A deformation heat treatment method to improve the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys

By combining low-temperature solution treatment and under-aging treatment with dislocation strengthening, the problem of synergistic optimization of strength and bending plasticity in Al-Mg-Si-Cu aluminum alloys has been solved, achieving a high-efficiency improvement in the forming performance of aluminum alloys, which is suitable for lightweight automotive components, rail transit structural parts, and high-end 3C products.

CN123108445APending Publication Date: 2026-11-17GUANGXI ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611622265.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing Al-Mg-Si-Cu aluminum alloys are difficult to optimize in a coordinated manner between strength and bending plasticity, and traditional heat treatment processes cannot meet the complex working conditions required for high-end applications.

Method used

A combination of low-temperature solution treatment, under-aging treatment, and tensile treatment is adopted, including high-temperature rolling, room-temperature rolling, low-temperature solution quenching, and under-aging treatment, to control the size and distribution of precipitated phases, and to replace precipitation strengthening with dislocation strengthening.

Benefits of technology

It significantly improves the strength and bending performance of aluminum alloys, shortens the production cycle, reduces energy consumption, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108445A_ABST
    Figure CN123108445A_ABST
Patent Text Reader

Abstract

This invention relates to the field of aluminum alloy manufacturing technology, specifically disclosing a deformation heat treatment method for improving the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys. It aims to solve the problem of difficulty in synergistically optimizing strength and bending plasticity in the production of existing aluminum alloys. The method includes casting, homogenization heat treatment, high-temperature rolling, room-temperature rolling, low-temperature solution quenching, under-aging, and tensile treatment. This method controls the solution quenching temperature at 500~510℃ to achieve partial dissolution and retention of strengthening phases. Under-aging treatment controls the number, size, and spacing of precipitated phases to be small. Tensile treatment introduces dislocation strengthening and induces dislocation configuration evolution, resulting in a yield plateau in the tensile curve. This method uses low-temperature solution treatment, reducing the solution temperature by approximately 50℃ compared to conventional processes, shortening the aging time to less than 1 hour, reducing energy consumption and shortening the production cycle, while simultaneously achieving a dual improvement in strength and elongation, and excellent bending performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy manufacturing technology, and specifically relates to a deformation heat treatment method for improving the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys. Background Technology

[0002] Al-Mg-Si-Cu aluminum alloys, as typical heat-treatable aluminum alloys, possess low density, high specific strength, excellent corrosion resistance, weldability, and paint hardening properties, making them core lightweight materials for automotive lightweight bodies, rail transit structural components, high-end 3C product shells, and new energy vehicle parts. This alloy primarily relies on precipitation strengthening through the formation of nano-sized Mg2Si, Mg5Al2Si4, and Q-Al5Cu2Mg8Si6 strengthening phases during the solution-aging process. By rationally controlling the alloy composition and heat treatment process, the mechanical load-bearing requirements of structural components can be met while ensuring lightweight design. With the continuous increase in the precision, reliability, and formability requirements of aluminum alloy components in high-end equipment manufacturing, traditional single heat treatment processes are no longer sufficient to meet the performance demands under complex working conditions. Currently, in industrial production, Al-Mg-Si-Cu aluminum alloys generally suffer from the core challenge of the difficulty in synergistically optimizing strength and bending plasticity.

[0003] On the one hand, simply increasing the aging temperature and extending the aging time to pursue high strength can easily lead to coarse and aggregated precipitates, increased stress concentration within the crystals, and problems such as cracks and forming failures during bending, which cannot meet the processing requirements of deep bending and complex curved surface forming.

[0004] On the other hand, if the strength index is reduced in order to ensure bending plasticity, it will lead to insufficient load-bearing capacity and shortened service life of the components, which will seriously restrict the expansion of high-end application scenarios of the alloy.

[0005] In existing technologies, some processes attempt to improve the overall properties of alloys through pre-deformation and graded aging, but significant drawbacks remain. While direct aging after conventional cold deformation can rapidly increase strength, the uneven dislocation distribution leads to internal microstructure incoordination, resulting in a significant decrease in bending performance. Conventional solution treatment combined with peak aging can achieve high ultimate strength, but it cannot effectively address the unique problems of uneven precipitate formation and grain boundary embrittlement caused by Cu in Al-Mg-Si-Cu alloys, which drastically reduce the material's bending performance. Therefore, developing a deformation heat treatment method that can simultaneously improve the strength and bendability of Al-Mg-Si-Cu aluminum alloys, with a simple process and suitability for industrial production, has become a pressing technical challenge in the high-end aluminum alloy processing field.

[0006] Based on this, the present invention proposes a deformation heat treatment method to improve the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys, so as to solve the problems existing in the prior art. Summary of the Invention

[0007] The purpose of this invention is to provide a deformation heat treatment method to improve the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys, so as to solve the problem that it is difficult to optimize the strength and bending plasticity of existing Al-Mg-Si-Cu aluminum alloys in actual production and application.

[0008] To achieve the above objectives, the present invention provides the following technical solution:

[0009] A deformation heat treatment method for improving the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys includes the following steps:

[0010] Melting and casting process: Al-Mg-Si-Cu aluminum alloy raw material is melted and cast to obtain ingots;

[0011] Homogenization heat treatment involves cutting off the head and tail of the ingot, milling the surface, and then performing homogenization heat treatment.

[0012] High-temperature rolling process involves directly rolling the homogenized heat-treated ingot at high temperature, and then allowing the coil to cool naturally in the air after rolling.

[0013] Room temperature rolling process involves cooling the high-temperature rolled coil to below 60°C and then rolling it at room temperature.

[0014] Low-temperature solution quenching treatment involves subjecting the room-temperature rolled coil to low-temperature solution quenching treatment, followed by water cooling after heat preservation.

[0015] The under-aging treatment involves holding the solution-quenched material at a temperature range of 180℃-200℃ for 6 to 20 minutes.

[0016] Al-Mg-Si-Cu aluminum alloys are graded 6011, 6013, and 6015.

[0017] In a preferred embodiment, the melting temperature during the casting process is 720°C-760°C.

[0018] In a preferred embodiment, during the homogenization heat treatment of the ingot, the holding temperature is 530℃-560℃ and the holding time is 5-10 hours.

[0019] In a preferred embodiment, when the ingot is subjected to high-temperature rolling, the hot rolling start temperature is 540℃-560℃, the final rolling temperature is 350℃-450℃, the total rolling rate is greater than 85%, and the number of rolling passes is less than 22.

[0020] In a preferred embodiment, when the ingot is rolled at room temperature, the rolling pass rate is 15% and the number of rolling passes is 3.

[0021] In a preferred embodiment, when performing low-temperature solution quenching on the ingot, the temperature is 500℃-510℃ and the holding time is 0.3-0.8 hours.

[0022] In a preferred embodiment, aluminum alloy coils or sheets are prepared by the deformation heat treatment method steps.

[0023] In a preferred embodiment, the chemical composition of the aluminum alloy coil or sheet, by mass percentage, is as follows: silicon content 0.6%-1.3%, iron content 0.4%-0.5%, copper content 0.5%-1.1%, manganese content 0.1%-1.0%, magnesium content 0.5%-1.2%, chromium content 0.1%-0.25%, zinc content 0.1%-0.7%, titanium content not exceeding 0.1%, with the balance being aluminum and unavoidable impurity elements.

[0024] In a preferred embodiment, the chemical composition of the aluminum alloy, by mass percentage, is as follows: 0.79% silicon, 0.45% iron, 0.80% copper, 0.24% manganese, 0.82% magnesium, 0.12% chromium, 0.05% zinc, 0.03% titanium, with the balance being aluminum and unavoidable impurity elements.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0026] This invention employs low-temperature solution treatment, which reduces the solution quenching temperature by approximately 50°C compared to conventional quenching temperatures, thereby reducing equipment operating power and effectively lowering production energy consumption.

[0027] This invention significantly shortens the production cycle and improves production efficiency by controlling the aging process time to within 1 hour, compared to the traditional peak aging process which requires 6-10 hours.

[0028] This invention controls the final rolling temperature within the range of 350℃-400℃, inducing the precipitation of strengthening phases through rolling deformation, thus providing a microstructure basis for subsequent strengthening phase regulation.

[0029] This invention achieves "partial dissolution" regulation of the strengthening phase by controlling the solution quenching temperature at 500℃-510℃, which not only provides a reserve of solid solution atoms for subsequent under-aging, but also retains the direct strengthening effect of the refractory strengthening phase.

[0030] This invention replaces the traditional precipitation strengthening route with dislocation strengthening introduced by tensile treatment. Combined with the microstructure characteristics of fewer, smaller, and more spaced underaged precipitates, it effectively avoids stress concentration caused by the pinning effect of the strengthening relative to dislocations, thereby significantly improving the bending properties of the material.

[0031] This invention, through under-aging treatment, can control the average size of the precipitated phase to not exceed 20 nm and the area fraction to not exceed 1.5%. This results in the precipitated phase in the matrix being in a state of low quantity, small size, and large spacing under-aging, providing sufficient solid solution atoms and a weaker pinning effect of the precipitated phase for subsequent stretching to introduce dislocations.

[0032] This solves the problem of difficulty in synergistically optimizing strength and bending plasticity in the actual production and application of existing Al-Mg-Si-Cu aluminum alloys. Attached Figure Description

[0033] Figure 1 This is a flowchart illustrating the technical route of the deformation heat treatment method for improving the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys according to the present invention.

[0034] Figure 2 This is a mechanical test curve diagram of Embodiment 1 of the present invention.

[0035] Figure 3 This is a tensile fracture morphology diagram of the finished aluminum alloy coil product of Embodiment 1 of the present invention.

[0036] Figure 4 This is a mechanical test curve of Comparative Example 1 of the present invention.

[0037] Figure 5 This is a tensile fracture morphology diagram of the finished aluminum alloy coil of Comparative Example 1 of the present invention.

[0038] Figure 6 The figures show the XRD patterns of Example 1 in the hot-rolled and solution-treated states, and the XRD patterns of Examples 2-4 in the hot-rolled state. Specifically, Figure (a) shows Example 1 in the hot-rolled state (final rolling temperature 360°C); Figure (b) shows Example 1 in the solution-treated state (solution temperature 500°C); Figure (c) shows Examples 2 and 3 in the hot-rolled state (final rolling temperature 350°C); and Figure (d) shows Example 4 in the hot-rolled state (final rolling temperature 400°C).

[0039] Figure 7Figure 1 shows the surface morphology after bending tests in Examples 1-4 of the present invention. Specifically, Figure (a) shows the surface morphology after bending tests in Example 1; Figure (b) shows the surface morphology after bending tests in Example 2; Figure (c) shows the surface morphology after bending tests in Example 3; and Figure (d) shows the surface morphology after bending tests in Example 4.

[0040] Figure 8 The figures shown are surface morphology images of Comparative Examples 1 to 4 after bending tests. Specifically, Figure (a) shows the surface morphology image of Comparative Example 1 after bending tests; Figure (b) shows the surface morphology image of Comparative Example 2 after bending tests; Figure (c) shows the surface morphology image of Comparative Example 3 after bending tests; and Figure (d) shows the surface morphology image of Comparative Example 4 after bending tests.

[0041] Figure 9 The method of this invention uses a sample heated to 180℃ for 20 min and pre-stretched by 10% as an example to illustrate the surface morphology of the sample after bending test. Figure (a) shows the morphology of the sample after bending test following heat treatment at 180℃ for 20 min and 10% stretching, with a bending angle of 135°; Figure (b) is a magnified view of the bending point of the sample after bending. Detailed Implementation

[0042] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0043] In the standard YS / T 591-2025 Heat Treatment of Wrought Aluminum and Aluminum Alloys, the reference values ​​for solution heat treatment temperatures for AlMgSiCu series alloys are: 6013 sheet 563~574℃, 6013 bar 560~571℃, 6056 extrusion 544~557℃, 6061 rolled ring 516~552℃, and 6063 plate 516~579℃. To achieve complete solution treatment, the solution temperature for all the above AlMgSiCu alloys is greater than 510℃. However, this invention sets the temperature at 500~510℃. The purpose is to utilize the differences in the solution temperature windows corresponding to the different resolvable phases within the alloy to achieve partial resolvation within this temperature range. In the standard GB / T 3880.2-2024 General Industrial Aluminum and Aluminum Alloy Plates and Strips Part 2: Mechanical Properties, for the AlMgSiCu system, the yield strength Rp0.2 of 6061 alloy in the T6 condition is ≥240MPa, the tensile strength Rm is ≥290MPa, the elongation after fracture is ≤10%, and the bending radius is ≥2.5t (t is the thickness of the plate). The yield strength Rp0.2 of 6063 alloy in the T6 condition is ≥180MPa, and the tensile strength Rm is ≥230MPa.

[0044] As per the instruction manual Figure 1 To be continued Figure 9As shown, in view of the problems existing in the prior art, the embodiments of the present invention provide a deformation heat treatment method to improve the mechanical properties and bending properties of Al-Mg-Si-Cu aluminum alloy. The Al-Mg-Si-Cu aluminum alloy obtained by this method not only has a yield strength that is better than that of the T6 state of standard GB / T 3880.2-2024, but also has an elongation after fracture that can exceed 10% under conditions higher than 300MPa. The chemical composition of the Al-Mg-Si-Cu aluminum alloy, by mass percentage, is as follows: silicon (Si) 0.6%-1.3%, iron (Fe) 0.4%-0.5%, copper (Cu) 0.5%-1.1%, manganese (Mn) 0.1%-1.0%, magnesium (Mg) 0.5%-1.2%, chromium (Cr) 0.1%-0.25%, zinc (Zn) 0.1%-0.7%, titanium (Ti) not exceeding 0.1%, with the balance being aluminum (Al) and unavoidable impurities. In industrial applications, Al-Mg-Si-Cu aluminum alloys with the above composition are mainly graded 6011, 6013, and 6015. Meanwhile, the aforementioned Al-Mg-Si-Cu aluminum alloy, as a typical heat-treatable aluminum alloy, possesses low density, high specific strength, excellent corrosion resistance, weldability, and paint hardening properties, making it a core lightweight material in fields such as lightweight automotive bodies, rail transit structural components, high-end 3C product shells, and new energy vehicle parts. The aforementioned processing method includes the following steps:

[0045] Step 1: First, melt and cast the aluminum alloy raw material to obtain an ingot;

[0046] Step 1.1: In the casting process, the proportioned Al-Mg-Si-Cu aluminum alloy raw materials are added to the melting furnace for melting. The melting temperature is controlled within the range of 720℃-760℃ to ensure that all elements are fully dissolved to form a uniform melt.

[0047] Step 1.2: After smelting, refining is carried out to remove gases and inclusions from the melt, and then casting is performed to obtain ingots;

[0048] Step 1.3: After the ingot solidifies, the head and tail are trimmed and the surface is milled to remove surface defects and segregation layers, and then it is sent to Step 2 for homogenization heat treatment.

[0049] Step 2: Perform homogenization heat treatment on the ingot obtained in Step 1;

[0050] The holding temperature for homogenization heat treatment is 530℃-560℃, and the holding time is set to 5-10 hours to obtain the homogenized heat-treated ingot.

[0051] By setting the homogenization temperature within the above range, the eutectic and non-equilibrium phases inside the ingot can be fully dissolved, eliminating compositional segregation and laying the microstructure foundation for subsequent rolling and heat treatment.

[0052] Step 3: High-temperature rolling treatment;

[0053] After the homogenization heat treatment of the ingot in step 2 is completed, the ingot is directly sent to the high-temperature rolling process. During the high-temperature hot rolling, the starting temperature is set to 540℃-560℃, the final rolling temperature is set to 350℃-400℃, the total rolling rate is set to be greater than 85%, and the number of rolling passes is controlled within 22 passes. After the rolling is completed, the coil is naturally cooled in the air.

[0054] In the high-temperature rolling process, controlling the final rolling temperature between 350℃ and 400℃ is a key innovation in achieving the technical effect of this embodiment. During rolling deformation within this temperature range, the dynamic precipitation effect induced by the rolling process causes Al... 1.9 CuMg 4.1 Si 3.3 Mg2Si, Al 55 Mn 20 Si 25 A large amount of strengthening phases, such as Al4Mn3Si2 and Al6CuMg4, precipitate. Due to the complex changes in the rheological and temperature fields during hot rolling, these precipitated strengthening phases exhibit non-uniform characteristics in morphology and size distribution. This non-uniform distribution provides a material basis for the subsequent low-temperature solution quenching to achieve "partial dissolution" control of the strengthening phases. After high-temperature rolling, the coil is naturally cooled in air.

[0055] Step 4: Room temperature rolling treatment;

[0056] After high-temperature rolling, the ingot is transformed into a high-temperature rolled coil. This process further refines the grains and introduces dislocations through cold deformation, providing microstructure preparation for subsequent heat treatment. Specifically, the high-temperature rolled coil is cooled to below 60°C and then rolled at room temperature. During the process, the rolling pass rate is 15%, and the number of rolling passes is 3. After room temperature rolling, the coil is sent to a low-temperature solution quenching process.

[0057] Step 5: Solution quenching treatment;

[0058] The room temperature rolled coil obtained in step 4 is subjected to solution quenching. The solution quenching temperature is set at 500℃-510℃ and the holding time is set at 0.3-0.8 hours. After the holding time is completed, it is water-cooled to obtain the solution-quenched coil. After the solution quenching is completed, the solution-quenched material is sent to the under-aging treatment process.

[0059] In this step, controlling the solution quenching temperature to 500℃-510℃ is the core of achieving the technical effect of this embodiment. Within this temperature range, combined with a holding time of 0.3-0.8 hours, selective dissolution of the strengthening phase can be achieved by controlling the temperature-time parameter combination of solution quenching.

[0060] Specifically, it is necessary to ensure that Al 1.9 CuMg 4.1 Si 3.3 The remelting rate of the Cu-containing strengthening phase is no less than 80% to reserve solid solution atoms; simultaneously, the volume fraction retention rate of the heat-resistant phase, such as Mg2Si, is controlled between 5% and 15% to maintain the initial strengthening effect. This remelting rate and retention rate can be calibrated by X-ray diffraction (XRD) or transmission electron microscopy (TEM) and a correspondence with solid solution parameters can be established. For example, for alloys with a Si / Cu mass ratio in the range of 0.8-1.5 as described in this application, the above effect can be achieved by holding at 500℃ for about 0.8 hours or at 510℃ for about 0.3 hours. This "partial remelting, partial retention" strategy avoids the problem of complete phase dissolution or grain coarsening caused by high-temperature solid solution, and also avoids the large amount of coarse precipitates resulting from peak aging treatment after solid solution treatment. Compared with the conventional solid solution quenching temperature of 560℃, the solid solution quenching temperature used in this embodiment is reduced by about 50℃, resulting in a corresponding reduction in equipment operating power and effectively reducing production energy consumption.

[0061] Step 6: Handling of under-time delivery;

[0062] The under-aging treatment involves holding the solution-quenched material at a temperature range of 180℃-220℃ for 6 to 20 minutes to control the average size of the precipitates to not exceed 20 nm and the area fraction to not exceed 1.5%. This ensures that the precipitates in the matrix are in a state of low quantity, small size, and large spacing under-aging, thereby providing sufficient solid solution atoms and a weak pinning effect of the precipitates for subsequent tensile dislocation introduction.

[0063] The aforementioned temperature and time parameters result in the strengthening phases precipitated in the under-aged state exhibiting a distribution characterized by fewer phases, smaller sizes, and larger spacing. Compared to the abundant strengthening phases precipitated in the peak-aged state, the precipitates in the under-aged state significantly reduce the pinning effect on dislocation motion, creating microstructural conditions for the full evolution of dislocation configurations during subsequent tensile treatment. When the holding time is 0 hours, it indicates that no artificial aging treatment is performed, and the solution-quenched material directly enters the tensile treatment process.

[0064] The temperature for the above-mentioned under-aging treatment is 180℃-220℃, and the holding time is 6 minutes-20 minutes.

[0065] The aforementioned reduction in under-time processing time significantly shortens the production cycle and improves production efficiency compared to the traditional peak-time processing method that requires 6-10 hours.

[0066] Step 7: Stretching treatment;

[0067] After the under-aging treatment step 6, the roll material is stretched, and the stretching rate is not less than 5%.

[0068] The large number of dislocations introduced by tensile treatment can effectively increase the strength of materials, specifically:

[0069] During the stretching process, at room temperature at 10 ﹣3 ~10 ﹣1 s ﹣1 Tensile deformation at strain rates of 5%-20% is applied. The dislocation strengthening introduced by the tensile treatment replaces the traditional precipitation strengthening pathway. Combined with the microstructure characteristics of fewer, smaller, and more widely spaced underaged precipitates, this effectively avoids stress concentration caused by pinning of dislocations in the strengthening phase. This deformation process introduces approximately 10¹²~10¹³ cm⁻¹ of dislocations into the matrix. ﹣2 Orders in magnitude of mobile dislocations. In the underaged state, the matrix retains a sufficient concentration of Mg, Si, and Cu solute atoms. During tensile deformation, these solute atoms form Cotillard atmospheres with dislocations, producing a pinning-unpinning effect. When the external stress exceeds the initial yield strength in subsequent mechanical property tests, a large number of pinned dislocations simultaneously unpin and begin to move, manifesting as a yield plateau with a length ≥2% on the tensile curve. This yield plateau indicates that dislocation strengthening effectively enhances the material's uniform deformation capability, thereby significantly improving bending plasticity. The appearance of the yield plateau effectively increases the material's uniform elongation, ultimately achieving a dual improvement in strength and elongation. This tensile-induced dislocation strengthening replaces the traditional precipitation strengthening route. Combined with the microstructure characteristics of fewer, smaller, and more spaced precipitates in the underaged state, it effectively avoids stress concentration caused by the pinning effect of the strengthening relative to dislocations, thus significantly improving the bending performance of the material.

[0070] The technical solution and its effects of the present invention will be described in detail below through specific embodiments.

[0071] Example 1:

[0072] This embodiment employs a process of directly performing a 15% tensile treatment after low-temperature solution quenching at 500℃. The chemical composition of the Al-Mg-Si-Cu aluminum alloy raw material, by mass percentage, is: Si 0.6%, Fe 0.4%, Cu 0.5%, Mn 0.1%, Mg 0.5%, Cr 0.1%, Zn 0.1%, Ti 0%, with the balance being Al and unavoidable impurity elements. The process includes the following steps:

[0073] After melting and casting the Al-Mg-Si-Cu aluminum alloy raw materials with the above components to obtain an ingot;

[0074] After undergoing homogenization heat treatment at 540℃ for 10 hours, the ingot is sent to the high-temperature rolling process.

[0075] The hot rolling start temperature is set at 540℃, the hot rolling finish temperature is set at 350℃, the total processing rate is set at 95%, the number of rolling passes is 22, and the coil is allowed to cool naturally in the air after rolling.

[0076] After high-temperature rolling, room-temperature rolling is performed with a pass rate of 15% and a total of 3 rolling passes.

[0077] After room temperature rolling, solution quenching is performed. The holding temperature is set at 500℃ and the holding time is set at 0.3 hours. After the holding time is completed, water cooling is performed to obtain solution quenched coils.

[0078] After solution quenching, the material is directly subjected to stretching treatment with a stretching rate of 15% to obtain aluminum alloy coils.

[0079] Tensile tests were performed on the aluminum alloy coil of this embodiment, and its engineering stress-strain curve is shown below. Figure 2 As shown in the figure, due to the tensile deformation treatment of the material, the yield strength and tensile strength can reach 309 MPa and 323 MPa, respectively. Moreover, the curve shows a clear yield plateau characteristic in the yield stage. The appearance of the yield plateau plays a role in increasing the elongation, and the elongation after fracture can reach 12.7%.

[0080] Figure 3 This is a scanning electron microscope (SEM) image of the tensile fracture surface of the aluminum alloy coil in Example 1, magnified at 500x with a scale bar of 10 μm. The fracture surface is covered with numerous dense dimples, exhibiting typical ductile fracture characteristics, indicating that the failure mechanism of the material is ductile fracture, and verifying that the material possesses excellent elongation.

[0081] Example 2:

[0082] This embodiment uses a process of solution treatment at 500℃ followed by under-aging at 180℃ for 20 minutes, and then 10% tensile treatment.

[0083] This embodiment uses the same chemical composition and front-end process parameters as Embodiment 1. The main difference lies in the under-aging treatment and stretching treatment parameters after solution treatment.

[0084] The final hot rolling temperature is set to 450℃;

[0085] The holding time for solution quenching is extended to 0.8 hours;

[0086] After solution quenching, a slight aging treatment is performed. The holding temperature for the slight aging treatment is set at 180℃, and the holding time is set at 20 minutes, in order to precipitate some strengthening phases and slightly improve the strength of the material. After the slight aging treatment, a tensile treatment is performed, with the elongation rate set at 10%.

[0087] The aluminum alloy coil obtained using this process has a yield strength of 302 MPa, a tensile strength of 324 MPa, and an elongation of 15.5%. Compared with Example 1, this example further improves the elongation of the material by introducing a short-term under-aging treatment.

[0088] Example 3:

[0089] This embodiment uses a process of solution treatment at 500℃ followed by under-aging at 220℃ for 6 minutes, and then 8% tensile treatment.

[0090] This embodiment uses the same chemical composition and front-end process parameters as Embodiment 1. The main difference lies in the under-aging treatment and stretching treatment parameters after solution treatment.

[0091] The final hot rolling temperature is set to 350℃.

[0092] The holding time for solution quenching is set to 0.8 hours;

[0093] After solution quenching, a short-term aging treatment was performed. The holding temperature for the short-term aging treatment was set at 220℃, and the holding time was set at 6 minutes. The elongation rate for the tensile treatment was set at 8%.

[0094] The aluminum alloy coils obtained using this process have a yield strength of 300 MPa, a tensile strength of 323 MPa, and an elongation of 15.8%. The bending test showed only slight orange peel texture on the surface, with no cracking.

[0095] Example 4:

[0096] This embodiment employs a composition design scheme that increases the Cu content and a process scheme that involves solution treatment at 510℃ followed by a 15% stretching treatment. The chemical composition of this embodiment, by mass percentage, is: Si 0.79%, Fe 0.45%, Cu 0.80%, Mn 0.24%, Mg 0.82%, Cr 0.12%, Zn 0.05%, Ti 0.03%, with the balance being Al and unavoidable impurity elements.

[0097] Compared with Example 1, the Cu content increased to 0.80% and the Si content decreased to 0.79%.

[0098] The ingot preparation, homogenization annealing, and room temperature rolling process parameters were exactly the same as in Example 1;

[0099] The hot rolling final rolling temperature was increased by 50°C compared to Example 1, and was set to 400°C;

[0100] The holding temperature for solution quenching was increased by 10°C compared to Example 1, set at 510°C, and the holding time was set at 0.8 hours. After solution quenching, the material was directly subjected to tensile treatment, with a tensile rate set at 15%.

[0101] The aluminum alloy coils obtained using this process have a yield strength of 310 MPa, a tensile strength of 334 MPa, and an elongation of 14.6%, exhibiting excellent overall performance.

[0102] Comparative Example 1:

[0103] The conventional process, as described in Example 1, involved solution quenching followed by peak aging treatment. The chemical composition and initial process parameters of this comparative example were identical to those of Example 1, with the solution quenching temperature set at 500°C and the holding time at 0.8 hours. Unlike Example 1, peak aging treatment was performed directly after solution quenching. The holding temperature for peak aging was set at 180°C and the holding time at 6 hours, resulting in peak material strength. Tensile tests were conducted on this comparative example sample, and its stress-strain curve is shown below. Figure 4 As shown.

[0104] It can be seen that the yield strength of this comparative example is 268 MPa, the tensile strength is 305 MPa, and the elongation is 11.6%, all of which are significantly lower than those of Example 1. Figure 5 The image shown is a scanning electron microscope (SEM) image of the tensile fracture surface of Comparative Example 1, magnified at 500x and with a scale bar of 20 μm. The number of dimples 10 on the fracture surface is significantly reduced and shallower, indicating that the coarse strengthening phase precipitated during peak aging hinders dislocation movement, leading to increased brittleness of the material.

[0105] Comparative Example 2:

[0106] The process scheme of solution treatment followed by stretching and then under-aging treatment differs from Example 1 mainly in the order of the steps. After solution quenching, the material is first pre-stretched by 15%, and then subjected to heat treatment at 220°C for 10 minutes.

[0107] The elongation of this comparative example was only 9.8%, which was significantly lower than that of Example 1, indicating that the process sequence of stretching followed by aging treatment would lead to a decrease in bending performance.

[0108] Comparative Example 3:

[0109] The traditional process of high-temperature solution treatment followed by peak aging was adopted. The chemical composition of this comparative example, by mass percentage, was: Si 0.65%, Fe 0.16%, Cu 0.69%, Mn 0.23%, Mg 0.75%, Cr 0.03%, Zn 0.01%, and Ti 0.04%, with reduced contents of the main elements Si, Cu, and Mg compared to Example 1. The ingot preparation, homogenization annealing, hot rolling, and cold rolling were exactly the same as in Example 1. The difference from Example 1 was that the cold-rolled coil was subjected to a high-temperature quenching at 560℃ for 20 minutes, followed by peak aging treatment at 180℃ for 6 hours.

[0110] The yield strength of the material using this process is 263 MPa, the tensile strength is 321 MPa, the elongation is 11.4%, and it breaks directly during bending tests.

[0111] Comparative Example 4:

[0112] The traditional process of high-temperature solution treatment followed by peak aging was also employed. The chemical composition of this comparative example was exactly the same as that of Example 4, and the preparation of the ingot, homogenization annealing, hot rolling, and cold rolling were also exactly the same as in Example 4. The difference from Example 4 was that the cold-rolled coil was subjected to high-temperature quenching at 560°C for 20 minutes, followed by peak aging treatment at 180°C for 6 hours.

[0113] The yield strength of the material using this process is 279 MPa, the tensile strength is 325 MPa, the elongation is 12.1%, and it breaks directly during bending tests.

[0114] The performance test results of the aluminum alloy coil products of the above embodiments and comparative examples are shown in Table 1.

[0115] Table 1: Performance test results of aluminum alloy coil products from Examples 1-4 and Comparative Examples 1-4

[0116]

[0117] The test results in Table 1 fully demonstrate the significant effect of the method of the present invention in improving the bending performance of Al-Mg-Si-Cu aluminum alloys.

[0118] like Figure 6 As shown in the XRD patterns of the hot-rolled coils in Examples 1-4, it can be seen that a large number of strengthening phases exist inside the coils after hot rolling, mainly containing Al. 1.9 CuMg 4.1 Si 3.3 Mg2Si, Al 55 Mn 20 Si 25Al4Mn3Si2, Al6CuMg4, etc. After solution treatment at 500℃, some reinforcing phases disappear their XRD diffraction peaks due to dissolution back into the matrix, for example... Figure 6 Al in solid solution state in Example 1 shown 1.9 CuMg 4.1 Si 3.3 The XRD diffraction peaks of one phase disappear, but other reinforcing phases remain because the solution temperature is insufficient to meet the re-dissolution conditions, such as... Figure 6 In Example 1, a large amount of Mg2Si phase exists in the solution-treated state. These reinforcing phases, which remain after hot rolling but do not re-dissolve after solution treatment, are beneficial to improving the mechanical properties of the material. In the method of the present invention, the large number of dislocations induced by the final stretching process can increase the strength of the material. Furthermore, in the stretching process, the stretch-induced dislocation configuration completes its evolution, resulting in a yield plateau in mechanical testing, while also increasing the overall elongation of the material.

[0119] Compared to conventional processes that use peak aging treatment after solution treatment at 560℃, which produces a large amount of reinforcing phase, this invention uses low-temperature solution treatment followed by short-term under-aging (or no aging) to control the quantity and size of the reinforcing phase precipitates. This reduces the amount of reinforcing phase precipitates due to aging during bending, avoiding pinning effects and stress concentration, thereby reducing the risk of material cracking. The surface morphology after bending tests in Examples 1-4 and Comparative Examples 1-4 is as follows: Figure 7 and Figure 8 As shown. Because this invention eliminates the need for lengthy manual aging processes, it improves production efficiency.

[0120] Taking a sample pre-stretched by 10% at 180℃ for 20 min as an example, a bending test was performed on the aluminum alloy sheet treated by the method described in this invention. The surface morphology of the sample after the bending test is as follows: Figure 9 As shown, the bending angle of the sample is 135°, indicating that the method described in this invention significantly improves the bendability of the material.

[0121] The above results demonstrate that this invention overcomes the technical bottleneck of the mutual constraint between strength and bending performance in Al-Mg-Si-Cu aluminum alloys through the synergistic combination of final rolling temperature control, low-temperature solution quenching, under-aging treatment, and tensile treatment. The dislocation strengthening introduced by the tensile treatment replaces the traditional precipitation strengthening route. Combined with the microstructure characteristics of fewer, smaller, and more widely spaced precipitates in the under-aging process, it effectively avoids stress concentration caused by the pinning effect of the strengthening relative to dislocations, thereby significantly improving the bending performance of the material. This deformation heat treatment method is simple, suitable for industrial production, and can meet the processing and use requirements of high-end lightweight components such as lightweight automotive bodies, rail transit structural parts, high-end 3C product shells, and new energy vehicle parts.

[0122] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A deformation heat treatment method for improving the mechanical and bending properties of Al-Mg-Si-Cu aluminum alloys, characterized in that, Al-Mg-Si-Cu aluminum alloys, designated as 6011, 6013, or 6015, include the following steps: Melting and casting process: Al-Mg-Si-Cu aluminum alloy raw material is melted and cast to obtain ingots; Homogenization heat treatment involves cutting off the head and tail of the ingot, milling the surface, and then performing homogenization heat treatment. High-temperature rolling process involves directly rolling the homogenized heat-treated ingot at high temperature, and then allowing the coil to cool naturally in the air after rolling. Room temperature rolling process involves cooling the high-temperature rolled coil to below 60°C and then rolling it at room temperature. Low-temperature solution quenching treatment involves subjecting the room-temperature rolled coil to low-temperature solution quenching treatment, followed by water cooling after heat preservation. For the under-aging treatment, the solution-quenched material is held at a temperature range of 180℃-220℃ for 6-20 minutes. Stretch treatment involves stretching the under-aged roll material, with a stretching rate of 5%-20%.

2. The deformation heat treatment method as described in claim 1, characterized in that, During the casting process, the melting temperature is 720℃-760℃.

3. The deformation heat treatment method as described in claim 1, characterized in that, When homogenizing the ingots, the holding temperature is 530℃-560℃ and the holding time is 5-10 hours.

4. The deformation heat treatment method as described in claim 1, characterized in that, When hot rolling ingots, the starting temperature is 540℃-560℃, the finishing temperature is 350℃-450℃, the total rolling rate is greater than 85%, and the number of rolling passes is less than 22.

5. The deformation heat treatment method as described in claim 1, characterized in that, When the ingot is rolled at room temperature, the rolling pass rate is 15%, and the number of rolling passes is 3.

6. The deformation heat treatment method as described in claim 1, characterized in that, When performing low-temperature solution quenching on ingots, the temperature is 500℃-510℃ and the holding time is 0.3-0.8 hours.

7. The deformation heat treatment method as described in claim 1, characterized in that, Aluminum alloy coils or sheets are prepared by the deformation heat treatment method described above.

8. The deformation heat treatment method as described in claim 7, characterized in that, The chemical composition of aluminum alloy coils or sheets, by mass percentage, is as follows: silicon content 0.6%-1.3%, iron content 0.4%-0.5%, copper content 0.5%-1.1%, manganese content 0.1%-1.0%, magnesium content 0.5%-1.2%, chromium content 0.1%-0.25%, zinc content 0.1%-0.7%, titanium content not exceeding 0.1%, with the balance being aluminum and unavoidable impurities.

9. The deformation heat treatment method as described in claim 8, characterized in that, The chemical composition of the aluminum alloy, by mass percentage, is as follows: silicon 0.79%, iron 0.45%, copper 0.80%, manganese 0.24%, magnesium 0.82%, chromium 0.12%, zinc 0.05%, titanium 0.03%, with the balance being aluminum and unavoidable impurities.