A method for controlling nitrogen and oxygen content in 700MPa high-strength container steel
By using materials such as magnetic separation powder, limestone, and CaC2, as well as argon protection, in the converter smelting, LF refining, and continuous casting processes, the problem of controlling nitrogen content in high-strength container steel was solved, and the mechanical properties of the steel plate were improved.
Patent Information
- Application Number
- CN202611373235.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot effectively control the nitrogen content in 700MPa high-strength container steel, leading to the formation of titanium nitride inclusions and affecting the mechanical properties of the steel plate.
In the converter smelting and LF refining processes, materials such as magnetic separation powder, limestone, and CaC2 are added, combined with bottom blowing argon and nitrogen protection, to form a slag layer and a slightly positive pressure environment, reducing the contact between molten steel and air and controlling the nitrogen content; in the continuous casting process, protective sleeves and argon protection are used to reduce the amount of nitrogen added to the molten steel.
It effectively reduces the nitrogen content in molten steel, reduces titanium nitride inclusions, improves the yield strength, tensile strength and elongation after fracture of steel plates, and ensures the stability of steel plate performance.
Smart Images

Figure REF-OBJ-1788396668505-000001 
Figure REF-OBJ-1788396668505-000002 
Figure REF-OBJ-1788396668505-000003
Abstract
Description
Technical Field
[0001] This invention belongs to the field of steelmaking technology, and specifically relates to a method for controlling the nitrogen and oxygen content of 700MPa grade high-strength container steel. Background Technology
[0002] Container steel is a low-alloy corrosion-resistant steel, with a focus on atmospheric corrosion resistance. Container plates with a yield strength greater than 700 MPa require high strength while also demanding good formability, corrosion resistance, and weldability. It is the highest strength and most technically challenging product in its class. The chemical composition design adopts a low-carbon, high-manganese approach, adding alloying elements such as niobium and titanium to achieve precipitation strengthening and grain refinement. The use of composite microalloying technology with multiple alloying elements such as molybdenum, niobium, vanadium, and titanium results in complex production process control, low yield, and high cost. Adding titanium separately to improve the strength of steel plates can significantly reduce production costs. During production, the nitrogen content of the finished product ranges from a minimum of 0.0030% to a maximum of over 0.0060%, with an average of 0.0043%. Nitrogen in steel has a strong affinity for titanium, resulting in titanium nitride inclusions of varying sizes. Larger titanium nitride inclusions neither prevent austenite grain growth nor provide precipitation strengthening; instead, they reduce the grain refinement and precipitation strengthening effects of titanium-carbon bonding. High nitrogen content in steel affects grain refinement, causing fluctuations in steel plate performance, reducing yield strength, tensile strength, and elongation after fracture, thus impacting its usability.
[0003] Chinese patent document (application number 202510832856.3) discloses "a smelting method for controlling nitrogen content in aluminum-killed steel through a whole-process smelting process", including the following steps: (1) when tapping iron from the blast furnace, scrap steel is added to the molten iron ladle in advance, with the amount of molten iron added at 725-735 kg / t of steel; (2) the amount of scrap steel added to the converter is calculated at 245-260 kg / t of steel, and inferior scrap steel that is prone to increasing nitrogen is not used; (3) the converter smelting adopts the bottom blowing argon mode throughout the process, and the high lance position blowing mode quickly forms a slag layer, and the C and P are both hit at the smelting endpoint; (4) after the converter taps out of the steel furnace, no aluminum-containing deoxidizing material is added for alloying, and the steel is tapped after the alloy and flux have melted evenly; (5) The bottom blowing argon flow rate of the LF refining ladle ensures that the molten steel does not break through the slag surface. Lime and slag refining agent are added, and slag is slag-smelting is performed. After the slag is smelted, diffusion deoxidation is performed. After the white slag is formed, the aluminum is adjusted to the upper limit of the process requirements in one go. Soft blowing argon for ≥5min is performed before hoisting the ladle. (6) The argon seal protection sleeve of the ladle and the immersion nozzle of the tundish are used throughout the continuous casting process. The tundish covering agent is added to reduce the nitrogen absorption of the molten steel during the casting process. The method of this invention is used to smelt aluminum-containing killed steel. The N in the steel is ≤50ppm. The proportion of edge crack defects in the finished steel plate is reduced to below 0.4%, which greatly improves the yield of the finished steel plate. This invention adopts measures to control the increase of nitrogen in the molten steel. Finally, the nitrogen content is controlled at a level not exceeding 0.0050%. For titanium-containing steel, this cannot inhibit the formation of titanium nitride inclusions, and the effect is not ideal.
[0004] Chinese invention patent application (application number 202311275790.X) discloses "a method for controlling the nitrogen content of molten steel," which discloses a method to control the nitrogen content in molten steel and ensure its stability by comprehensively controlling the amount of nitrogen removal or control in the converter smelting, LF refining, and slab continuous casting processes. By improving the converter's denitrification capacity, reducing the amount of nitrogen added in the LF process, and stabilizing the slab continuous casting process, the nitrogen content in the tundish molten steel is controlled to within 60 ppm when the steel consumption is 800 kg / t. However, the final nitrogen content in the molten steel is still not low enough to meet the requirements of steel production and processing. This invention, by controlling the nitrogen addition in molten steel, can control the nitrogen content in the tundish molten steel to within 0.0060%, but it cannot suppress the formation of titanium nitride inclusions by titanium, the element with the strongest binding affinity to nitrogen, which affects the performance of the steel.
[0005] In summary, current technologies cannot achieve extremely low nitrogen content in steel. When producing titanium-containing steels, titanium readily combines with nitrogen to form large titanium nitride inclusions, which fail to provide fine-grain strengthening and precipitation strengthening, thus affecting the mechanical properties of the steel plate. Therefore, there is an urgent need to develop a method to reduce the nitrogen content and oxygen content of high-strength container steel, thereby achieving excellent overall performance for high-strength container steel. Summary of the Invention
[0006] The purpose of this invention is to address the problem of excessively high nitrogen content and low steel plate performance in existing high-strength container steel. This is because titanium and nitrogen combine in the steel to form large titanium nitride inclusions, which neither prevent austenite grain growth nor provide precipitation strengthening, thus reducing the grain refinement and precipitation strengthening effects of titanium-carbon bonding. Therefore, this invention develops a method for controlling the nitrogen and oxygen content of 700MPa grade high-strength container steel, which can reduce the nitrogen content of the finished high-strength container steel at this level, thereby ensuring the stable performance of the steel plate.
[0007] To achieve the above objectives, the present invention employs the following technical solution: A method for controlling nitrogen and oxygen content in 700MPa high-strength container steel involves controlling the scrap ratio of the converter raw materials during converter smelting, adding low-cost magnetic separation powder for rapid slag formation in the early stages, avoiding direct contact between the molten steel and air, thus reducing nitrogen absorption. During the initial silicon-manganese oxidation in the blowing stage, nitrogen is used for bottom blowing; when a violent carbon-oxygen reaction occurs, it is switched to argon for bottom blowing. The blowing process is completed in one pass without spot blowing, and the converter's movable fume hood is lowered to its lowest position during the blowing process. During tapping, silicon-manganese alloy is used for weak deoxidation and alloying to prevent nitrogen absorption from the air. After adding the alloy, limestone is added, utilizing the CO2 released from the decomposition of limestone to further remove nitrogen from the molten steel. The lime generated from the decomposition of limestone creates a slag layer of a certain thickness on the surface of the molten steel, preventing nitrogen absorption from the air. The tapping process ensures a round taphole shape. After the ladle enters the LF refining station, bottom blowing argon is activated, and lime is added for slag formation. A refining slag-forming agent is added based on the slag melting process. During electrode heating, CaC2 is used to form foam slag during refining to prevent the molten steel from absorbing nitrogen from the air. The blower speed is reduced during refining to achieve a slightly positive pressure state inside the furnace cover. After the formation of calcium carbide slag, ferrosilicon and ferromanganese are added to adjust the silicon and manganese content in the steel. Aluminum segments are added to the molten steel for deep deoxidation and alloying, followed by the addition of ferrotitanium for alloying. Refining is completed after a net circulation of 3-5 minutes. Throughout the casting process, a protective sleeve is used below the long nozzle of the ladle, and a sealing cup is used at the interface of the protective sleeve. Argon gas is blown into the tundish stopper rod, slide plate, and submerged entry nozzle for protection to reduce air intake during casting. The continuously cast billet is then heated and rolled to obtain a steel plate of a certain thickness, which is then subjected to performance testing.
[0008] Specifically, the methods and steps are as follows: 1) Converter and tapping: During the converter smelting process, the scrap steel ratio of the raw materials added to the converter is controlled. The scrap steel addition amount is 16% to 18%. Inexpensive magnetic separation powder is added. The particle size of the magnetic separation powder is 0.030 to 0.100 mm. The composition contains: CaO: 30wt% to 35wt%, SiO2: 7wt% to 9wt%, Al2O3: 4wt% to 6wt%, MgO: 4wt% to 6wt%, TFe: 20wt% to 26wt%, MFe: 13wt% to 20wt%, and the remainder is impurities. The magnetic separation powder is added at a rate of 2wt%–4wt% of the total converter steel feed. Containing alumina and ferrous oxide, the powder helps lower the slag's melting point and enhances its oxidizing properties, promoting the carbon-oxygen reaction. It is added along with the scrap steel to fully utilize this low-cost material, enabling rapid slag formation in the early stages and quickly creating a slag layer of a certain thickness on the molten steel surface. This prevents direct contact between the molten steel and air, thus reducing nitrogen absorption. During the initial silicon-manganese oxidation stage of the blowing process, nitrogen is used for bottom blowing. After 4–5 minutes of blowing, when the carbon-oxygen reaction becomes vigorous, the process switches to argon for bottom blowing, with a gas flow rate of 0.08–0.12 Nm³. 3 The CO gas generated by the reaction is equivalent to a vacuum for nitrogen, and can be carried out of the molten steel by the CO gas. The blowing process is completed in one go, without spot blowing, reducing nitrogen absorption. During the blowing process, the converter's movable fume hood is lowered to the lowest position, and the molten pool temperature is controlled at 1570-1590℃ during the smelting process, which is conducive to the vigorous reaction of carbon and oxygen and the removal of nitrogen from the molten steel. During the converter steelmaking process, silicon-manganese alloy is used for weak deoxidation and alloying, retaining 0.015%–0.025% active oxygen in the molten steel. The distribution of oxygen and other active elements on the surface of the molten steel helps prevent nitrogen absorption from the air. After adding the alloy, limestone with a particle size of 2–10 mm is added to the ladle at a rate of 0.3–0.4 kg / t at a rate of 300–400 kg / min. The molten steel mixes with the limestone under gravity. The CO2 released from the decomposition of the limestone further removes nitrogen from the molten steel. Simultaneously, the dissolution of nitrogen in the molten steel is an endothermic reaction; solubility increases with temperature, and conversely, as the temperature of the molten steel decreases during tapping, it facilitates nitrogen removal. Before the end of tapping, the lime produced by the decomposition of the limestone creates a slag layer of a certain thickness on the surface of the molten steel, preventing nitrogen absorption from the air. During tapping, the taphole shape must be kept round to prevent the steel stream from branching and absorbing nitrogen. Argon blowing is initiated at the bottom of the ladle during the tapping process, with an argon flow rate of 200–290 L / min. This further achieves the purpose of denitrification, and the nitrogen content in the molten steel ladle after the converter can be controlled at 0.0010 wt%–0.0015 wt%.
[0009] 2) Refining: After the ladle enters the LF refining station, turn on the bottom blowing argon gas and adjust the flow rate of the bottom blowing argon gas to 1000-1170 L / min. Add lime to form slag, with an addition amount of 1.8-2.8 kg / t. The lime contains ≥90% CaO and has an activity (4N HCl titration method) ≥300. Add refining slag-forming agent according to the slag melting situation, with an addition amount of 0.5-0.7 kg / t. During the electrode heating process, use CaC2 to form foam slag in the refining process to prevent air from being ionized by the electric arc and causing the molten steel to absorb nitrogen. The addition amount of CaC2 is 0.3-0.4 kg / t, added in 2-3 times. During the refining process, the fan speed is reduced by 5%-10% compared with the normal situation to achieve a slightly positive pressure state inside the furnace cover and prevent air from entering the refining furnace. After the formation of carbide slag, ferrosilicon and ferromanganese are added to adjust the silicon and manganese content in the molten steel. Then, aluminum wire segments are added to the molten steel for deep deoxidation and alloying. The argon gas flow rate is controlled at 80-120 L / min. After a net circulation of 3-5 min, ferrotitanium is added for alloying. After another net circulation of 3-5 min, the refining is completed and the steel is removed. The nitrogen content in the molten steel at the end of the refining process is controlled at 0.0015 wt% to 0.0018 wt%.
[0010] 3) Continuous casting: Protective casting is adopted in the continuous casting process. During the casting process, a protective sleeve is used below the long nozzle of the ladle. A sealing cup is used at the interface of the protective sleeve. Argon gas is blown in to protect the tundish stopper rod, slide plate and submersible nozzle to reduce the intake of air during casting. The nitrogen increase of the steel refined to the tundish is ≤0.0002wt%. The chemical composition of the molten steel in the ladle, by mass percentage, is as follows: C: 0.09%~0.10%, Si: 0.20%~0.30%, Mn: 1.4%~1.5%, P≤0.013%, S≤0.0030%, Ti: 0.16%~0.18%, N≤0.0020%, TO: 0.0010%~0.0014%, with the remainder being Fe and unavoidable impurities.
[0011] 4) Rolling and testing: After the continuous casting billet is heated in a heating furnace, it is rolled into steel plates of 2-8mm. Samples of the steel plates are taken for performance testing. The yield strength of the steel plates reaches 780-800MPa, the tensile strength reaches 850-880MPa, and the elongation after fracture reaches 21%-25%.
[0012] Compared with the prior art, the beneficial effects of the present invention are: 1. In the converter smelting process, the present invention adds low-cost magnetic separation powder after steel slag treatment to achieve rapid slag formation in the early stage of blowing, protect the molten steel and reduce nitrogen absorption. At the same time, the high oxidizing power provided by the magnetic separation powder is conducive to the vigorous reaction of carbon and oxygen in the molten steel and promotes the removal of nitrogen from the molten steel.
[0013] 2. During the smelting process, the molten pool is kept at a high temperature, which is conducive to the vigorous reaction of carbon and oxygen and the removal of nitrogen from the molten steel.
[0014] 3. In the process of tapping steel, limestone is added and mixed with molten steel to promote the rapid generation of CO2 from the limestone. Before leaving the molten steel, the CO2 will carry away the nitrogen in the molten steel, further reducing the nitrogen content.
[0015] 4. During the tapping process of the converter, the molten steel undergoes weak deoxidation to retain a certain amount of active oxygen and prevent the molten steel from absorbing nitrogen from the air.
[0016] 5. CaC2 is added during the LF refining process to form foam slag, which prevents air from being ionized by the electric arc and causing the molten steel to absorb nitrogen.
[0017] 6. By controlling the nitrogen content in steel, the number and size of titanium nitride inclusions in the steel are reduced, the grain-refining strengthening effect of titanium carbide is fully utilized, and the yield strength, tensile strength and elongation after fracture of high-strength container steel are improved. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the specific implementation methods of this invention will be further described below in conjunction with the embodiments. The following embodiments are used to specifically illustrate the content of this invention. These embodiments are only general descriptions of the content of this invention and do not limit the content of this invention.
[0019] The relevant process parameters for converter smelting and tapping in the examples and comparative examples are shown in Table 1. The comparative example uses molten iron and scrap steel for smelting, aluminum deoxidation and killing are carried out during tapping, and active lime is added above the ladle in the later stage.
[0020] Table 1. Relevant process parameters for converter smelting and tapping:
[0021] The relevant process parameters for refining in the examples and comparative examples are shown in Table 2. The comparative examples do not use CaC2 for slagging during the refining process.
[0022] Table 2 Relevant process parameters for refining:
[0023] The results of the smelting composition in the examples and comparative examples are shown in Table 3.
[0024] Table 3. Results of smelting composition in the ladle:
[0025] In summary, as can be seen from the table, the nitrogen content in the high-strength container steel produced by this method is controlled at 0.0017%-0.0020%, while the total oxygen content is controlled at 0.0010%-0.0014%. The titanium and carbon are fully combined, which plays a good role in fine grain strengthening, thereby improving the yield strength, tensile strength and elongation after fracture of the steel plate.
[0026] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel, characterized in that, Specifically, the methods and steps are as follows: 1) Converter and tapping: During the converter smelting process, the scrap steel ratio of the raw materials added to the converter is controlled, with the scrap steel addition amount being 16%–18%. Magnetic separation powder is added, with the amount of magnetic separation powder accounting for 22wt%–4wt% of the total amount of steel added to the converter. During the initial blowing of ferrosilicon oxidation, nitrogen is used for bottom blowing, and after 4–5 minutes of blowing, it is switched to argon for bottom blowing, with a gas flow rate of 0.08–0.12 Nm³. 3 / min·t, the blowing process is completed in one hit without spot blowing. During the blowing process, the converter movable hood is lowered to the lowest position. During the smelting process, the molten pool temperature is controlled at 1570~1590℃. During the tapping process in the converter, silicon-manganese alloy is used for weak deoxidation and alloying. 0.015% to 0.025% active oxygen is retained in the molten steel. After the alloy is added, limestone is added to the ladle. Argon is blown into the bottom of the ladle during the tapping process, and the argon flow rate is 200 to 290 L / min. 2) Refining: After the ladle enters the LF refining station, bottom blowing argon is started, and the flow rate of bottom blowing argon is adjusted to 1000-1170 L / min. Lime is added for slag formation, and refining slag-forming agent is added. During electrode heating, CaC2 is used to form foam slag in the refining process. The amount of CaC2 added is 0.3-0.4 kg / t, added in 2-3 times. After the formation of calcium carbide slag, ferrosilicon and ferromanganese are added to adjust the silicon and manganese content in the molten steel. Then, aluminum wire segments are added to the molten steel for deep deoxidation and alloying. The argon blowing flow rate is controlled at 80-120 L / min. After net circulation for 3-5 minutes, ferrotitanium is added for alloying. After another net circulation for 3-5 minutes, the refining is completed and the ladle is unloaded. 3) Continuous casting: The continuous casting process adopts protective casting, and the nitrogen increase of the molten steel from the end of refining to the tundish is ≤0.0002wt%.
2. The method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel according to claim 1, characterized in that, The magnetic separation powder has a particle size of 0.030–0.100 mm and contains the following components: CaO: 30 wt%–35 wt%, SiO2: 7 wt%–9 wt%, Al2O3: 4 wt%–6 wt%, MgO: 4 wt%–6 wt%, TFe: 20 wt%–26 wt%, MFe: 13 wt%–20 wt%, with the remainder being impurities.
3. The method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel according to claim 1, characterized in that, In step 1), the limestone has a particle size of 2-10 mm, an addition amount of 0.3-0.4 kg / t, and an addition rate of 300-400 kg / min.
4. The method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel according to claim 1, characterized in that, The nitrogen content in the molten steel in the ladle after the converter is controlled at 0.0010wt% to 0.0015wt%.
5. The method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel according to claim 1, characterized in that, In step 2), the amount of lime added is 1.8 to 2.8 kg / t, the lime contains ≥90% CaO and has an activity of ≥300, and the amount of refining slag agent added is 0.5 to 0.7 kg / t.
6. The method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel according to claim 1, characterized in that, The nitrogen content in the molten steel after finishing is controlled at 0.0015wt% to 0.0018wt%.
7. The method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel according to claim 1, characterized in that, The chemical composition of the molten steel in the ladle, by mass percentage, is as follows: C: 0.09%~0.10%, Si: 0.20%~0.30%, Mn: 1.4%~1.5%, P≤0.013%, S≤0.0030%, Ti: 0.16%~0.18%, N: ≤0.0020%, TO: 0.0010%~0.0014%, with the remainder being Fe and unavoidable impurities.
8. The method for controlling nitrogen and oxygen content in 700MPa grade high-strength container steel according to claim 1, characterized in that, After being heated in a heating furnace, the continuously cast billet is rolled into a steel plate with a thickness of 2-8 mm. The yield strength of the steel plate is 780-800 MPa, the tensile strength is 850-880 MPa, and the elongation after fracture is 21%-25%.
Citation Information
Patent Citations
Method for controlling nitrogen content of molten steel
CN117126977A
Smelting method for controlling nitrogen content in aluminum-containing killed steel through full-process smelting