Intelligent powder mixing and spraying method and system based on CrSi target material

By injecting chromium powder and silicon powder into the core region and evolution region of the plasma jet respectively, and combining this with a smart powder mixing and spraying method that dynamically adjusts hydrogen and powder feeding rate, the problem of CrSi target material composition deviation was solved, achieving the preparation of target material with high density and consistent composition, which is suitable for the manufacture of thin film resistors and semiconductor devices.

CN123108461APending Publication Date: 2026-11-17JIANGSU HAITAI PHOTOELECTRIC MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611632922.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the preparation of CrSi targets using existing plasma spraying technology, the significant differences in the thermophysical properties of chromium and silicon cause uncontrollable vaporization loss of silicon powder, resulting in a serious deviation of the target composition from the preset deposition atomic ratio and uneven internal structure of the deposition layer, which makes it difficult to meet the requirements of high-performance electronic devices.

Method used

A smart powder mixing and spraying method is adopted. Chromium powder is injected into the core area of ​​the plasma jet and silicon powder is injected into the evolution zone. The temperature is monitored in real time using an infrared pyrometer, and the hydrogen mixing and silicon powder feeding rate are dynamically adjusted to construct a multi-flow field spatial decoupling and gas-powder linkage mechanism. This enables in-situ chemical cooling and quality repair. Combined with vacuum heating annealing, the consistency of target material composition and density are ensured.

Benefits of technology

It effectively avoids uncontrollable vaporization loss of silicon powder, maintains the consistency of target material composition, improves the density of the deposited layer, eliminates hydrogen embrittlement defects, and meets the composition and structural requirements of high-performance electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108461A_ABST
    Figure CN123108461A_ABST
Patent Text Reader

Abstract

This application relates to the field of target material preparation technology, and discloses an intelligent powder mixing and spraying method and system based on CrSi target material. Addressing the problem that silicon powder is easily vaporized and lost due to heat during target material preparation, leading to a significant deviation from the actual composition, this invention injects high-melting-point chromium powder into the core region of the plasma jet and easily vaporized silicon powder into the downstream, lower-temperature evolution region, achieving spatial enthalpy field decoupling. An infrared pyrometer is used to monitor the transient temperature of the deposition zone. When this temperature is determined to be greater than the safe sublimation vaporization threshold, hydrogen gas is dynamically mixed into the carrier gas at the auxiliary powder feed port. The endothermic dissociation of hydrogen molecules achieves in-situ chemical cooling of the micro-flow field, and simultaneously increases the instantaneous silicon powder feed rate to compensate for the mass loss due to pneumatic vaporization. After spraying, the deposited target material undergoes vacuum heating annealing to forcibly remove residual free hydrogen atoms. This invention suppresses overheating and sublimation of the silicon phase, maintains the preset deposition atomic ratio, improves the target material density, and eliminates the risk of hydrogen embrittlement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of target material preparation technology, specifically to an intelligent powder mixing and spraying method and system based on CrSi target material. Background Technology

[0002] Chromium-silicon composite targets are widely used in the manufacturing processes of thin-film resistors and semiconductor devices. In the processing of large-size semiconductor targets, plasma spraying technology has become one of the main preparation processes due to its high deposition efficiency and wide applicability to various materials.

[0003] In actual plasma spraying processes, the differences in thermophysical properties between chromium and silicon present inherent challenges to reconciling traditional mixed powder feeding techniques. To ensure complete penetration of the high-melting-point chromium powder, the plasma generator needs to output high arc power to maintain a high heat flux density in the jet core region. However, the sublimation vaporization critical temperature of silicon is much lower than the core region temperature. This makes the low-melting-point silicon powder prone to severe overheating and uncontrolled aerodynamic vaporization in the high-temperature, high-enthalpy field of co-spraying, ultimately leading to a significant deviation of the actual composition of the deposited target material from the pre-set atomic ratio.

[0004] Furthermore, the interface temperature fluctuates greatly due to the turbulent impact of the plasma jet and the transient heat accumulation on the substrate during the spray deposition process. Most existing conventional spray coating equipment relies on fixed static process parameters for continuous operation, making it impossible to dynamically intervene in the micro-flow field and control cooling based on the real-time thermal load of the deposition zone surface. This passive processing mode not only exacerbates the continuous vaporization loss of silicon phase powder but also easily leads to localized overheating of the substrate, resulting in uneven internal structure and reduced overall density of the deposited layer, making it difficult to meet the stringent requirements of high-performance electronic devices for target material composition consistency and phase structure. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides an intelligent powder mixing and spraying method and system based on CrSi target material. This solves the problem that when preparing CrSi target material using existing plasma spraying technology, the significant difference in the thermophysical properties of chromium and silicon leads to uncontrollable vaporization loss of silicon powder, resulting in a serious deviation of the final target material composition from the preset deposition atomic ratio.

[0006] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides an intelligent powder mixing and spraying method based on CrSi target material, employing the following technical solution: Take chromium powder and silicon powder, start the plasma generator to generate a plasma jet, inject the chromium powder into the core area of ​​the plasma jet through the main powder feeding port, and inject the silicon powder into the evolution area of ​​the plasma jet through the auxiliary powder feeding port. The auxiliary powder feeding port is located downstream of the main powder feeding port. In the initial state, argon gas is introduced into the auxiliary powder feeding port as a carrier gas, and the silicon powder is delivered at a preset basic powder feeding rate. The transient temperature of the deposition zone surface is continuously collected using an infrared pyrometer, and the temperature deviation between the transient temperature and the system's preset safe sublimation vaporization threshold temperature is calculated in real time. When the transient temperature is determined to be greater than the safe sublimation vaporization threshold temperature, the main arc power of the plasma generator is kept constant, hydrogen is dynamically mixed into the argon gas introduced into the auxiliary powder feeding port, and the instantaneous powder feeding rate of the silicon powder is increased simultaneously. The deposited target material obtained after spraying and deposition is placed in a vacuum environment for heating and annealing, and then cooled to obtain CrSi target material.

[0007] By adopting the above technical solution, and due to the use of a multi-flow field spatial decoupling and gas-powder linkage dynamic intervention mechanism, the following effects are achieved: Step one achieves spatial decoupling of the thermodynamic enthalpy field. High-melting-point chromium powder is injected into the jet core region with a high heat flux density to ensure instantaneous melting; at the same time, easily vaporized silicon powder is injected into the relatively low-temperature jet evolution region to avoid excessive thermal shock to the silicon powder in the initial stage.

[0008] Steps two and three synergistically construct a closed loop for in-situ chemical cooling and mass repair based on transient thermal load. This loop contains two core reaction stages and a compensation mechanism: The first reaction stage involves the endothermic in-situ dissociation of hydrogen molecules. When the temperature overshoots, the hydrogen gas mixed into the system enters the high-temperature evolution region, undergoing a diatomic molecular bond-breaking and dissociation reaction.

[0009] This dissociation process absorbs a large amount of latent heat, forming a heat-absorbing and cooling layer around the microscopic flow field of silicon powder, rapidly suppressing the local thermodynamic temperature, and blocking the exponential sublimation and vaporization of silicon powder through chemical pathways.

[0010] The second stage of the reaction involves the exothermic recombination of hydrogen atoms at the interface. As the molten silicon droplets impact the relatively low-temperature deposition zone surface, free hydrogen atoms undergo a reverse recombination reaction at the liquid chromium-silicon solidification interface. The heat released by this reaction provides secondary in-situ heating to the initial solidified liquid phase interface, reducing the surface tension of the interface and promoting the homogeneous distribution of the two-phase droplets to improve the density of the target material.

[0011] The quality compensation mechanism compensates for the minute aerodynamic vaporization losses that have occurred during the intervention response delay period by simultaneously increasing the instantaneous powder feeding rate of silicon powder, thus maintaining the atomic ratio in the final coating.

[0012] Step four utilizes vacuum thermal driving force to eliminate free hydrogen atoms dissolved or adsorbed at grain boundaries during the deposition process, thus eliminating the risk of hydrogen embrittlement.

[0013] Preferably, the purity of the chromium powder is not less than 99.95%, and the median diameter is 15.0 μm-45.0 μm; the purity of the silicon powder is not less than 99.999%, and the median diameter is 10.0 μm-30.0 μm; the deposition atomic ratio of the chromium powder to the silicon powder is set to 1:1-1:4.

[0014] By adopting the above technical solution and setting a specific narrow-band particle size distribution, powders with different heat capacities can achieve synchronous melting in their respective enthalpy fields. The finer silicon powder has a large specific surface area and can quickly absorb heat and melt in the shorter residence time in the evolution zone, while the coarser chromium powder can resist extremely strong heat flow in the core region without excessive vaporization. The particle size of the two is matched with the characteristics of their respective enthalpy fields.

[0015] Preferably, the main arc power of the plasma generator is set to 35.0kW-55.0kW; the auxiliary powder feed port is located 20.0mm-45.0mm downstream of the main powder feed port, so that the axial average thermodynamic temperature of the evolution zone is between 2500K-4000K; and the safe sublimation vaporization threshold temperature is set between 1073K-1273K.

[0016] By adopting the above technical solution, the optimal thermodynamic window for CrSi target preparation was defined. This axial distance parameter ensures that the evolution zone temperature meets both the latent heat of melting requirements of silicon powder and, through the setting of the hydrogen dissociation critical temperature, allows for the immediate initiation of an endothermic dissociation reaction upon the introduction of hydrogen gas. The safe sublimation vaporization threshold temperature is set based on the inflection point of the silicon material's saturated vapor pressure curve, constituting a precise critical point for initiating cooling intervention.

[0017] Preferably, the instantaneous mixing volume flow rate of hydrogen is dynamically adjusted by a proportional-integral closed-loop control algorithm. The value of the instantaneous mixing volume flow rate is the sum of the first product of the temperature deviation value and the preset proportional coefficient, and the second product of the integral value of the temperature deviation value during the continuous overheating period and the preset integral coefficient. The improved instantaneous powder feeding rate of the silicon powder is the sum of the base powder feeding rate and the third product of the temperature deviation value and the preset mass loss compensation coefficient. When it is determined that the transient temperature is not greater than the safe sublimation vaporization threshold temperature, the mixing of hydrogen is stopped and the basic powder feeding rate is restored.

[0018] By adopting the above technical solution, a continuous compensation logic is established. The proportional adjustment term directly responds to sudden local overheating peaks, determining the instantaneous rapid cooling amplitude; The integral adjustment term continuously accumulates the temperature deviation over time to offset the macroscopic heat accumulation and baseline temperature drift caused by prolonged heating of the substrate. When the temperature drops back to a safe range, the system stops intervening and restores the initial reference powder feeding state to prevent overcooling from causing unmelted powder inclusions, thus forming a complete logic control closed loop.

[0019] Preferably, the operating vacuum pressure of the vacuum environment is no greater than 0.0005 Pa, and the heating temperature of the heating annealing treatment is 450℃-550℃.

[0020] By adopting the above technical solution, the extremely low vacuum pressure and medium-temperature heating conditions create a strong concentration gradient and thermodynamic driving force inside and outside the target material, which promotes the rapid diffusion and escape of the remaining highly active free hydrogen atoms along the grain boundary after the violent hydrogen dissociation reaction, ensuring the minimization of the insulating impurity content of the target material.

[0021] Secondly, the present invention provides an intelligent powder mixing and spraying system based on CrSi target material, which adopts the following technical solution: It includes a dual-zone jetting module, a powder supply module, a carrier gas modulation module, a status monitoring module, and a control module; the dual-zone jetting module includes a plasma generator, a main powder supply port disposed at the root of the nozzle of the plasma generator, and a secondary powder supply port disposed in the evolution zone of the plasma jet, the secondary powder supply port being located downstream of the main powder supply port; The powder supply module includes a first weightless spiral powder feeder connected to the main powder feed port and a second weightless spiral powder feeder connected to the auxiliary powder feed port; the carrier gas modulation module includes a first argon mass flow meter, a second argon mass flow meter, a hydrogen mass flow meter, and a mixed flow profiler. The output end of the first argon mass flow meter is connected to the main powder inlet, the output ends of the second argon mass flow meter and the hydrogen mass flow meter are respectively connected to the input end of the mixed flow profiler, and the output end of the mixed flow profiler is connected to the auxiliary powder inlet; The status monitoring module includes an infrared pyrometer for non-contact temperature measurement of the deposition zone surface to obtain transient temperature; the control module is electrically connected to the first weightless spiral powder feeder, the second weightless spiral powder feeder, the hydrogen mass flow meter, and the infrared pyrometer.

[0022] By adopting the above technical solution, a closed-loop data communication system is established between the gas path, powder path, and temperature monitoring information in the hardware architecture. The mixed flow profiler ensures uniform mixing of the inert carrier gas and the reducing cooling gas before entering the auxiliary powder feed port, and the weightless spiral powder feeder provides millisecond-level mass output response capability. The entire system separates and injects complex spatial multiphase flows, providing a rigorous execution platform for achieving dynamic temperature control.

[0023] Preferably, the carrier gas modulation module is equipped with a limiting protection program, which controls the upper limit of the instantaneous mixed hydrogen volume flow rate output by the hydrogen mass flow meter to not exceed 15.0 SLPM when the control module issues a command to mix in hydrogen.

[0024] By adopting the above technical solutions, the output command may exceed the limit due to the temperature not dropping below the threshold for an extended period during the algorithm's integration phase. Limiting the upper limit of hydrogen flow rate can prevent an excessively high proportion of diatomic gases in the mixed gas, thus preventing overall arc interruption of the plasma jet and potential equipment safety hazards.

[0025] Preferably, the infrared pyrometer is a dual-color infrared pyrometer, and the temperature response sampling frequency of the dual-color infrared pyrometer is not less than 100Hz. The dual-color infrared pyrometer is used to input the transient temperature to the control module in real time.

[0026] By adopting the above technical solution, the influence of strong arc light interference from the plasma jet and fluctuations in the emissivity of the molten pool surface on the temperature measurement results is eliminated using the colorimetric thermometry principle. The high-frequency sampling frequency meets the data density acquisition requirements for microscopic thermal field changes under transient turbulent impact.

[0027] Preferably, the control module is an industrial programmable logic controller (PLC). The PLC has a pre-set proportional-integral (PI) control algorithm model. The PLC is used to synchronously adjust the output of the second weightless spiral feeder and the hydrogen mass flow meter based on the temperature deviation between the transient temperature and the preset safe sublimation vaporization threshold temperature.

[0028] By adopting the above technical solution, the time alignment operation mechanism built into the industrial programmable logic controller can keep the discrete high-frequency temperature measurement data synchronized with the system scan cycle at zero order, ensuring that the input of the calculation cycle is accurately aligned and avoiding phase lag in the closed-loop control signal.

[0029] Preferably, the auxiliary powder feed port is mounted on the external support of the plasma generator via an axial precision displacement stage, so that the auxiliary powder feed port can be moved and adjusted along the axial direction of the plasma jet.

[0030] By adopting the above technical solution, the injection position of the second phase powder can be changed from a purely mechanical perspective to target different power settings and material particle size requirements, so that it can be targeted into a preset specific thermodynamic temperature evolution range.

[0031] This invention provides an intelligent powder mixing and spraying method and system based on CrSi target material. It has the following beneficial effects: 1. This invention injects high-melting-point chromium powder into the core region of the plasma jet and easily vaporized silicon powder into the relatively low-temperature evolution region, so that powders with different thermophysical properties are independently heated in their respective matched spatial enthalpy fields, thereby avoiding uncontrollable initial aerodynamic vaporization loss of silicon powder due to high heat flow impact during co-spraying.

[0032] 2. In this invention, hydrogen is dynamically mixed into the carrier gas at the auxiliary powder feed port when the transient temperature of the deposition zone is detected to be greater than the safe sublimation vaporization threshold temperature, and the instantaneous powder feeding rate of silicon powder is increased simultaneously. The hydrogen molecules absorb latent heat by undergoing a dissociation reaction in the high-temperature zone to achieve in-situ cooling of the micro-flow field, while positively compensating for the mass loss caused by the high temperature. Therefore, it can suppress the sublimation of silicon material and maintain the final atomic ratio of the target material.

[0033] 3. This invention utilizes the reverse recombination reaction of dissociated free hydrogen atoms at the solidification interface of the target material to release heat and promote the homogeneous distribution of the two-phase droplets. Furthermore, the deposited target material is placed in a vacuum environment for heating and annealing. The vacuum thermal gradient driving force is used to forcibly remove the free hydrogen remaining at the grain boundary, thereby improving the density of the target material structure and eliminating hydrogen embrittlement defects caused by residual heterogeneous gases. Attached Figure Description

[0034] Figure 1 This is a structural block diagram of the intelligent powder mixing and spraying system of the present invention; Figure 2 This is a flowchart of the steps of the intelligent powder mixing and spraying method of the present invention. Detailed Implementation

[0035] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be noted that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0037] See attached document Figure 1 The intelligent powder mixing and spraying system provided by this invention is mainly composed of a dual-zone spraying module, a powder supply module, a carrier gas modulation module, a status monitoring module, and a control module. These modules are interconnected via air paths, powder paths, and electrical signal transmission lines.

[0038] The dual-zone jet module is used to establish a spatial enthalpy field with a temperature gradient. It includes a plasma generator, a main powder feed port, and a secondary powder feed port. In this embodiment, the plasma generator produces a high-temperature plasma jet that gradually decreases in temperature from the center outwards and from the outlet downstream. As a preferred embodiment, the main powder feed port is located at the root of the plasma generator nozzle. Since this location corresponds to the core region of the plasma jet and has a high heat flux density, it can ensure that high-melting-point components melt instantly.

[0039] As the plasma jet propagates downstream, it forms an evolution zone with gradually decreasing temperature. The secondary powder feed port is located within this evolution zone, downstream of the main powder feed port. Due to the significant temperature gradient within the evolution zone, the secondary powder feed port is mounted on an external support of the plasma generator via an axial precision displacement stage. This assembly structure allows the secondary powder feed port to be moved and adjusted along the axial direction of the plasma jet, thus enabling it to feed plasma within a specific range where the axial average thermodynamic temperature is between 2500K and 4000K.

[0040] The powder supply module is responsible for conveying powder raw materials to the aforementioned dual-zone injection module. It includes a first loss-in-weight screw feeder connected to the main powder inlet and a second loss-in-weight screw feeder connected to the auxiliary powder inlet. Due to the high requirements for feeding accuracy of the target material composition, the loss-in-weight screw feeder is equipped with a weighing sensor and a closed-loop speed-regulating motor, which can change the speed of the screw in real time according to the external electrical signal to maintain or dynamically adjust the instantaneous mass delivery rate of the powder.

[0041] The carrier gas modulation module provides the powder transport power to the powder supply module and performs chemical flow field intervention in specific areas. This module includes a first argon mass flow meter, a second argon mass flow meter, a hydrogen mass flow meter, and a mixed flow profiler. The output of the first argon mass flow meter is directly connected to the main powder inlet, providing a single inert carrier gas to the core area. To achieve dynamic cooling intervention in the evolution zone, the outputs of the second argon mass flow meter and the hydrogen mass flow meter are respectively connected to the input of the mixed flow profiler. The mixed flow profiler has a static mixing channel inside to uniformly mix the two gases, and its output is connected to the auxiliary powder inlet. Each mass flow meter contains a thermal flow sensor and a proportional solenoid valve, which adjusts the valve opening by receiving standard analog signals.

[0042] The condition monitoring module includes an infrared pyrometer for non-contact temperature measurement of the deposition zone surface. Considering the strong interference from the plasma jet arc and the emissivity variations on the molten pool surface, a dual-color infrared pyrometer is specifically used. This dual-color infrared pyrometer calculates the temperature by measuring the ratio of the radiant energy of two adjacent wavelengths, and its temperature response sampling frequency is no less than 100Hz to meet the data density requirements for acquiring transient temperatures.

[0043] The control module is the central component of the system, specifically an industrial programmable logic controller (PLC). This PLC has analog input and output ports, which are electrically connected to the first and second loss-in-weight spiral feeders, a hydrogen mass flow meter, and a dual-color infrared pyrometer. The dual-color infrared pyrometer inputs real-time transient temperature data of the deposition zone surface to the PLC.

[0044] To control the thermodynamic state of the evolution zone and avoid a disconnect between the theory and the pure mathematical model, the principle of the intervention mechanism needs to be clearly defined beforehand. During plasma spraying, the heat accumulation in the substrate region does not increase linearly, but exhibits strong transient fluctuations accompanied by turbulent impacts. Therefore, this embodiment does not employ simple on / off control, but introduces continuous compensation logic that includes proportional and integral dimensions. The proportional adjustment specifically addresses sudden local overheating peaks, while the integral adjustment is used to offset the long-term baseline temperature drift caused by the absorption of heat from the overall heat capacity of the substrate.

[0045] Industrial programmable logic controllers (PLCs) have pre-set proportional-integral (PI) control algorithm models based on the aforementioned principles. Considering the asynchronous nature of multi-source data, this model incorporates time alignment logic to maintain zero-order synchronization between the discrete temperature measurement data input from the dual-color infrared pyrometer at a frequency of 100Hz and the control module's own cyclic scanning cycle, which is typically 10ms, ensuring that the input quantities are aligned within each calculation cycle.

[0046] Based on data synchronization, this model uses the transient temperature transmitted by a dual-color infrared pyrometer as a feedback variable and retrieves the safe sublimation vaporization threshold temperature pre-stored in an internal register. Based on this, the algorithm model calculates the temperature deviation between the transient temperature and the safe sublimation vaporization threshold temperature in real time. Through a specific discretized control relationship, the industrial programmable logic controller converts the processed calculation results into control signals, which are synchronously output to the drive circuit of the second weightless spiral powder feeder and the proportional solenoid valve of the hydrogen mass flow meter, thereby synchronously adjusting the instantaneous powder feeding rate of silicon powder and the output of hydrogen. The specific hardware-modulated control relationship involved in the above algorithm model is as follows:

[0047]

[0048] In the formula, Indicates the current discrete sampling period number; This indicates the computational step size period of the algorithm model.

[0049] This indicates the number of data collected and synchronized by the dual-color infrared pyrometer. The transient temperature of the period; This represents the system's preset safe sublimation vaporization threshold temperature, which is set within the range of 1073K-1273K. This range is determined based on the saturated vapor pressure curve of silicon material. Within this temperature range, the microscopic sublimation rate of the silicon material surface begins to increase exponentially, thus serving as the safe critical point for triggering flow field cooling. Indicates the first Temperature deviation value over a period of time; This indicates the instantaneous mixed volume flow rate of hydrogen output by the hydrogen mass flow meter. Its physical purpose is to induce a diatomic molecule bond breaking endothermic reaction by injecting hydrogen, forming an in-situ chemical cooling shield to rapidly reduce the temperature of the micro-flow field. This represents the preset proportionality coefficient, whose value is preset based on the molar latent heat equivalent of hydrogen dissociation and the volumetric specific heat capacity of the local flow field around the silicon droplet. This represents the preset integral coefficient, used to compensate for the macroscopic thermal accumulation effect between the deposited coating and the substrate during long-term spraying. This indicates that the second loss-in-weight spiral feeder is in the first... Instantaneous powder feeding rate of silicon powder during cycle output; This indicates the system's preset basic silicon powder feeding rate; This represents the preset mass loss compensation coefficient. Since even with the hydrogen cooling shield activated, it is impossible to completely suppress the slight burn-off caused by the plasma jet, this coefficient is used to positively compensate for this part of the irreversible aerodynamic vaporization loss. This represents the step function, which is 1 when triggered by continuous overheating and 0 otherwise.

[0050] The carrier gas modulation module is equipped with a limit protection program, which is embedded in the operation logic of the industrial programmable logic controller.

[0051] When using discrete integral calculation, if the temperature does not drop below the threshold for a long time, the integral term will continue to accumulate, causing the control quantity to exceed the limit.

[0052] To address this issue, the algorithm incorporates internal anti-integral saturation processing logic, which pauses integration when the output reaches the limit value. On the other hand, the program forcibly controls the upper limit of the instantaneous mixed volume flow rate of hydrogen output by the hydrogen mass flow meter to be no more than 15.0 SLPM, thereby avoiding the instability caused by excessive hydrogen ratio leading to overall arc interruption of the plasma jet, or even causing equipment safety hazards.

[0053] For the arc ignition control principle of plasma generators and the basic setup of communication buses in industrial programmable logic controllers, those skilled in the art can use conventional industrial automation integration solutions.

[0054] Preparation Example 1: This preparation example provides a method for preparing raw material powder for spraying CrSi target material, including the following steps: S101 uses commercially available high-purity chromium powder with a purity of not less than 99.95% and commercially available high-purity polycrystalline silicon powder with a purity of not less than 99.999% as initial raw materials.

[0055] S102, the initial raw materials are screened for particle size using an air classifier protected by inert gas. After multi-stage cyclone separation and interception, the median diameter of the obtained chromium powder is controlled to 15.0 μm, and the median diameter of the obtained silicon powder is controlled to 10.0 μm.

[0056] Based on this particle size setting, the powder has an extremely high specific surface area, enabling it to rapidly absorb heat and reach a molten state within a very short jet residence time.

[0057] S103. The sieved chromium powder and silicon powder are placed separately in a vacuum drying oven. They are baked continuously for 4 hours in a vacuum environment with an absolute pressure of less than 100 Pa and a temperature set at 120°C to remove adsorbed water and trace amounts of volatile organic compounds from the powder surface, thereby ensuring that the powder maintains excellent flowability in the subsequent weightless spiral feeder.

[0058] S104, the deposition atomic ratio of chromium powder to silicon powder is set to 1:1. Since the theoretical molar mass of chromium is approximately 52.0 g / mol and the theoretical molar mass of silicon is approximately 28.1 g / mol, based on this deposition atomic ratio, the theoretical mass supply ratio of chromium powder to silicon powder is calculated to be approximately 1.85:1.

[0059] After determining the final basic powder feeding quality benchmark by combining the estimated single-component deposition efficiency, the dried chromium powder and silicon powder are separated and packaged separately to provide standardized raw materials for the dual-zone independent powder supply module.

[0060] Preparation Example 2: This preparation example provides a method for preparing raw material powder for spraying CrSi target material, including the following steps: S201, obtain high-purity chromium powder with a purity of not less than 99.95%, and high-purity silicon powder with a purity of not less than 99.999%.

[0061] S202, the obtained powder was subjected to narrow-band particle size distribution control using an ultrasonic vibrating screen. After sieving, the median diameter of the collected chromium powder was 30.0 μm, and the median diameter of the silicon powder was 20.0 μm.

[0062] In this embodiment, this particle size setting can avoid the aerodynamic rebound effect of ultrafine powders, while preventing the unmelted defects of coarse particles.

[0063] S203 involves separately loading chromium powder and silicon powder of specific particle sizes into a double-cone rotary vacuum dryer for dynamic dehydration. The equipment operates continuously at 80°C, allowing the powder to be uniformly degassed while tumbling, further improving the consistency of its loose packing density.

[0064] S204, based on the application requirements of silicon-rich phase targets for specific semiconductor devices, sets the target deposition atomic ratio to 1:2.5.

[0065] After molar mass conversion, the theoretical mass supply ratio of chromium powder to silicon powder is approximately 1:1.35.

[0066] After the proportioning calculation is completed, the chromium powder that has been processed above is packaged in the first powder storage tank for use by the main powder delivery port, and the silicon powder is packaged in the second powder storage tank for use by the auxiliary powder delivery port. The entire packaging process is completed in an argon glove box to isolate secondary pollution from ambient oxygen.

[0067] Preparation Example 3: This preparation example provides a method for preparing raw material powder for spraying CrSi target material, including the following steps: S301 directly uses crystalline chromium powder with a purity of not less than 99.95% and semiconductor-grade silicon powder with a purity of not less than 99.999%.

[0068] S302 uses mechanical sieving to trap large particles, resulting in a median diameter of 45.0 μm for chromium powder and 30.0 μm for silicon powder in the final feed. The larger particle size forces the droplets to absorb more latent heat during flight, thus providing a natural thermodynamic buffering capacity in strong enthalpy fields.

[0069] S303 involves placing the prepared coarse-particle chromium powder and silicon powder into a vacuum heating furnace for pretreatment. Simultaneously, pulsed microwave heating is applied, causing the deep moisture within the capillaries of the particles to expand and escape, thus eliminating the risk of droplet explosion and splashing caused by moisture vaporization during the high-temperature spraying stage.

[0070] S304 establishes the limiting deposition atomic ratio of chromium powder to silicon powder as 1:4.

[0071] After molar mass conversion, the theoretical mass supply ratio of chromium powder to silicon powder is approximately 1:2.16.

[0072] Under this ratio setting, the batch weight of the packaged powder is recorded to establish the initial data file of the powder supply module. Example

[0073] See attached document Figure 2 This embodiment provides a smart powder mixing spraying method based on CrSi target material. It is implemented using the smart powder mixing spraying system in System Example 1 and the raw materials in Preparation Example 2, and includes the following steps: Obtain the chromium powder and silicon powder that have undergone pretreatment in Preparation Example 2. At this time, the median diameter of the chromium powder is 30.0 μm, the median diameter of the silicon powder is 20.0 μm, and the target deposition atomic ratio of the chromium powder and silicon powder is set to 1:2.5.

[0074] The plasma generator is activated to produce a plasma jet, and the main arc power of the plasma generator is set to 45.0 kW. The system injects chromium powder into the core region of the plasma jet through the main powder feed port, allowing the high-melting-point chromium powder to completely melt under extremely high heat flux density.

[0075] To prevent excessive burning of low-melting-point silicon powder in the core region, the silicon powder is injected into the evolution zone of the plasma jet through a secondary powder feed port. In this embodiment, the secondary powder feed port is located 30.0 mm downstream of the main powder feed port, so that the axial average thermodynamic temperature of the evolution zone is approximately 3200 K.

[0076] In the initial state, only high-purity argon gas is introduced into the auxiliary powder feeding port as the carrier gas, and the initial rotation speed of the first and second weightless spiral powder feeders is controlled according to the theoretical mass powder supply ratio of approximately 1:1.35 calculated in Preparation Example 2, so as to transport chromium powder and silicon powder respectively at the preset basic powder feeding rate.

[0077] During the process of plasma jet carrying molten droplets impacting the substrate to form a coating, the transient temperature of the deposition area surface is continuously collected using a dual-color infrared pyrometer at a sampling frequency of 100Hz.

[0078] The industrial programmable logic controller (PLC) acquires the transient temperature in real time and calculates the temperature deviation between the transient temperature and the system's preset safe sublimation vaporization threshold temperature. Based on the process heat load of this embodiment, the safe sublimation vaporization threshold temperature is set to 1173K.

[0079] Based on the above online analysis results, when the transient temperature is determined to be greater than 1173K, the control system maintains the main arc power of the plasma generator unchanged to avoid the phenomenon of unmelted inclusions of chromium powder caused by a sudden drop in power.

[0080] Based on this constant power premise, the industrial programmable logic controller synchronously sends instructions to the carrier gas modulation module to dynamically mix hydrogen into the argon gas introduced into the auxiliary powder feed port. The instantaneous mixing volumetric flow rate of hydrogen is dynamically adjusted through a built-in proportional-integral closed-loop control algorithm. The specific execution logic is as follows: The instantaneous mixed-in volumetric flow rate is obtained by adding the first product of the temperature deviation value and a preset proportional coefficient, and the second product of the integral value of the temperature deviation value over the continuous overheating period and a preset integral coefficient, and output to the hydrogen mass flow meter. By mixing in hydrogen, the latent heat absorbed by the diatomic dissociation reaction of hydrogen in the 3200K evolution region is utilized to perform in-situ cooling and quenching of the local micro-flow field of silicon powder, thereby suppressing the overheating and sublimation of silicon powder.

[0081] Based on this cooling intervention, to compensate for the aerodynamic vaporization losses caused by the instantaneous high temperature, the control system synchronously increases the instantaneous powder delivery rate of the silicon powder. The increased instantaneous powder delivery rate is obtained through the following logical calculation: The basic silicon powder feeding rate is added to the third product of the temperature deviation value and the preset mass loss compensation coefficient to dynamically maintain a final deposition atomic ratio of 1:2.5, preventing the coating composition from deviating from chromium enrichment. When the dual-color infrared pyrometer detects a transient temperature of no more than 1173K, the system immediately stops mixing hydrogen and restores the basic powder feeding rate.

[0082] During the spraying process described above, atomic hydrogen generated by the thermal dissociation of hydrogen gas is impacted onto the surface of the deposition zone along with silicon powder droplets. Since the temperature of the deposition zone surface is much lower than the dissociation temperature of hydrogen gas, the atomic hydrogen undergoes a reverse recombination reaction at the initially condensed liquid chromium-silicon interface, releasing heat. This recombination heat can provide secondary in-situ heating of the liquid phase interface, reducing the surface tension of the interface and promoting the homogeneous distribution of the two-phase droplets.

[0083] The deposited target material obtained after spraying deposition is placed in the vacuum environment of an annealing furnace for heating and annealing. The vacuum pump group is turned on to maintain the operating vacuum pressure at 0.0001 Pa, and the heating temperature is set to 500℃.

[0084] Driven by both thermodynamics and vacuum gradient, trace amounts of free hydrogen atoms remaining in the lattice during deposition diffuse along the grain boundaries to the surface and are removed, eliminating the risk of hydrogen embrittlement in the target material. After heat treatment, the material is cooled in the furnace, ultimately yielding a highly dense CrSi target material free of insulating impurities.

[0085] Example 2: This example provides a smart powder mixing spraying method based on CrSi target material, implemented using the fine-particle-size raw material prepared in Preparation Example 1, including the following steps: The raw materials from Preparation Example 1 (median diameter of chromium powder 15.0 μm, median diameter of silicon powder 10.0 μm, deposition atomic ratio 1:1) were used. The plasma generator was started and the main arc power was set to 35.0 kW. Chromium powder was injected into the jet core region through the main powder inlet.

[0086] The auxiliary powder feed port is adjusted to be 45.0 mm downstream of the main powder feed port, so that the axial average thermodynamic temperature of the cross-sectional evolution zone is in the lower limit range of about 2500 K. In the initial state, argon gas is introduced into the auxiliary powder feed port as a carrier gas, and the initial feeding is performed according to the theoretical mass powder supply ratio of about 1.85:1, and silicon powder is conveyed at the basic powder feeding rate.

[0087] The transient temperature of the deposition zone surface is continuously collected using a dual-color infrared pyrometer, and the temperature deviation between this temperature and the system's preset safe sublimation vaporization threshold temperature is calculated in real time. Due to the relatively small plasma heat input in this embodiment, the safe sublimation vaporization threshold temperature is set to 1073 K.

[0088] When the transient temperature exceeds 1073 K, hydrogen is dynamically mixed into the argon gas introduced into the auxiliary powder feed port under a constant main arc power of 35.0 kW. The control module uses the sum of the first and second products resulting from the temperature deviation as the instantaneous hydrogen mixing volume flow rate control signal, based on the proportional-integral control algorithm model.

[0089] Simultaneously, the sum of the base powder feeding rate and the third product is used as the improved instantaneous silicon powder feeding rate. This gas-powder bidirectional linkage compensation mechanism achieves protection and quality restoration in lower temperature flow fields. When the transient temperature is determined to be no greater than 1073K, hydrogen mixing is stopped.

[0090] The deposited target material is placed in an annealing furnace and subjected to heating annealing at a heating temperature of 450°C under an operating vacuum pressure of no more than 0.0005 Pa. After cooling, the CrSi target material is obtained. Example

[0091] This embodiment provides a smart powder mixing and spraying method based on CrSi target material, implemented using the coarse-particle-size silicon-rich raw material prepared in Preparation Example 3, and includes the following steps: The raw materials from Preparation Example 3 (median diameter of chromium powder 45.0 μm, median diameter of silicon powder 30.0 μm, deposition atomic ratio 1:4) were extracted. The main arc power of the plasma generator was increased to 55.0 kW to generate a high-energy jet. Coarse-grained chromium powder was injected into the main powder inlet to ensure that it was heat-absorbing and melted through in a high enthalpy field.

[0092] The auxiliary powder feeder is moved to a position 20.0 mm downstream of the main powder feeder using an axial precision displacement stage. At this point, the axial average thermodynamic temperature of the evolution zone reaches approximately 4000 K.

[0093] In the initial stage, argon gas is used and silicon powder is transported into the evolution zone according to a theoretical mass powder supply ratio of approximately 1:2.16.

[0094] Transient temperature is continuously acquired using a dual-color infrared pyrometer. Due to the heat accumulation on the substrate caused by the high-energy jet, the system's safe sublimation vaporization threshold temperature is set to the upper limit of 1273K, and the deviation between the actual temperature and this threshold is calculated in real time.

[0095] Once the transient temperature exceeds 1273K, the system immediately triggers the hydrogen dissociation cooling shield while maintaining a constant power of 55.0kW. Based on the temperature deviation, the industrial programmable logic controller outputs the sum of the first and second products to adjust the instantaneous hydrogen mixing volume flow rate, while using the sum of the basic powder feeding rate and the third product as the improved silicon powder feeding rate.

[0096] The extremely high temperature evolution zone causes the injected hydrogen to undergo an extremely violent bond-breaking endothermic reaction, significantly suppressing the local thermodynamic temperature of the flow field and preventing the catastrophic vaporization loss of a large amount of excess silicon powder. As the transient temperature drops to 1273K or below, the system stops mixing hydrogen and adjusts the powder feeding rate.

[0097] The silicon-rich spray-deposited target was placed in a vacuum annealing furnace. Under an extremely high vacuum pressure of 0.00005 Pa, the heating temperature was raised to 550 °C for isothermal purification. This deep vacuum and high temperature provided a very strong concentration gradient driving force, which forced the free hydrogen remaining between the grain boundaries of the high-ratio silicon phase after the violent hydrogen dissociation reaction to be removed. After cooling, a CrSi target was obtained.

[0098] Comparative Example 1: Compared with Example 1, the difference is that this comparative example did not adopt the dual-zone powder feeding and dynamic gas adjustment cooling mechanism. Specifically, after the chromium powder and silicon powder were pre-mixed, they were all injected into the core area of ​​the plasma jet from the main powder feeding port of the plasma generator. Furthermore, no closed-loop temperature judgment was performed using an infrared pyrometer during the entire spraying process, no hydrogen was mixed into the carrier gas, and the powder feeding rate of silicon powder was not dynamically increased. Everything else was the same.

[0099] Comparative Example 2: Compared with Example 1, the difference is that when the transient temperature of the deposition zone surface is determined to be greater than the safe sublimation vaporization threshold temperature (1173K), this comparative example only dynamically increases the flow rate of high-purity argon gas into the carrier gas introduced into the auxiliary powder feed port in an attempt to cool it down, without mixing hydrogen gas into it, so as not to trigger the in-situ chemical cooling shield effect of hydrogen diatomic bond breaking and dissociation endothermic reaction. All other aspects are the same.

[0100] Comparative Example 3: Compared with Example 1, the difference is that when the transient temperature of the deposition zone surface is determined to be greater than the safe sublimation vaporization threshold temperature (1173K), this comparative example only dynamically mixes hydrogen into the argon gas introduced into the auxiliary powder feeding port to quench and cool the flow field, but does not simultaneously increase the instantaneous powder feeding rate of the silicon powder to compensate for the positive mass loss of aerodynamic vaporization. All other aspects are the same.

[0101] Comparative Example 4: Compared with Example 1, the difference is that after the deposited target material was obtained by spraying and deposition, the deposited target material was not placed in a vacuum environment for heating and annealing, but was directly cooled naturally in the ambient atmosphere and at room temperature. All other aspects are the same.

[0102] Test example: To verify the engineering effectiveness of the intelligent powder mixing and spraying method based on CrSi target material provided by this invention, the physicochemical properties and electrical properties of the CrSi target material products prepared in Examples 1-3 and Comparative Examples 1-4 were characterized. The testing process included the following steps: Wire-cut samples were taken along the thickness direction of each target material, and metallographic specimens were prepared by epoxy resin embedding, rough grinding, fine grinding, and polishing. The microstructure of the specimen cross-section was observed using a scanning electron microscope in backscattered electron mode. Ten different fields of view were randomly selected, and the area ratio of dark-colored pore regions in the total field of view was calculated using image analysis software. The arithmetic mean of the ten fields of view was taken as the macroscopic porosity of the target material.

[0103] Five sampling points were evenly selected on the surface of the working area of ​​each target material, and powder was extracted using a micro-drill. The powder samples were then microwave-digested in a mixed acid solution of nitric acid and hydrofluoric acid. After volume adjustment, the mass concentrations of Cr and Si elements in the solution were determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). The actual atomic ratio of Cr to Si was calculated based on the mass concentrations, and the relative deviation rate of the Si proportion in this actual atomic ratio compared to the target values ​​set for each embodiment and comparative example was calculated.

[0104] Small samples, each weighing approximately 1.0 g, were cut from the target material of each group. After surface cleaning and degreasing, the samples were placed in the graphite crucible of an inert gas melting-infrared absorption analyzer. The samples were melted by high-temperature pulse heating under a helium carrier gas flow. The mass fraction of hydrogen in the released gas was determined by infrared detection, thus obtaining the microscopic hydrogen content inside the target material.

[0105] Sixteen test nodes were planned along concentric circles and cross paths on the effective sputtering surface of the entire target material. A four-probe resistivity meter was used to measure the sheet resistance of the surface at each node and convert it to resistivity. The standard deviation of the resistivity data for these 16 nodes was calculated and divided by the average value to obtain the resistivity non-uniformity, which reflects the macroscopic electrical consistency of the target material.

[0106] The experimental data obtained from the above testing phases are summarized in Table 1.

[0107] Table 1. Test results of comprehensive performance of CrSi sputtering materials prepared in each embodiment and comparative example

[0108] in conclusion: According to the data in Table 1, Comparative Example 1 used single-tube premixed injection spraying. Due to the much higher melting point of Cr compared to Si, the high enthalpy in the plasma jet core region caused large-scale boiling and vaporization of low-boiling-point Si, resulting in a Si element deviation rate of -28.64%. Simultaneously, Cr failed to form a continuous molten network, leading to high macroscopic porosity and extremely uneven resistivity. Examples 1 to 3, through decoupled injection in a main and auxiliary dual-zone system, bypassed the core region and injected Si powder into the evolution zone with a decreasing temperature gradient. This mitigated Si burn-off from a spatial fluid dynamics perspective, controlling the porosity below 1.2%.

[0109] Comparing the data from Example 1 and Comparative Example 2, it can be seen that when overheating occurs in the evolution zone, simply increasing the argon flow rate has a limited effect on cooling by specific heat capacity. The Si element deviation rate in Comparative Example 2 still shows a deviation of -12.37%. Example 1 uses a proportional-integral closed-loop algorithm that introduces hydrogen gas when the temperature threshold is triggered, utilizing the diatomic bond-breaking reaction that occurs in a flow field at 3000K. This latent heat of chemical dissociation extracts heat from the microscopic local flow field, and its cooling rate and magnitude are superior to the physical cooling of inert gases, keeping the thermodynamic vaporization of Si at a lower level.

[0110] Comparing the data from Example 1 and Comparative Example 3, it can be seen that even with the introduction of a hydrogen dissociation cooling mechanism, the erosion and evaporation of Si by the high-temperature jet cannot be completely avoided; in Comparative Example 3, the Si element still exhibits a negative deviation of -7.56%. In Example 1, while triggering cooling, the system's underlying layer simultaneously converts the temperature deviation into a positive compensation control quantity for the powder feeding motor, dynamically increasing the silicon powder input. By offsetting evaporation losses through the positive intervention of the pneumatic mass flow, Example 1 ultimately converged the Si deviation in the target material composition to -1.41%.

[0111] Comparing the data from Example 1 and Comparative Example 4, it is evident that introducing hydrogen into the plasma working gas leads to the negative effect of hydrogen entering the coating lattice. In Comparative Example 4, due to the omission of post-processing steps, the microscopic hydrogen content within the target material reached as high as 456.8 ppm. Interstitial hydrogen atoms easily form Koch clusters in the target matrix and accumulate at grain boundaries, inducing localized microcracks and causing the resistivity non-uniformity to rise to 7.29%. Example 1, through thermodynamic vacuum driving at 0.0001 Pa and 500°C, caused interstitial hydrogen atoms to escape via diffusion, reducing the final hydrogen content of the target material to within the safe threshold of 12.3 ppm, restoring the electrical consistency of the target material and establishing the closed-loop feasibility of the process technology chain.

Claims

1. A smart powder mixing and spraying method based on CrSi target material, characterized in that, Includes the following steps: Take chromium powder and silicon powder, start the plasma generator to generate a plasma jet, inject the chromium powder into the core area of ​​the plasma jet through the main powder feeding port, and inject the silicon powder into the evolution area of ​​the plasma jet through the auxiliary powder feeding port. The auxiliary powder feeding port is located downstream of the main powder feeding port. In the initial state, argon gas is introduced into the auxiliary powder feeding port as a carrier gas, and the silicon powder is delivered at a preset basic powder feeding rate. The transient temperature of the deposition zone surface is continuously collected using an infrared pyrometer, and the temperature deviation between the transient temperature and the system's preset safe sublimation vaporization threshold temperature is calculated in real time. When the transient temperature is determined to be greater than the safe sublimation vaporization threshold temperature, the main arc power of the plasma generator is kept constant, hydrogen is dynamically mixed into the argon gas introduced into the auxiliary powder feeding port, and the instantaneous powder feeding rate of the silicon powder is increased simultaneously. The deposited target material obtained after spraying and deposition is placed in a vacuum environment for heating and annealing, and then cooled to obtain CrSi target material.

2. The intelligent powder mixing and spraying method based on CrSi target material according to claim 1, characterized in that, The purity of the chromium powder is not less than 99.95%, and the median diameter is 15.0 μm-45.0 μm; The purity of the silicon powder is not less than 99.999%, and the median diameter is 10.0μm-30.0μm; The deposition atomic ratio of the chromium powder to the silicon powder is set to 1:1-1:

4.

3. The intelligent powder mixing and spraying method based on CrSi target material according to claim 1, characterized in that, The main arc power of the plasma generator is set to 35.0kW-55.0kW; The auxiliary powder feeding port is located 20.0mm-45.0mm downstream of the main powder feeding port, so that the axial average thermodynamic temperature of the evolution zone is between 2500K and 4000K. The safe sublimation vaporization threshold temperature is set between 1073K and 1273K.

4. The intelligent powder mixing and spraying method based on CrSi target material according to claim 1, characterized in that, The instantaneous mixing volume flow rate of hydrogen is dynamically adjusted by a proportional-integral closed-loop control algorithm. The value of the instantaneous mixing volume flow rate is the sum of the first product of the temperature deviation value and the preset proportional coefficient, and the second product of the integral value of the temperature deviation value during the continuous overheating period and the preset integral coefficient. The improved instantaneous powder feeding rate of the silicon powder is the sum of the base powder feeding rate and the third product of the temperature deviation value and the preset mass loss compensation coefficient. When it is determined that the transient temperature is not greater than the safe sublimation vaporization threshold temperature, the mixing of hydrogen is stopped and the basic powder feeding rate is restored.

5. The intelligent powder mixing and spraying method based on CrSi target material according to claim 1, characterized in that, The operating vacuum pressure of the vacuum environment is no greater than 0.0005 Pa, and the heating temperature of the heating annealing treatment is 450℃-550℃.

6. A smart powder mixing and spraying system based on CrSi target material, used to implement the smart powder mixing and spraying method based on CrSi target material as described in any one of claims 1-5, characterized in that, include: The dual-zone jet module includes a plasma generator, a main powder feed port located at the root of the nozzle of the plasma generator, and a secondary powder feed port located in the evolution zone of the plasma jet, wherein the secondary powder feed port is located downstream of the main powder feed port. The powder supply module includes a first weightless spiral powder feeder connected to the main powder feeding port and a second weightless spiral powder feeder connected to the auxiliary powder feeding port. The carrier gas modulation module includes a first argon mass flow meter, a second argon mass flow meter, a hydrogen mass flow meter, and a mixed flow profiler. The output end of the first argon mass flow meter is connected to the main powder inlet, the output ends of the second argon mass flow meter and the hydrogen mass flow meter are respectively connected to the input end of the mixed flow profiler, and the output end of the mixed flow profiler is connected to the auxiliary powder inlet; The status monitoring module includes an infrared pyrometer for non-contact temperature measurement of the deposition area surface to obtain transient temperatures; The control module is electrically connected to the first loss-in-weight spiral feeder, the second loss-in-weight spiral feeder, the hydrogen mass flow meter, and the infrared pyrometer, respectively.

7. The intelligent powder mixing and spraying system based on CrSi target material according to claim 6, characterized in that, The carrier gas modulation module is equipped with a limiting protection program. When the control module issues a command to mix in hydrogen, the upper limit of the instantaneous mixed volume flow rate of hydrogen output by the hydrogen mass flow meter is controlled to be no greater than 15.0 SLPM.

8. The intelligent powder mixing and spraying system based on CrSi target material according to claim 6, characterized in that, The infrared pyrometer is a dual-color infrared pyrometer, and the temperature measurement response sampling frequency of the dual-color infrared pyrometer is not less than 100Hz. The dual-color infrared pyrometer is used to input the transient temperature to the control module in real time.

9. The intelligent powder mixing and spraying system based on CrSi target material according to claim 6, characterized in that, The control module is an industrial programmable logic controller (PLC). The PLC has a pre-set proportional-integral (PI) control algorithm model. The PLC is used to synchronously adjust the output of the second weightless spiral powder feeder and the hydrogen mass flow meter based on the temperature deviation between the transient temperature and the preset safe sublimation vaporization threshold temperature.

10. The intelligent powder mixing and spraying system based on CrSi target material according to claim 6, characterized in that, The auxiliary powder feed port is mounted on the external support of the plasma generator via an axial precision displacement stage, so that the auxiliary powder feed port can be moved and adjusted along the axial direction of the plasma jet.