Electro-melting-continuous casting method for preparing p92 heat-resistant steel for ultra-supercritical high-pressure boiler

By optimizing the slag composition and the staged nitrogen enrichment process, combined with dynamic water distribution and slow cooling processes, the problems of unstable nitrogen control and continuous casting quality of P92 steel were solved, achieving stable production of high-performance P92 steel and reducing production costs.

CN123108402APending Publication Date: 2026-11-17SHANDONG IRON & STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611146466.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously solve the problems of precise nitrogen control, slag system optimization, continuous casting quality improvement, and process economy for P92 steel, resulting in defects such as uneven composition, excessive inclusions, and unqualified high-temperature creep strength, making them unsuitable for short-process production in ordinary electric furnaces.

Method used

By adopting coordinated adjustments to raw material control, slag system optimization, staged nitrogen increase, dynamic water distribution for continuous casting, and slow cooling process, including optimizing slag composition, staged nitrogen increase, dynamic secondary cooling water distribution, and segmented electromagnetic stirring, combined with slow cooling process, stable production of high-quality P92 steel can be achieved.

Benefits of technology

It achieves precise control and stable improvement of nitrogen content, improves the purity of molten steel, produces excellent quality continuously cast billets, reduces production costs, has strong adaptability, and meets the high-performance requirements of steel for ultra-supercritical boilers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108402A_ABST
    Figure CN123108402A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of iron and steel metallurgy, specifically relating to an electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers. The method includes the following steps: raw material preparation; electric furnace steelmaking; LF refining; VD vacuum treatment; continuous casting; and slow cooling annealing. Through coordinated adjustments of raw material control, slag system optimization, staged nitrogen addition, dynamic water distribution during continuous casting, and slow cooling processes, the problems of unstable nitrogen content control, high nitrogen addition costs, and numerous defects in continuously cast billets in existing technologies are solved. Stable production of high-quality P92 steel can be achieved in a conventional electric furnace-LF-VD short-process production line, reducing production costs and meeting the high-performance requirements of steel for ultra-supercritical boilers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of iron and steel metallurgy, specifically relating to an electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers. Background Technology

[0002] P92 steel is a ferritic heat-resistant steel specifically designed for ultra-supercritical high-pressure boilers. Unlike conventional boiler steels such as P91, 12Cr1MoV, and austenitic stainless steel, its core characteristic is a 9Cr matrix composite W, Mo, V, Nb, and N multi-element strengthening alloy. It achieves excellent high-temperature creep resistance and oxidation resistance at 600℃ through dual strengthening by solid solution and carbonitride precipitation, making it an irreplaceable material for high-end thermal power pressure-bearing components.

[0003] P92 steel presents several technical challenges in smelting due to its unique alloy system: high specific gravity makes W and Nb prone to segregation; nitrogen content needs to be precisely controlled within a narrow range; the control thresholds for impurities such as S, O, Ti, and Al are much lower than those for other heat-resistant steels; and the morphology of deoxidized inclusions needs to be directionally modified to suppress high-temperature performance degradation.

[0004] Traditional smelting methods designed for single-molybdenum P91, low-alloy chromium-molybdenum steel, and austenitic stainless steel cannot meet the special process requirements of P92, such as multi-alloy synergistic control, ultra-purification, nitrogen control, and inclusion modification. If the above-mentioned traditional smelting methods are used, defects such as uneven composition, excessive inclusions, and unqualified high-temperature creep strength will occur, making them completely unsuitable for the smelting and production of P92 steel.

[0005] Patent CN115044823B discloses a production process for P92 continuous casting large round billets. It adopts a fixed two-stage secondary cooling water supply, and the nitrogen addition process relies on the addition of nitriding alloys. It does not optimize the nitrogen addition process and slag system in a targeted manner, resulting in problems such as low nitrogen recovery rate and poor adaptability of continuous casting parameters, and it cannot meet the quality control requirements under different casting speeds.

[0006] Patent CN121610618A discloses a negative pressure bottom blowing nitrogen enhancement process, which requires adding a separate negative pressure bottom blowing nitrogen step after VD treatment, increasing the production cycle and equipment costs. Furthermore, it does not perform synergistic optimization of the refining slag system and continuous casting process, resulting in insufficient economic efficiency and stability of the overall process.

[0007] Patent CN115522115A discloses a process for smelting P92 steel using an argon-oxygen furnace. This process involves a complex route of "electric furnace + induction furnace + argon-oxygen furnace," which has high equipment requirements and is only suitable for production lines of a specific scale. It is difficult to promote and apply this process in ordinary short-process electric furnace production lines.

[0008] In summary, existing technologies cannot simultaneously solve the problems of precise nitrogen control, slag system optimization, continuous casting quality improvement, and process economy. There is an urgent need to develop a P92 steel preparation method that is suitable for short-process electric arc furnaces and achieve stable improvement in product quality through the synergistic optimization of multi-process parameters. Summary of the Invention

[0009] The purpose of this invention is to provide an electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers. By coordinating adjustments to raw material control, slag system optimization, staged nitrogen addition, dynamic water distribution during continuous casting, and slow cooling process, this method solves the problems of unstable nitrogen content control, high nitrogen addition costs, and numerous defects in continuous casting billets in existing technologies. High-quality P92 steel can be stably produced in a conventional electric furnace-LF-VD short-process production line, reducing production costs and meeting the high-performance requirements of steel for ultra-supercritical boilers.

[0010] The technical solution of this invention is as follows: An electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers includes the following steps: (1) Raw material preparation: High-quality, low-impurity scrap steel and pig iron are selected as raw materials.

[0011] The preferred raw material ratio is: 58wt% scrap steel, 32wt% pig iron, and 10wt% high chromium.

[0012] Strict control of impurity elements in raw materials: Ti content in scrap steel ≤ 0.005% to avoid Ti consuming nitrogen and affecting nitrogen enrichment efficiency; harmful element content ≤ 0.01%, Sn content ≤ 0.01%, Pb content ≤ 0.01%, Sb content ≤ 0.01%, Bi content ≤ 0.01%, and the total content of As+Sn+Pb+Sb+Bi ≤ 0.035% to ensure the purity of molten steel.

[0013] Existing conventional P92 smelting processes mostly employ nitriding alloys for nitrogen enrichment, without strict control over the Ti content in scrap steel; generally, ≤0.01% is acceptable. This invention uses a pure gas-based, staged nitrogen enrichment process. Ti preferentially combines with nitrogen to form TiN hard inclusions, which consumes nitrogen, reducing enrichment efficiency, and degrades high-temperature creep performance. Therefore, the upper limit for Ti content is compressed to 0.005%, in conjunction with the aforementioned nitriding alloy-free nitrogen enrichment route.

[0014] (2) Electric arc furnace steelmaking process: S1, Endpoint Control: The carbon content at the end of the electric furnace tapping process is controlled at 0.02-0.03%, and the phosphorus content is ≤0.004%. The tapping temperature is controlled at 1630-1650℃ to ensure the melting of high-melting-point ferrotungsten while avoiding excessively high temperatures that would reduce the solubility of nitrogen.

[0015] The endpoint carbon content is controlled at 0.02-0.03%, which can effectively avoid excessive carbon during the electric furnace oxidation period, which would lead to a heavy decarburization burden and a rebound in phosphorus content.

[0016] S2. Steel tapping operation: The slag-free tapping process is adopted. Before tapping, bottom blowing argon gas is turned on, and argon gas is blown and stirred throughout the tapping process: when the molten steel is poured to less than 2 / 3 of the ladle, the argon gas flow rate is 500-600 NL / min to strengthen stirring and promote the rapid melting and mixing of high specific gravity alloys; when the steel is poured to more than 2 / 3 of the ladle, the flow rate is adjusted to 200-300 NL / min to reduce stirring and prevent the molten steel from churning and oxidizing upon contact with air, thus reducing nitrogen loss.

[0017] S3, Pre-deoxidized alloying: When 1 / 4 of the steel has been tapped, 0.6-1.0 kg / t of aluminum blocks are added with the steel stream. Simultaneously, low-carbon ferrochrome, low-titanium micro-carbon ferrochrome, and metallic manganese are added for preliminary alloying, completing the pre-deoxidation process. After pre-deoxidation, the total oxygen content of the molten steel is controlled at 80-120 ppm.

[0018] At the same time, 4.5-5.0 kg / t of special synthetic slag is added for slag formation; the composition of the special synthetic slag by mass percentage is: CaO content 55-58%, Al2O3 content 30-33%, SiO2 content 4-6%, MgO content 6-8%.

[0019] The conventional amount of pre-deoxidized aluminum added is 1.0-1.5 kg / t. This invention adopts a combination route of low-aluminum pre-deoxidation + LF deep deoxidation to avoid excessive aluminum generating a large amount of Al2O3 cluster inclusions. At the same time, adding aluminum at 1 / 4 of the tapping time can ensure that the aluminum block and the steel flow are fully mixed, and the deoxidation efficiency is improved by more than 15%.

[0020] The low-carbon ferrochrome has a carbon content of 0.13%-0.2%, a chromium content of 55%-59%, P≤0.03%, and S≤0.03%.

[0021] The aforementioned low-titanium micro-carbon ferrochrome has a carbon content of 0.05%-0.08%, a chromium content of 59%-62%, P≤0.03%, and S≤0.03%.

[0022] Depending on the steel output, approximately 4 tons of low-carbon ferrochrome, approximately 8 tons of low-titanium micro-carbon ferrochrome, and approximately 0.16 tons of metallic manganese are added.

[0023] (3) LF refining process: S1. Optimize slag system control: After the molten steel enters the station, 7.5-8.0 kg / t of lime is added. The lime is added to adjust the slag system parameters, controlling the CaO / Al2O3 ratio of the slag to 1.8-1.9 and the basicity R to 4.0-5.0, so as to quickly form white slag, which is maintained for ≥20 minutes.

[0024] The CaO / Al₂O₃ ratio of conventional electric arc furnace slag is typically 2.0-2.5. The special slag described in this invention has a CaO / Al₂O₃ ratio controlled within the range of 1.8-1.9, placing it in the low-melting-point region of the calcium aluminate slag system. This slag system possesses excellent reducing properties and low viscosity, enabling it to efficiently adsorb inclusions and promote nitrogen absorption by the molten steel. The slag viscosity remains stable at 0.25-0.35 Pa at 1600℃. The viscosity of conventional P92 refining slag is 0.4-0.6 Pa. Compared to conventional slag systems, the viscosity is reduced by more than 30%, which can quickly form slag to adsorb deoxidation products, reduce the slag-steel interfacial tension, improve the nitrogen absorption efficiency of subsequent LF processes, and increase the flotation speed of inclusions by 40%.

[0025] S2, Deoxygenation Procedure: A composite deoxidizer composed of ferrosilicon powder and silicon carbide is used for diffusion deoxidation; wherein the mass ratio of ferrosilicon powder to silicon carbide is (3~4):1, and the total amount of ferrosilicon powder added is 1.5~2.2kg / t; Furthermore, the composite deoxidizer is added in 4-6 batches, with an interval of 8-10 minutes between each batch. The amount added in each batch is 1 / 6 to 1 / 4 of the total amount added. The reducing atmosphere of the slag is maintained throughout the process to avoid local SiO2 exceeding the standard and alkalinity fluctuations in the slag system due to a one-time addition.

[0026] S3, Alloy addition sequence: First, ferromolybdenum is added for pre-alloying. When the temperature of the molten steel rises to above 1630℃, ferrotungsten is added in batches to ensure that the high-melting-point ferrotungsten is fully melted. Subsequently, ferrovanadium and ferroniobium were added to complete the microalloying process; Finally, ferroboron is added to adjust the boron content of the molten steel to 0.001-0.003 wt%, which strengthens the grain boundary properties while avoiding hot brittleness caused by excessive boron.

[0027] This sequence ensures that nitride-forming elements such as V and Nb dissolve completely before nitrogen addition, which can effectively improve the solubility of nitrogen.

[0028] The timing for adding ferrotungsten is when the temperature of the molten steel is ≥1630℃. If the temperature of the molten steel is below 1630℃, the melting rate of ferrotungsten decreases by more than 60%, and it is easy to deposit at the bottom of the ladle, causing component segregation. The temperature threshold for adding ferrotungsten as described in this invention can avoid the above problems.

[0029] Furthermore, ferrotungsten is added in batches, at a rate of 1.75% of the finished tungsten content, with a total ferrotungsten content of 26-28 kg / t. It is added in 3 batches, with each batch containing 1 / 3 of the total ferrotungsten content and an interval of 10 minutes between each batch.

[0030] Furthermore, the vanadium content of the ferrovanadium is ≥50wt%, and the amount of ferrovanadium added is based on the minimum vanadium content of 0.20% in the finished product. The amount of ferrovanadium added per ton of steel is 2.0-2.5kg.

[0031] Furthermore, the niobium content of the ferroniobium is ≥60%, and the amount of ferroniobium added is based on the minimum niobium content of 0.065% in the finished product. The amount of ferroniobium added per ton of steel is 1.0-1.2 kg.

[0032] S4. Pre-nitrogen enrichment treatment: After alloying, the temperature of the molten steel is adjusted to 1630-1660℃, the bottom blowing gas is switched to nitrogen, the nitrogen flow rate is controlled at 30-50 NL / min, and the nitrogen blowing time is 15-20min to complete the pre-nitrogen increase and raise the nitrogen content of the molten steel to 80-85% of the target value.

[0033] Within the aforementioned pre-nitrogenation temperature range, the solubility of nitrogen in the steel can reach over 0.08%, while the slag fluidity is optimal and the nitrogen addition efficiency is highest. When the temperature exceeds 1660℃, the nitrogen solubility decreases, and when it is below 1630℃, the slag viscosity increases and the nitrogen mass transfer efficiency decreases.

[0034] (4) VD vacuum treatment process: S1. Vacuum controlled nitrogen retention treatment: Before the molten steel enters the VD furnace, slag is removed. After removing 300-500 kg of slag, the ladle is placed into the VD furnace.

[0035] First, evacuate to 200-300 Pa and maintain for 8-10 minutes. At this vacuum level, the hydrogen partial pressure is extremely low, which can effectively remove more than 70% of the hydrogen in the molten steel. At the same time, the nitrogen partial pressure is higher than the equilibrium nitrogen partial pressure of the molten steel, so almost no nitrogen will be precipitated, thus achieving synergistic dehydrogenation and nitrogen retention.

[0036] Subsequently, the vacuum level was reduced to ≤67Pa and maintained for 20 minutes to remove oxygen and residual hydrogen under deep vacuum, with only a small amount of nitrogen precipitated, ensuring purity while reducing the amount of subsequent fine-tuning.

[0037] S2, Nitrogen Enhancement Fine-tuning: Under the low vacuum conditions formed by S1, argon is blown for 10 minutes at an argon flow rate of 70-80 L / min.

[0038] After 10 minutes, switch from argon to nitrogen, using bypass mode for nitrogen blowing, with the pressure controlled at 0.8-1.0 MPa and the blowing time at 11-13 minutes.

[0039] After venting, switch to bottom blowing argon, control the flow rate at 10-40 NL / min, and blow argon for 20-25 minutes to finally stabilize the nitrogen content at 0.052-0.060%.

[0040] Existing technologies mostly employ LF nitriding alloy nitrogen enrichment or VD followed by separate bottom blowing nitrogen enrichment. The nitrogen yield of the LF nitriding alloy nitrogen enrichment process fluctuates greatly and the alloy cost is high; the VD followed by separate bottom blowing nitrogen enrichment process has low nitrogen enrichment efficiency and poor uniformity.

[0041] The nitrogen-enhancing fine-tuning process described in this invention adopts a high-pressure nitrogen blowing process with a VD pre-vacuum bypass mode. By utilizing the strong stirring effect of molten steel under vacuum, nitrogen elements are rapidly and uniformly dissolved. After the vacuum is broken, soft stirring further homogenizes the mixture, resulting in a final nitrogen content fluctuation of ≤0.005%. No nitriding alloys are required throughout the process, and the cost of nitrogen enhancement per ton of steel is only about 3 yuan, which is far lower than the 25 yuan / ton cost of nitrogen enhancement with nitriding alloys.

[0042] (5) Continuous casting process: S1, Protective casting: Argon gas is used for the entire casting process, and long gates and immersion gates are used for sealing to prevent secondary oxidation of the molten steel.

[0043] Casting parameters: control the superheat of molten steel in the tundish to 25-30℃, and control the casting speed of φ500 cross section billet to 0.37-0.40m / min.

[0044] The tundish uses a double-layer covering agent for insulation and adsorption of inclusions. The lower layer of the tundish uses a low-titanium alkaline tundish covering agent. The TiO2 content of this low-titanium alkaline tundish covering agent is ≤0.05%. Its chemical composition is: CaO content is 45-50wt%, SiO2 ≤10%, Al2O3 content is 30-35wt%, MgO content is 5-8wt%, and the melting point is 1350-1400℃. It has a strong ability to adsorb inclusions.

[0045] The upper layer of the intermediate liner uses a low-titanium hollow particle intermediate liner covering agent; the TiO2 content of this low-titanium hollow particle intermediate liner covering agent is ≤0.05%; its chemical composition is: CaO content 30-35%, SiO2 content 40-45%, Al2O3 content 10-15%, and bulk density 0.6-0.8 g / cm³. 3 Thermal conductivity ≤0.1W / (m K) has excellent thermal insulation properties, preventing the formation of a crust on the surface of molten steel.

[0046] S2, Dynamic Secondary Cooling Water Distribution: A dynamic water distribution mode is adopted, with the total specific water volume controlled at 0.1-0.12L / kg; the water volume proportions of each section are as follows: foot roller section 25%, cooling zone 1 35%, cooling zone 2 25%, and cooling zone 3 15%. The system adjusts the water volume in real time according to the casting speed. For every 0.01 m / min increase in casting speed, the water volume increases by 0.01 L / kg to ensure a stable surface temperature of the billet without temperature rebound, effectively reducing thermal stress.

[0047] S3. Segmented electromagnetic stirring: A two-stage electromagnetic stirring system is used, with the following parameters: Electromagnetic stirring in the crystallizer: current 300A, frequency 1.2Hz, to refine the surface grains; End electromagnetic stirring: current 1000A, frequency 7Hz.

[0048] The crystallizer electromagnetic stirring of the present invention uses a low frequency of 1.2Hz and a high current of 300A in synergy: to reduce the fluctuation of the meniscus liquid surface, avoid slag entrapment, and at the same time enhance the convection of the surface molten steel and refine equiaxed crystals.

[0049] The end electromagnetic stirring uses a high frequency of 7Hz and a high current of 1000A to work together, which is suitable for the solidification end depth of a φ500mm large cross section, strengthens the flow of molten steel in the central area, breaks up columnar crystals, and reduces central segregation and porosity.

[0050] (6) Slow cooling annealing process: After the continuous casting billet is cut, it is hot-sent into the temperature-controlled slow cooling pit, and the furnace charging temperature is ≥600℃; The slow cooling process shall be carried out according to the following procedures: Heating stage: 600-800℃ brittle range, heating rate ≤60℃ / h, to avoid excessive thermal stress and cracks; Incubation stage: After heating to 800±10℃, keep warm for 40-48h to promote tissue homogenization and nitride precipitation; Cooling stage: After cooling to 450℃ in the pit, it is cooled to 180℃ at a rate of ≤30℃ / h, and then removed from the pit and air-cooled.

[0051] The beneficial effects of the present invention are as follows: The electric furnace-continuous casting preparation method of P92 heat-resistant steel for ultra-supercritical high-pressure boilers described in the present invention has innovatively designed the slag system control, nitrogen addition process and cooling, stirring and pressing process parameters of the continuous casting process in the steelmaking process. In particular, it adopts a three-stage nitrogen addition method of LF pre-nitrogen addition + VD vacuum control nitrogen preservation + VD pre-vacuum fine adjustment.

[0052] Compared with existing technologies, the specific advantages are as follows: 1. High nitrogen control precision and significantly improved yield: Through optimized reducing slag system, V / Nb pre-alloying, and a staged nitrogen enhancement process of "LF pre-nitrogen enhancement + VD vacuum nitrogen preservation + vacuum fine-tuning", the nitrogen yield is increased to over 85%, and the nitrogen content fluctuation is controlled within ≤0.005%, achieving precise control within a narrow range and solving the problem of unstable nitrogen content in traditional processes.

[0053] 2. Improved refining efficiency and high steel purity: The special refining slag system developed for P92 steel has a CaO / Al2O3 ratio of 1.8-1.9 and a basicity R of 4.0-5.0. It has excellent deoxidation and desulfurization capabilities, which can control the S content in the steel to ≤0.003%, the O content to ≤15ppm, and the inclusions of types A, B, C, and D to ≤1.0 grade, and inclusions of type DS to ≤0.5 grade, thus significantly improving the purity of the molten steel.

[0054] The above inclusion classification follows GB / T10561-2005 "Standard Rating Chart Microscopic Examination Method for Determination of Non-metallic Inclusion Content in Steel", where Class A is sulfide inclusions, Class B is alumina inclusions, Class C is silicate inclusions, Class D is spherical oxide inclusions, and Class DS is single-particle spherical inclusions.

[0055] 3. Excellent quality of continuously cast billets: The synergistic effect of dynamic secondary cooling water distribution and optimized segmented electromagnetic stirring effectively solves the problem of hot cracking sensitivity of P92 steel. The central porosity of the continuously cast billet is ≤1.5 grade, the shrinkage cavity is ≤1.5 grade, and the central crack is ≤2.0 grade, which fully meets the quality requirements of steel for ultra-supercritical boilers.

[0056] 4. Strong process adaptability and low cost: This invention does not require additional special equipment and can be realized in a normal "electric furnace + LF + VD" short process production line. Compared with other methods that add nitrogen by adding equipment, the production cost is reduced by 22 yuan / ton, which has good promotion and application value.

[0057] 5. Optimized slow cooling process for stable microstructure and properties: The slow cooling process optimized for the brittle range of P92 steel effectively reduces thermal stress, promotes uniform precipitation of nitrides, and significantly improves performance stability. Attached Figure Description

[0058] Figure 1 This is a flow chart of the annealing process for ultra-supercritical P92 heat-resistant steel in this invention.

[0059] Figure 2 The images show a comparison of the low-magnification microstructure of the billets of Example 1 and Comparative Example 1; the left side shows the low-magnification morphology of the billet of Comparative Example 1, and the right side shows the low-magnification morphology of the billet of Example 1. Detailed Implementation

[0060] The technical solution of the present invention will be described in detail below.

[0061] Example 1 In this embodiment, a 100t electric arc furnace is used for smelting to produce P92 heat-resistant steel billets with a cross-sectional specification of φ500mm.

[0062] The electric furnace-continuous casting preparation method for P92 heat-resistant steel for ultra-supercritical high-pressure boilers comprises the following specific steps: (1) Raw material preparation: High-quality, low-impurity scrap steel and pig iron are selected as raw materials, and the iron-to-water ratio is controlled at 32%. The raw material ratio is: scrap steel 58wt%, pig iron 32wt%, and high chromium 10wt%.

[0063] Strict control of impurities in raw materials: Ti content in scrap steel is 0.003%; harmful elements As content is 0.008%, Sn content is 0.007%, Pb content is 0.004%, Sb content is 0.005%, and Bi content is 0.002%, and the total content of As+Sn+Pb+Sb+Bi is 0.026%, ensuring the purity of molten steel.

[0064] (2) Electric arc furnace steelmaking process: S1, Endpoint Control: The final carbon content of the electric arc furnace steel is controlled at 0.025%, the phosphorus content at 0.003%, and the tapping temperature is controlled at 1640℃. The final carbon content is controlled at 0.02%.

[0065] S2. Steel tapping operation: The slag-free tapping process is adopted. Before tapping, bottom blowing argon gas is turned on, and argon gas is blown and stirred throughout the tapping process: when the molten steel is poured to less than 2 / 3 of the ladle, the argon gas flow rate is 550NL / min to promote alloy melting; when the molten steel is poured to more than 2 / 3 of the ladle, the argon gas flow rate is adjusted to 250NL / min to avoid turbulence and oxidation of the molten steel.

[0066] S3, Pre-deoxidized alloying: When 1 / 4 of the steel has been tapped, 0.8 kg / t of aluminum blocks are added with the steel stream, along with low-carbon ferrochrome, low-titanium micro-carbon ferrochrome, and metallic manganese for preliminary alloying, completing the pre-deoxidation process. After pre-deoxidation, the total oxygen content of the molten steel is controlled at 80 ppm.

[0067] At the same time, 4.8 kg / t of special synthetic slag is added for slag formation; the composition of the special synthetic slag by mass percentage is: CaO content 56.5%, Al2O3 content 31.5%, SiO2 content 5%, and MgO content 7%.

[0068] (3) LF refining process: S1. Optimize slag system control: After the molten steel enters the station, 7.8 kg / t of lime is added. The lime is added to adjust the slag system parameters, controlling the CaO / Al2O3 ratio of the slag to 1.88 and the basicity R to 4.2, so as to quickly form white slag, and the white slag is maintained for ≥20 min.

[0069] S2, Deoxygenation Procedure: A composite deoxidizer consisting of 1.8 kg / t ferrosilicon powder and 0.5 kg / t silicon carbide was used for diffusion deoxidation. The composite deoxidizer was added in 5 batches with an interval of 9 minutes between each batch. The amount added in each batch was 1 / 5 of the total amount added. The reducing atmosphere of the slag was maintained throughout the process.

[0070] S3, Alloy addition sequence: After the ferromolybdenum pre-alloying is completed, wait for the temperature of the molten steel to rise to 1640℃, then add ferrotungsten in 3 batches, 9 kg / t per batch, with an interval of 10 min.

[0071] Subsequently, ferrovanadium and ferroniobium were added to complete the microalloying process. The amount of ferrovanadium added was 2.2 kg / t, and the amount of ferroniobium added was 1.1 kg / t.

[0072] Finally, ferroboron is added to adjust the boron content of the molten steel to 0.002%.

[0073] S4. Pre-nitrogen enrichment treatment: After alloying, the temperature of the molten steel was adjusted to 1645℃, the bottom blowing gas was switched to nitrogen, the nitrogen flow rate was controlled at 40NL / min, and the nitrogen blowing time was 18min to complete the pre-nitrogen increase and pre-control the initial nitrogen content of the molten steel to 280ppm, ensuring the purity of the molten steel and laying the foundation for subsequent nitrogen control.

[0074] (4) VD vacuum treatment process: S1. Vacuum controlled nitrogen retention treatment: Before the molten steel enters the VD furnace, slag is removed. After removing 400 kg of slag, the ladle is placed into the VD furnace.

[0075] First, evacuate to 215 Pa and maintain for 9 minutes. This vacuum level can effectively remove hydrogen from the molten steel while avoiding the large-scale precipitation of nitrogen.

[0076] Subsequently, the vacuum level was reduced to 60 Pa and maintained for 20 minutes to further remove oxygen and a small amount of nitrogen, ensuring the purity of the molten steel.

[0077] S2, Nitrogen Enhancement Fine-tuning: Under the low vacuum conditions created by S1, argon is blown for 10 minutes at an argon flow rate of 75 L / min.

[0078] After 10 minutes, switch from argon to nitrogen, using bypass mode for nitrogen blowing, with the pressure controlled at 0.9 MPa and the blowing time at 12 minutes.

[0079] After venting, switch to bottom blowing argon gas, control the flow rate at 25 NL / min, and blow argon for 22 minutes to finally stabilize the nitrogen content at 0.056%.

[0080] No nitriding alloys were added throughout the process; precise nitrogen enrichment was achieved through a three-stage pure gas process.

[0081] (5) Continuous casting process: S1, Protective casting: Argon gas is used for the entire casting process, and long gates and immersion gates are used for sealing to prevent secondary oxidation of the molten steel.

[0082] Casting parameters: control the superheat of molten steel in the tundish to 25℃, and control the casting speed of φ500 cross section billet to 0.38m / min.

[0083] The intermediate tundish uses a double-layer covering agent for insulation and to absorb impurities. The lower layer uses a low-titanium alkaline intermediate tundish covering agent, and the upper layer uses a low-titanium hollow particle intermediate tundish covering agent.

[0084] The low-titanium alkaline intermediate coating agent has TiO2 ≤ 0.05%; its chemical composition is: CaO content 50wt%, SiO2 ≤ 10%, Al2O3 content 35wt%, MgO content 8wt%, and melting point 1400℃.

[0085] The TiO2 content of the covering agent in the low-titanium hollow particles is ≤0.05%; its chemical composition is: CaO content 30%, SiO2 content 40%, Al2O3 content 10%, and bulk density 0.6 g / cm³. 3 Thermal conductivity ≤0.1W / (m K).

[0086] S2, Dynamic Secondary Cooling Water Distribution: A dynamic water distribution model is adopted, with the total specific water volume controlled at 0.10L / kg; the water volume proportions of each section are as follows: foot roller section 25%, cooling zone 1 35%, cooling zone 2 25%, and cooling zone 3 15%. The system adjusts the water volume in real time according to the casting speed. For every 0.01 m / min change in casting speed, the water volume is adjusted by 0.01 L / kg to ensure a stable surface temperature of the billet without temperature rebound, effectively reducing thermal stress.

[0087] S3. Segmented electromagnetic stirring: A two-stage electromagnetic stirring system is used, with the following parameters: Electromagnetic stirring in the crystallizer: current 300A, frequency 1.2Hz, to refine the surface grains; End electromagnetic stirring: current 1000A, frequency 7Hz.

[0088] Electromagnetic stirring is used throughout the entire process, including in the crystallizer and at the end of the casting process. The stirring parameters are optimized in conjunction with the solidification process to effectively improve the solidification segregation and porosity defects of the casting.

[0089] (6) Slow cooling annealing process: After the continuously cast billet is cut, it is hot-loaded into a temperature-controlled slow cooling pit. The furnace temperature is 615℃, and it is continuously sealed and slowly cooled for 72 hours to eliminate internal structural stress and thermal stress of the billet and avoid the generation of low-temperature cracks.

[0090] The slow cooling process shall be carried out according to the following procedures: Heating stage: 600-800℃ brittle range, heating rate 55℃ / h, to avoid excessive thermal stress and cracking; Incubation stage: After heating to 800℃, keep warm for 44 hours to promote tissue homogenization and nitride precipitation; Cooling stage: After cooling to 450°C in the pit, it is cooled to 180°C at a rate of 28°C / h, and then removed from the pit and air-cooled.

[0091] The finished product test results of this embodiment are as follows: the nitrogen content of the molten steel fluctuates within ±22ppm, and the composition uniformity is excellent; the center segregation grade of the billet is 1.0, the center shrinkage cavity is 0.5, and the center crack is 0.5; the equiaxed crystal ratio is 42%; and the comprehensive cost of adding nitrogen per ton of steel is only 3.1 yuan.

[0092] Comparative Example 1 The difference from Example 1 is that in step (3) LF refining process described in this comparative example: S1 slag system optimization control slag CaO / Al2O3=2.3, alkalinity R=3.2.

[0093] The others are the same as in Example 1.

[0094] Finished product test results: LF pre-nitrogenation efficiency decreased by 23%, nitrogen recovery rate was 72%; S content in steel was 0.005%, D-class inclusions were grade 1.5, and purity did not meet the standard.

[0095] Comparative Example 2 The difference from Example 1 is that in step (4) VD vacuum treatment process described in this comparative example: S1 vacuum nitrogen preservation treatment adopts constant 60Pa vacuum treatment for 29min.

[0096] Finished product test results: After VD, the nitrogen content decreased by 41%, and after final fine-tuning, the nitrogen content fluctuated by ±58ppm, with a deviation exceeding 0.005%, which could not meet the narrow range control requirements; the hydrogen content was not significantly different from that in Example 1.

[0097] Comparative Example 3 The difference from Example 1 is that in step (4) of this comparative example, the VD vacuum treatment process is as follows: after VD venting is used in the nitrogen fine-tuning of S2, the bottom blowing nitrogen is fine-tuned with a flow rate of 100NL / min and nitrogen blowing for 20min.

[0098] Finished product testing results: The uniformity of nitrogen content in the molten steel was poor, with a nitrogen content deviation of 0.012% between the upper and lower parts of the same furnace, failing to meet the requirements for narrow-range control. The nitrogen recovery rate was only 65%, and the cost of adding nitrogen increased to 12 yuan / ton.

[0099] Comparative Example 4 The difference from Example 1 is that in step (5) of the continuous casting process described in this comparative example, the static water distribution mode with a fixed specific water volume of 0.10 L / kg is adopted in the dynamic secondary cooling water distribution of S2.

[0100] Finished product inspection results: The maximum temperature difference on the surface of the billet was 120℃ when the casting speed fluctuated, and there was a significant temperature rebound; the central crack of the billet was grade 2.0, and surface cracks appeared, which did not meet the quality requirements.

[0101] Comparative Example 5 The difference from Example 1 is that in step (5) of the continuous casting process described in this comparative example: the S3 segmented electromagnetic stirring uses crystallizer electromagnetic stirring: current 250A, frequency 2.5Hz; end electromagnetic stirring: current 400A, frequency 1.2Hz.

[0102] Finished product inspection results: The center of the billet showed segregation grade 2.0, the center was porous grade 1.5, columnar crystals were well developed, and the equiaxed crystal ratio was only 28% (the equiaxed crystal ratio in Example 1 was 42%).

Claims

1. A method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers by electric furnace-continuous casting, characterized in that, Includes the following steps: (1) Raw material preparation: Low-impurity scrap steel and pig iron are selected as raw materials; The scrap steel contains Ti content ≤ 0.005%; As content ≤ 0.01%, Sn content ≤ 0.01%, Pb content ≤ 0.01%, Sb content ≤ 0.01%, Bi content ≤ 0.01%, and the total content of As+Sn+Pb+Sb+Bi ≤ 0.035%. (2) Electric arc furnace steelmaking process: S1, Endpoint Control: The carbon content at the end of the electric arc furnace tapping process should be controlled at 0.02-0.03%, the phosphorus content at ≤0.004%, and the tapping temperature at 1630-1650℃. S2. Steel tapping operation: Before tapping, start the bottom blowing argon gas and stir with argon gas throughout the tapping process; when the molten steel is poured to less than 2 / 3 of the ladle, the argon gas flow rate is 500-600 NL / min; when the molten steel is poured to more than 2 / 3 of the ladle, adjust it to 200-300 NL / min. S3, Pre-deoxidized alloying: When 1 / 4 of the steel is tapped, 0.6-1.0 kg / t of aluminum blocks are added with the steel stream, along with low-carbon ferrochrome, low-titanium micro-carbon ferrochrome, and metallic manganese for preliminary alloying to complete pre-deoxidation; after pre-deoxidation, the total oxygen content of the molten steel is controlled at 80-120 ppm. Simultaneously, 4.5-5.0 kg / t of special synthetic slag is added for slag formation; the composition of the special synthetic slag, by mass percentage, is: CaO content 55-58%, Al2O3 content 30-33%, SiO2 content 4-6%, MgO content 6-8%; (3) LF refining process: S1. Optimize slag system control: After the molten steel enters the station, 7.5-8.0 kg / t of lime is added; Add lime to adjust the slag system parameters, controlling the CaO / Al2O3 ratio of the slag to be 1.8-1.9 and the alkalinity R to be 4.0-5.0; S2, Deoxygenation Procedure: A composite deoxidizer composed of ferrosilicon powder and silicon carbide is used for diffusion deoxidation; wherein the mass ratio of ferrosilicon powder to silicon carbide is (3~4):1, and the total amount of ferrosilicon powder added is 1.5~2.2kg / t; S3, Alloy addition sequence: First, ferromolybdenum is added for pre-alloying. When the temperature of the molten steel rises to above 1630°C, ferrotungsten is added in batches. Subsequently, ferrovanadium and ferroniobium were added to complete the microalloying process; Finally, ferroboron is added to adjust the boron content of the molten steel to 0.001-0.003 wt%. S4. Pre-nitrogen enrichment treatment: After alloying, adjust the temperature of the molten steel to 1630-1660℃, switch the bottom blowing gas to nitrogen, control the nitrogen flow rate to 30-50 NL / min, and the nitrogen blowing time to 15-20 min to complete the pre-nitrogen addition. (4) VD vacuum treatment process: S1. Vacuum controlled nitrogen retention treatment: Before the molten steel enters the VD furnace, slag is removed. After removing 300-500 kg of slag, the ladle is placed into the VD furnace. First, evacuate to 200-300 Pa and maintain for 8-10 minutes; Then, reduce the vacuum level to ≤67Pa and maintain it for 20 minutes; S2, Nitrogen fine-tuning: Under the low vacuum conditions formed in S1, maintain argon blowing for 10 minutes, with an argon flow rate of 70-80 L / min; After 10 minutes, switch from argon to nitrogen, using bypass mode for nitrogen blowing, with the pressure controlled at 0.8-1.0 MPa and the blowing time at 11-13 minutes; After venting, switch to bottom-blowing argon gas, control the flow rate at 10-40 NL / min, and blow argon for 20-25 minutes, ultimately stabilizing the nitrogen content at 0.052-0.060%. (5) Continuous casting process: S1, Protective casting: Argon gas protection was used throughout the casting process; the superheat of the molten steel in the tundish was controlled at 25-30℃. The tundish uses a double-layer covering agent for insulation and adsorption of inclusions. The lower layer of the tundish uses a low-titanium alkaline tundish covering agent. The TiO2 content of this low-titanium alkaline tundish covering agent is ≤0.05%. Its chemical composition is: CaO content is 45-50wt%, SiO2 ≤10%, Al2O3 content is 30-35wt%, MgO content is 5-8wt%, and melting point is 1350-1400℃. The upper layer of the intermediate liner uses a low-titanium hollow particle intermediate liner covering agent; the TiO2 content of this low-titanium hollow particle intermediate liner covering agent is ≤0.05%; its chemical composition is: CaO content 30-35%, SiO2 content 40-45%, Al2O3 content 10-15%, and bulk density 0.6-0.8 g / cm³. 3 Thermal conductivity ≤0.1W / (m K); S2, Dynamic Secondary Cooling Water Distribution: A dynamic water distribution mode is adopted, with the total specific water volume controlled at 0.1-0.12L / kg; the water volume proportions of each section are as follows: foot roller section 25%, cooling zone 1 35%, cooling zone 2 25%, and cooling zone 3 15%. The water volume is adjusted in real time according to the pulling speed. For every 0.01m / min increase in pulling speed, the water volume increases by 0.01L / kg. S3. Segmented electromagnetic stirring: A two-stage electromagnetic stirring system is used, with the following parameters: Electromagnetic stirring in the crystallizer: current 300A, frequency 1.2Hz; End-efficiency electromagnetic stirring: current 1000A, frequency 7Hz; (6) Slow cooling annealing process: After the continuous casting billet is cut, it is hot-sent into the temperature-controlled slow cooling pit, and the furnace charging temperature is ≥600℃; The slow cooling process shall be carried out according to the following procedures: Heating stage: 600-800℃ brittle range, heating rate ≤60℃ / h; Insulation stage: After heating to 800±10℃, keep warm for 40-48 hours; Cooling stage: After cooling to 450℃ in the pit, it is cooled to 180℃ at a rate of ≤30℃ / h, and then removed from the pit and air-cooled.

2. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, The specific ratio of raw materials in step (1) is: 58wt% scrap steel, 32wt% pig iron, and 10wt% high chromium.

3. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, The low-carbon ferrochrome in step (2) has a carbon content of 0.13%-0.2%, a chromium content of 55%-59%, and P≤0.03% and S≤0.03%.

4. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, The low-titanium micro-carbon ferrochrome in step (2) has a carbon content of 0.05%-0.08%, a chromium content of 59%-62%, and P≤0.03% and S≤0.03%.

5. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, In step (3) S2, the composite deoxidizer is added in 4-6 batches, with an interval of 8-10 minutes between each batch, and the amount added in each batch is 1 / 6 to 1 / 4 of the total amount added.

6. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, In step (3) S3, the total amount of ferrotungsten added is 26-28 kg / t, added in 3 batches, with each batch adding 1 / 3 of the total amount of ferrotungsten, and each batch being 10 min apart.

7. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, In step (3) S3, the vanadium content of the ferrovanadium is ≥50wt%; the amount of ferrovanadium added per ton of steel is 2.0-2.5kg.

8. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, In step (3) S3, the niobium content of the ferro-niobium is ≥60%; the amount of ferro-niobium added per ton of steel is 1.0-1.2 kg.

9. The electric furnace-continuous casting method for preparing P92 heat-resistant steel for ultra-supercritical high-pressure boilers according to claim 1, characterized in that, In step (5), the casting speed of the φ500 section billet in S1 is controlled at 0.37-0.40 m / min.

Citation Information

Patent Citations

  • Negative-pressure bottom-blowing nitrogen increasing process method for P92 heat-resistant steel

    CN121610618A