A heat-resistant and corrosion-resistant stainless steel and its manufacturing method
By optimizing the chemical composition and processing technology, the problems of high cost and limited thickness range of existing duplex stainless steel have been solved, and the high-temperature mechanical properties and corrosion resistance have been improved, producing heat-resistant and highly corrosion-resistant stainless steel suitable for engineering applications.
Patent Information
- Application Number
- CN202611366443.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing duplex stainless steel products are expensive and have a limited thickness range, which cannot meet the high-temperature mechanical properties and corrosion resistance requirements of engineering applications.
By optimizing the chemical composition design and process, controlling the proportion of alloying elements, and employing forging, segmented rolling, and solution treatment, a reasonable ratio of austenite to ferrite is ensured, the formation of δ-ferrite is suppressed, the quality of the billet is improved, the solid solubility of alloying elements is enhanced, and high-pressure cooling technology is used to form a stable passivation film, restricting harmful impurities, thereby achieving a synergistic improvement in high-temperature mechanical properties and corrosion resistance.
The stainless steel products produced have good room temperature and high temperature mechanical properties and corrosion resistance in the thickness range of 10~80 mm, meeting the actual needs of equipment manufacturing. They have high yield strength, tensile strength and corrosion resistance, and are suitable for high temperature and corrosion environments.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention pertains to ferrous metal materials, and specifically relates to a heat-resistant and highly corrosion-resistant stainless steel and its manufacturing method. Background Technology
[0002] Duplex stainless steel, a special type of stainless steel, exhibits numerous superior properties due to its unique austenitic and ferritic dual-phase microstructure, making it a research hotspot in the materials science field. Duplex stainless steel demonstrates significant advantages in corrosion resistance; compared to austenitic stainless steel, its resistance to chloride pitting and crevice corrosion is particularly outstanding, making it especially suitable for environments with high chloride ion concentrations, such as seawater and some chemical media. In terms of mechanical properties, duplex stainless steel has significantly higher strength than austenitic stainless steel, with a yield strength typically about twice that of austenitic stainless steel, while also possessing good plasticity and toughness. Regarding weldability, compared to austenitic stainless steel, duplex stainless steel has a lower tendency for hot cracking, requiring no preheating during welding and no complex post-weld heat treatment. This effectively improves production efficiency and reduces costs when manufacturing large structural components and complex parts.
[0003] The invention patent CN117265418A, entitled "A Crack-Free Duplex Stainless Steel and Its Preparation", relates to a crack-free duplex stainless steel. The thickness of the cold-rolled steel plate is 1~2 mm, which cannot meet the requirements for use of thick duplex stainless steel products.
[0004] The published invention patent CN119663115A, "A Duplex Stainless Steel Containing Rare Earth Elements and Its Preparation Process", discloses a duplex stainless steel containing rare earth elements and its preparation process. Judging from the disclosed chemical composition, a large amount of rare earth elements needs to be added, resulting in high costs. Furthermore, the patent does not disclose mechanical properties, which cannot meet the design requirements for engineering applications.
[0005] The publicly disclosed invention patent CN118957454A, "A duplex stainless steel plate with strong corrosion resistance and low anisotropy and its manufacturing method," shows that the steel plate is produced using a cold rolling process, based on the disclosed composition, production method, and beneficial effects. This process cannot meet the requirements for hot-rolled medium-thick plates.
[0006] Although the duplex stainless steel products disclosed above improve the performance of duplex stainless steel by adding alloying elements, the products involved are expensive and cover a small range of thicknesses, so they cannot be widely used in engineering. Summary of the Invention
[0007] To meet the performance requirements of design units for heat-resistant and corrosion-resistant stainless steel, this invention provides a heat-resistant and highly corrosion-resistant stainless steel and its manufacturing method. Through optimized design of chemical composition and reasonable matching of forging, hot rolling and heat treatment processes, the steel plate has good mechanical properties and corrosion resistance at room temperature and high temperature, which can effectively serve the actual needs of stainless steel production and equipment manufacturing.
[0008] One of the technical solutions of this invention is to propose a heat-resistant and highly corrosion-resistant stainless steel. The specific technical solution is as follows: the chemical composition by mass percentage is: C: 0.040~0.060%, Si: 1.01~1.65%, Mn: 1.50~1.95%, P≤0.020%, S≤0.010%, Ni: 9.01~14.59%, Cr: 20.50~24.99%, Mo: 4.50~7.00%, Ta: 0.09~0.25%, Nb: 0.15~0.39%, N: 0.10~0.17%, with the remainder being Fe and unavoidable impurities.
[0009] The reasons for selecting the above alloying elements and their contents in this invention are as follows: C: Carbon (C) is a key element affecting the mechanical properties of steel. This invention employs a medium-to-high carbon design. On one hand, based on the high alloying characteristics of this invention, increasing the C content can effectively suppress the formation of δ-ferrite in the finished steel, avoiding segregation under high-temperature service conditions and preventing a decline in mechanical properties. On the other hand, it is necessary to further control the upper limit of the carbon content to prevent C from precipitating in the form of alloy compounds, which would lead to a loss of mechanical properties. Therefore, this invention requires the C content to be controlled between 0.040% and 0.060%.
[0010] Si: For the high-temperature service conditions of the products of this invention, the addition of Si can significantly improve the high-temperature oxidation resistance of steel. However, Si promotes the formation of ferrite, which increases the brittleness of the steel. Therefore, this invention requires the Si content in the steel to be controlled at 1.01~1.65%.
[0011] Mn: Mn remains in steel as a deoxidizing element, and its role is manifested in two aspects: first, it forms MnS compound with sulfur in steel, which can improve the processing performance of steel; second, it produces a solid solution strengthening effect on the matrix, improving the mechanical properties of steel. Considering that excessive Mn content will aggravate component segregation in steel, this invention requires the Mn content to be controlled at 1.50~1.95%.
[0012] Cr and Ni: Ni strengthens the matrix through solid solution and stabilizes the austenite / ferrite ratio, improving oxidation resistance. Cr strengthens the matrix through solid solution and forms carbides, making it the most important element for providing corrosion resistance to stainless steel. Furthermore, controlling the Cr / Ni ratio effectively controls the distribution of austenite in the δ-ferrite matrix during solidification, preventing defects in the billet caused by ferrite dendrite aggregation and insufficient liquid phase feeding. Controlling the Cr / Ni ratio also improves billet and weld quality. Simultaneously, controlling the austenite / ferrite volume fraction ratio to 0.67–1.50 further enhances the steel's mechanical properties. Therefore, the steel of this invention contains 9.01–14.59% Ni and 20.50–24.99% Cr.
[0013] Preferably, the Cr / Ni equivalent ratio σ It should be within the range of 1.70 to 2.35.
[0014] Preferably, the stainless steel microstructure comprises austenite and ferrite, wherein the volume fraction of austenite is 44.5% to 48.5%, and the remainder is ferrite.
[0015] Mo: Mo can form a passivation film on the surface of stainless steel, thereby improving the steel's oxidation resistance. In stainless steel, it enhances the mechanical properties through solid solution strengthening and carbides (such as Mo2C), while also improving the high-temperature stability of ferrite and austenite, inhibiting high-temperature precipitation, and improving the structural stability under high-temperature conditions. However, the Mo content should not exceed 8%, as it easily leads to an imbalance in oxidation. Therefore, this invention requires controlling the Mo content to be between 4.50% and 7.00%.
[0016] Nb and Ta: Nb has a strong affinity for nitrogen in stainless steel, forming NbN compounds, which can effectively improve the stability of nitrogen, thereby reducing denitrification and porosity formation during smelting and heating, and improving the quality of the cast billet. The fine carbonitrides dispersed in the matrix can play a role in second-phase strengthening and grain refinement, significantly improving the mechanical properties of the steel. Simultaneously, Nb has a stronger affinity for carbon than Cr, preferentially combining with C, effectively inhibiting Cr precipitation at grain boundaries, avoiding chromium depletion at grain boundaries, and thus improving the intergranular corrosion resistance of stainless steel. Ta is a group element with Nb, and its role in stainless steel is similar to that of Nb. However, Ta compounds have superior stability under high-temperature corrosion environments. Using partial Ta substitution for Nb not only enables the steel to obtain good high-temperature corrosion resistance but also improves its weldability. Therefore, the Nb content in this invention is 0.15~0.39%, and the Ta content is controlled at 0.09~0.25%.
[0017] Preferably, the contents of Ta, Nb, C, and N satisfy the following relationship: ,in,β It should meet the range of 0.10~0.22.
[0018] P and S: Both P and S are harmful elements that exacerbate the brittleness of steel, worsen its plasticity and toughness, and easily cause hot cracks during hot working, thereby weakening the steel's performance and corrosion resistance. Therefore, this invention controls the P content to below 0.020% and the S content to below 0.010%.
[0019] Nitrogen (N): Nitrogen has a strong austenite-stabilizing effect, significantly improving the corrosion resistance of steel. Simultaneously, it combines with Nb and Ta elements in the steel to form fine, dispersed second-phase particles, which can significantly improve the strength and toughness of the steel. However, excessively high N content can cause defects such as porosity within the steel. Therefore, this invention requires controlling the N content to be between 0.10% and 0.17%.
[0020] Preferably, the stainless steel has a thickness ranging from 10 to 80 mm; the stainless steel possesses good mechanical properties, including a room temperature yield strength in the solution-treated state. R p0.2 ≥625 MPa, tensile strength R m≥800 MPa, elongation A ≥39%; Tensile yield strength at 550 ℃ R p0.2 ≥440 MPa, tensile strength R m≥675 MPa, elongation A ≥33%; the impact resistance of the stainless steel is -40℃ KV 2≥180J; The stainless steel has good corrosion resistance. According to the ASTM G48 standard, the corrosion resistance of the product is tested and the pitting corrosion rate is less than 3 mdd.
[0021] The second technical solution of this invention is to propose a method for manufacturing heat-resistant and corrosion-resistant stainless steel, including a production process of billet forging, rolling and solution treatment, characterized in that: Rolling: The forged steel billet is heated to 1255~1265 ℃, with a total furnace time of 4.5~5.5 h. The initial rolling temperature is 1220~1250 ℃, and the deformation amount of the first pass is 28%~35%. The steel plate is then left to heat up. The initial rolling temperature of the second stage is controlled at 1100~1150 ℃, and the deformation amount of the remaining single passes is 10%~20%. The final rolling temperature is 950~980 ℃.
[0022] Solution treatment: As the final heat treatment process of the product of this invention, its purpose is to fully dissolve the alloying elements in the steel plate into the matrix to obtain excellent corrosion resistance and a suitable two-phase microstructure ratio. The specific process is as follows: heating time coefficient is 1.4~2.0 min / mm, heating to 1075~1100 ℃ and holding for 1.5~2.2 min / mm, followed by rapid cooling to room temperature at a cooling rate of 180~220 ℃ / min using high-pressure cooling water at a laminar flow rate of 250~300 m / min. 3 / h.
[0023] Furthermore, the continuously cast billet needs to undergo forging to ensure the quality of the billet core and eliminate harmful structures such as dendrites and porosity from the solidification process. The specific process is as follows: the billet is heated to 1201~1250 ℃ and held for 5~6 h, with the forging ratio maintained between 1.8 and 2.5; the initial forging temperature is 1200~1265 ℃, and the final forging temperature is 1000~1050 ℃; if the temperature drops below 1000 ℃ during forging, it should be reheated in the furnace, and the billet should be allowed to cool naturally after forging.
[0024] By applying the above-mentioned chemical composition and process, the heat-resistant and corrosion-resistant stainless steel of the present invention achieves a synergistic improvement in high-temperature mechanical properties and corrosion resistance through optimized composition design and adjustment of production process, and can be applied to engineering environments under harsh working conditions such as high temperature and corrosive media.
[0025] Compared with the prior art, the present invention has the following advantages: 1. This invention precisely adjusts the alloy element ratio, sets the Cr / Ni equivalent range and the Nb-Ta-CN correlation coefficient, and precisely controls the proportion of austenite and ferrite phases to suppress excessive δ-ferrite formation, avoid dendrite overlap and internal porosity defects in the cast billet, and improve the quality of the cast billet and welding. By utilizing the synergistic effect of Nb and Ta, it preferentially combines with C to suppress Cr depletion at grain boundaries, reduce denitrification and porosity defects, and strengthens and refines grains with the help of the second phase, significantly improving the resistance to intergranular corrosion. N stabilizes austenite, Mo constructs a stable passivation film, and Si ensures high-temperature oxidation resistance, while strictly limiting harmful impurities such as P and S, achieving simultaneous improvement in room temperature and high-temperature mechanical properties and pitting corrosion resistance, making it suitable for harsh high-temperature corrosion service conditions.
[0026] 2. This invention provides a complete process encompassing forging, segmented rolling, and solution treatment with rapid cooling. The forging process controls the forging ratio and forging temperature to eliminate core defects such as dendrites and porosity in the cast billet, improving its internal microstructure. The rolling process employs a two-stage rolling technique, strictly controlling the furnace heating time, initial rolling temperature, and final rolling temperature. The first pass involves a large deformation, followed by subsequent smaller deformation rolling, balancing deformation penetration and microstructure control to avoid processing defects. The solution treatment uses a reasonable heating and holding time coefficient, employing high-pressure water cooling at a high cooling rate to ensure sufficient dissolution of alloying elements into the matrix, precisely locking the target austenite-ferrite two-phase ratio. This complete process can stably produce steel plates ranging from 10 to 80 mm thick, achieving high yield strength, excellent low-temperature impact resistance, and low pitting rate, with high product performance consistency, meeting the actual production needs of equipment manufacturing.
[0027] 3. The stainless steel products produced by the process of this invention have good mechanical properties, and their room temperature yield strength in the solution-treated state is [not specified]. R p0.2 Tensile strength can reach 625 MPa and above. R m can reach 800 MPa and above, elongation A ≥39%; Tensile yield strength at 550 ℃ R p0.2 Tensile strength can reach 440 MPa and above. R The strength can reach 675 MPa and above, with an elongation of [missing information]. A ≥33%. It can meet the mechanical performance requirements under different working conditions.
[0028] 4. The stainless steel products produced by the process of this invention have a thickness range of 10~80 mm and have good corrosion resistance. According to the ASTM G48 standard, the product's pitting corrosion rate is less than 3 mdd.
[0029] The heat-resistant and corrosion-resistant stainless steel manufactured using this technical solution has a thickness range of 10~80 mm and a room temperature yield strength in the solution-treated state. R p0.2 ≥625 MPa, tensile strength R m≥800 MPa, elongation A ≥39%; Tensile yield strength at 550 ℃ R p0.2 ≥440 MPa, tensile strength R m≥675 MPa, elongation A ≥33%; Impact resistance -40℃ KV 2≥180 J; This product has good corrosion resistance. According to the ASTM G48 standard, the product's corrosion resistance is tested and the pitting corrosion rate is less than 3 mdd. Detailed Implementation
[0030] The present invention will be further illustrated below through embodiments. The embodiments described below provide a more detailed account of the invention. These embodiments are merely descriptions of the best mode of implementation and do not limit the scope of the invention in any way. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0031] This invention is achieved through the following process steps: The continuously cast billet needs to be forged. The billet is first heated to 1201~1250 ℃ and held for 5~6 hours, with a forging ratio maintained between 1.8 and 2.5. The initial forging temperature is 1200~1265 ℃, and the final forging temperature is 1000~1050 ℃. If the temperature drops below 1000 ℃ during forging, the billet should be reheated in the furnace. After forging, the billet cools naturally. The forged billet is then heated to 1255~1265 ℃, with a total furnace time of 4.5~5.5 hours. The initial rolling temperature is 1220~1250 ℃, with a first-pass deformation of 28%~35%. The billet is then allowed to cool to room temperature. The second-stage initial rolling temperature is controlled at 1100~1150 ℃, with subsequent single-pass deformations of 10%~20%, and a final rolling temperature of 950~980 ℃. Following this, solution treatment is performed with a heating time coefficient of 1.4~2.0 min / mm, heating to 1075~1100 ℃. The temperature is maintained at ℃, with the holding time coefficient controlled within the range of 1.5~2.2 min / mm. Subsequently, it is rapidly cooled to room temperature by high-pressure cooling water at a cooling rate of 180~220 ℃ / min, with a laminar flow rate of 250~300 m / min. 3 / h.
[0032] The following examples are merely some preferred embodiments of the present invention and do not limit the scope and technical means of the invention in any way. Table 1 shows the chemical composition of Examples 1-10, Table 2 shows the process parameters for forging the billets in each example, Table 3 shows the process parameters for rolling and solution treatment in each example, and Table 4 shows the microstructure and mechanical properties of each example.
[0033] Table 1 Chemical composition of the examples Example C / % Si / % Mn / % P / % S / % Ni / % Cr / % Mo / % Ta / % Nb / % N / % 1 0.059 1.01 1.51 0.010 0.001 14.50 24.99 6.80 0.24 0.15 0.10 1.72 0.13 2 0.058 1.02 1.53 0.019 0.002 14.00 24.95 6.10 0.23 0.17 0.11 1.77 0.12 3 0.056 1.06 1.62 0.018 0.003 13.50 24.53 5.90 0.21 0.39 0.12 1.81 0.16 4 0.054 1.21 1.66 0.017 0.004 13.00 24.51 6.90 0.21 0.35 0.13 1.87 0.14 5 0.053 1.23 1.74 0.015 0.005 12.00 24.69 6.60 0.18 0.25 0.14 2.05 0.10 6 0.051 1.34 1.79 0.005 0.004 11.00 24.78 6.70 0.16 0.28 0.15 2.22 0.10 7 0.046 1.46 1.82 0.004 0.003 10.50 23.07 7.00 0.15 0.30 0.16 2.19 0.10 8 0.044 1.49 1.86 0.011 0.002 10.00 22.48 6.50 0.2 0.33 0.14 2.25 0.13 9 0.043 1.57 1.93 0.010 0.002 9.50 21.63 4.50 0.23 0.37 0.12 2.28 0.17 10 0.041 1.60 1.95 0.003 0.001 9.30 21.14 5.00 0.25 0.39 0.10 2.28 0.21 Table 2. Process parameters for billet forging in each embodiment Example Heating temperature / ℃ Insulation time / h Forging ratio Forging temperature / °C Final forging temperature / °C 1 1246 5.1 1.80 1200 1011 2 1236 5.6 1.90 1203 1014 3 1230 5.3 1.95 1217 1021 4 1240 5.7 2.00 1221 1024 5 1235 6.0 2.10 1227 1028 6 1243 5.2 2.20 1234 1031 7 1245 5.8 2.30 1247 1036 8 1231 6.0 2.35 1251 1042 9 1201 5.8 2.40 1257 1043 10 1207 5.7 2.50 1260 1049 Table 3 Process parameters for rolling and solution treatment in each embodiment Example Heating temperature / ℃ Furnace time / h Rolling temperature / ℃ First pass deformation amount / % Second-stage rolling temperature / ℃ Other single-pass deformation amount / % Final rolling temperature / ℃ <![CDATA[Heating time coefficient / min·mm -1 > Insulation temperature / ℃ <![CDATA[Holding time coefficient / min·mm -1 > <![CDATA[Cooling rate / °C·min -1 > <![CDATA[Laminar flow velocity / m 3 ·h -1 > 1 1255 4.5 1221 28 1101 13 951 1.41 1075 1.51 220 251 2 1257 5.0 1222 28 1102 18 952 1.42 1077 1.52 217 253 3 1256 4.7 1224 29 1113 10 954 1.53 1081 1.61 212 257 4 1256 5.0 1225 30 1122 12 961 1.54 1083 1.64 210 263 5 1259 5.3 1231 30 1126 11 964 1.65 1084 1.77 207 272 6 1264 4.7 1232 31 1131 19 967 1.66 1092 1.81 204 273 7 1262 5.3 1233 32 1133 18 971 1.81 1093 1.92 201 281 8 1263 5.4 1236 33 1142 18 972 1.87 1096 2.01 198 286 9 1260 5.2 1244 34 1147 15 974 1.92 1097 2.16 197 297 10 1264 4.9 1250 35 1150 13 980 2.00 1100 2.20 195 300 Table 4. Microstructure and mechanical properties of each embodiment
[0034] As can be seen from Table 4, the room temperature yield strength of stainless steel in the solution-treated state in the embodiments of the present invention is...R p0.2 The tensile strength ranges from 625 to 656 MPa, with all values ≥625 MPa. R m is 806~846 MPa, all ≥800 MPa, elongation A All ≥39%; 550 ℃ high temperature tensile yield strength R p0.2 The tensile strength ranges from 441 to 457 MPa, with all values ≥440 MPa. R m is 677~712 MPa, all ≥675MPa, elongation A All ≥33%; Impact resistance -40 ℃ KV Both values are between 181 and 217 J. The corrosion resistance of the products was tested according to ASTM G48 standard, and the pitting corrosion rate was less than 3 mdd.
[0035] It is hereby noted that the above embodiments are only for illustrating the technical concept and features of the present invention, and are not intended to limit the present invention. Any equivalent substitutions or modifications made without departing from the essence of the present invention fall within the protection scope of the present invention.
Claims
1. A heat-resistant and highly corrosion-resistant stainless steel, characterized in that, The steel plate's chemical composition by weight percentage is as follows: C: 0.040%~0.060%, Si: 1.01%~1.65%, Mn: 1.50%~1.95%, P≤0.020%, S≤0.010%, Ni: 9.01%~14.59%, Cr: 20.50%~24.99%, Mo: 4.50%~7.00%, Ta: 0.09%~0.25%, Nb: 0.15%~0.39%, N: 0.10%~0.17%, with the remainder being Fe and unavoidable impurities; Cr / Ni equivalent ratio... σ It is in the range of 1.70 to 2.
35.
2. The heat-resistant and corrosion-resistant stainless steel according to claim 1, characterized in that, The contents of Ta, Nb, C, and N satisfy the following relationship: The β The range is 0.10~0.
22.
3. The heat-resistant and corrosion-resistant stainless steel according to claim 1, characterized in that, The stainless steel microstructure comprises austenite and ferrite, wherein the volume fraction of austenite is 44.5% to 48.5%, and the remainder is ferrite.
4. The heat-resistant and corrosion-resistant stainless steel according to claim 1, characterized in that, The stainless steel in its solution-treated state has a room temperature yield strength ≥625 MPa, a tensile strength ≥800 MPa, and an elongation of... A ≥39%; 550℃ high-temperature tensile yield strength ≥440MPa, tensile strength ≥675 MPa, elongation A ≥33%; the impact resistance of the stainless steel is -40 ℃ KV 2≥180 J, pitting corrosion rate less than 3 mdd; the thickness of the stainless steel is in the range of 10~80 mm.
5. A method for manufacturing the heat-resistant and corrosion-resistant stainless steel according to any one of claims 1 to 4, comprising billet forging, rolling, and solution treatment processes, characterized in that, Rolling: The forged steel billet is heated to 1255~1265 ℃, with a total furnace time of 4.5~5.5 h. The initial rolling temperature is 1220~1250 ℃, and the deformation amount in the first pass is 28%~35%. The steel plate is then left to heat up. The initial rolling temperature in the second stage is controlled at 1100~1150 ℃, and the deformation amount in the remaining single passes is 10%~20%. The final rolling temperature is 950~980 ℃. Solution treatment: The heating time coefficient is 1.4~2.0 min / mm, heated to 1075~1100 ℃ and held for 1.5~2.2 min / mm, followed by rapid cooling to room temperature at a cooling rate of 180~220 ℃ / min using high-pressure cooling water at a laminar flow rate of 250~300 m / min. 3 / h.
6. The method for manufacturing heat-resistant and corrosion-resistant stainless steel according to claim 5, characterized in that, The continuously cast billet needs to be forged. The billet is heated to 1201~1250 ℃ and held for 5~6 h. The forging ratio is between 1.8 and 2.
5. The initial forging temperature is 1200~1265 ℃, and the final forging temperature is 1000~1050 ℃.
Citation Information
Patent Citations
Edge-crack-free duplex stainless steel and preparation thereof
CN117265418A
Double-phase stainless steel plate with high corrosion resistance and small anisotropy and manufacturing method
CN118957454A
Duplex stainless steel containing rare earth elements and preparation process of duplex stainless steel