accounts for 50% of the volume, and the total gas flow rate is 300 NL / min. When the furnace charge is completely melted and the temperature of the initial molten steel reaches 1650℃, the molten steel is transferred to the ladle using a slag-blocking tapping process.
[0041] (2) LF furnace refining and deep purification The ladle is hoisted to the LF refining station, where 250 kg of refining slag is added. The slag composition is: CaO 58%, SiO 26%, Al2O3 28%, MgO 7.6%, FeO + MnO 0.4%. Hydrogen plasma is formed by blowing hydrogen gas into the arc zone through hollow electrodes at a flow rate of 230 NL / min and a pressure of 0.7 MPa. Simultaneously, nitrogen gas is blown from the bottom of the ladle for stirring at a flow rate of 70 NL / min and a pressure of 0.9 MPa. The refining time is 25 min, and the molten steel temperature is controlled at 1590~1610℃.
[0042] (3) LF furnace alloying and molten steel nitrogen addition After deep purification, the molten steel temperature was maintained at 1600℃. Nitrogen gas was blown into the arc zone through hollow graphite electrodes to form nitrogen plasma at a flow rate of 350 NL / min and a pressure of 0.6 MPa. The bottom-blowing nitrogen flow rate was maintained at 70 NL / min. During the nitrogen enrichment process, metallic chromium, metallic molybdenum, and electrolytic manganese were added to adjust the composition of the molten steel. The nitrogen enrichment and alloying time for the molten steel was 28 minutes.
[0043] (4) Pressure casting The ladle is hoisted to the pressure casting equipment, and nitrogen gas is first introduced to purge the equipment cavity for 3 minutes to remove all air. Then, casting is completed under a nitrogen pressure atmosphere of 0.8 MPa, with a casting superheat of 90°C. The nitrogen pressure atmosphere is maintained until the molten steel completely cools and solidifies, resulting in a high-nitrogen steel ingot.
[0044] Testing revealed that the average nitrogen content of the ingots obtained in this embodiment was 0.45 wt%, the oxygen content was 11 ppm, and the sulfur content was 28 ppm, thus achieving the preparation of high-nitrogen austenitic stainless steel.
[0045] Comparative Example 1 The smelting method of this comparative example includes the following steps: Steps (1) and (2) are the same as in Example 1.
[0046] (3) Nitrogen alloying of molten steel in a pressurized ladle, with nitrogen blown from the bottom during the alloying process.
[0047] Step (4) is the same as in Example 1.
[0048] Testing revealed that the average nitrogen content of the ingots obtained in this comparative example was 0.19 wt%, the oxygen content was 18 ppm, and the sulfur content was 27 ppm. The multiple transfers of the molten steel resulted in the cleanliness of the molten steel not reaching the expected level.
[0049] Comparative Example 2 The smelting method of this comparative example includes the following steps: Steps (1), (2) and (3) are the same as in Example 1.
[0050] Step (4) involves casting in an atmospheric pressure atmosphere.
[0051] The tests showed that the average nitrogen content of the ingots obtained in this comparative example was 0.15 wt%, the oxygen content was 23 ppm, and the sulfur content was 27 ppm. During the solidification process of the ingots at normal pressure, the nitrogen solubility decreased, a large amount of dissolved nitrogen escaped, and the air caused some pollution to the molten steel. The nitrogen content and cleanliness of the ingots did not reach the expected level.
[0052] Comparative Example 3 The smelting method of this comparative example includes the following steps: Steps (1) and (2) are the same as in Example 2.
[0053] In step (3), chromium nitride is used for nitrogen alloying in the LF furnace refining process instead of nitrogen plasma for nitrogen enrichment.
[0054] Step (4) is the same as in Example 2.
[0055] Testing revealed that the average nitrogen content of the ingots obtained in this comparative example was 0.45 wt%, the oxygen content was 18 ppm, and the sulfur content was 29 ppm. During the process of adding nitride alloy to increase nitrogen content, the reaction in the molten pool was violent, resulting in the ingot cleanliness not reaching the expected level.
[0056] Comparative Example 4 The smelting method of this comparative example includes the following steps: Step (1) is the same as in Example 2.
[0057] In step (2), hydrogen plasma refining is not used in the LF furnace refining process; instead, deoxidation is carried out by adding aluminum and silicon particles.
[0058] Steps (3) and (4) are the same as in Example 2.
[0059] Testing revealed that the average nitrogen content of the ingots obtained in this comparative example was 0.44 wt%, the oxygen content was 21 ppm, and the sulfur content was 37 ppm. The aluminum and silicon deoxidation products were not completely removed and remained in the molten steel, resulting in the ingot cleanliness not reaching the expected level.
[0060] It is understood that those skilled in the art can make changes, modifications or substitutions to the above embodiments within the scope of the present invention without departing from the principles and spirit of the present invention, and such changes, modifications or substitutions do not cause the essence of the corresponding technical solutions to depart from the scope of the technical solutions of the various embodiments of the present invention.
Claims
1. A method for efficiently increasing nitrogen content and achieving high purity in the smelting of high-nitrogen steel, characterized in that, Includes the following steps: (1) The raw materials are smelted in an electric arc furnace. A hydrogen-containing mixed gas is blown into the electric arc zone to form a hydrogen-containing plasma electric arc for heating and melting. When the furnace charge is completely melted and the temperature of the initial molten steel rises to above 1600°C, the molten steel is tapped into the ladle. (2) Perform LF refining, add refining slag, blow hydrogen into the arc zone to form a hydrogen plasma arc, and simultaneously stir by blowing nitrogen from the bottom of the ladle; (3) Nitrogen gas is blown into the arc region to form nitrogen plasma, and alloying is carried out simultaneously; (4) The casting is completed under nitrogen pressure atmosphere, with a casting pressure of 0.3~1.0MPa and a casting superheat of 50~100℃. The nitrogen pressure atmosphere is maintained until the molten steel is completely cooled and formed to obtain high nitrogen steel ingot.
2. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, The hydrogen-containing mixed gas includes hydrogen and an inert gas, wherein the inert gas includes argon or nitrogen.
3. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1 or 2, characterized in that, The hydrogen-containing gas mixture contains 10% to 50% hydrogen by volume percentage.
4. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, In step (1), the injection flow rate is 10~50 NL / (min·t).
5. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, The refining slag, by mass fraction, comprises 50-60 parts CaO, 5-10 parts SiO2, 20-30 parts Al2O3, 5-10 parts MgO, and <1 part FeO and MnO. The amount of refining slag added is 1-3% of the mass of molten steel.
6. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, In step (2), the hydrogen injection flow rate is 10~30NL / (min·t) and the injection pressure is 0.4~0.7MPa.
7. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, In step (2), the refining time is 5~25 min and the molten steel temperature is 1550~1620℃.
8. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, In step (2), the flow rate of nitrogen is 5~25NL / (min·t) and the injection pressure is 0.7~1.0MPa.
9. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, In step (3), the nitrogen injection flow rate is 10~50NL / (min·t) and the injection pressure is 0.4~0.7MPa.
10. The method for high-efficiency nitrogen enrichment and high-purity smelting of high-nitrogen steel according to claim 1, characterized in that, In step (3), the time for adding nitrogen and alloying molten steel is 10~30 min.
Citation Information
Patent Citations
Smelting method of high-cleanliness nitrogen-containing and sulfur-containing steel
CN122279365A
Low-cost nitrogen-increasing smelting method for non-quenched and tempered steel for crankshaft