A method for producing oxidation-resistant hot-formed steel
By regulating the dew point of the heating furnace atmosphere and controlling the temperature and phase transformation, a continuous and dense oxide scale is formed, which solves the problem of oxide scale peeling off the surface of hot-formed steel, improves production efficiency and product quality, and reduces production costs.
Patent Information
- Application Number
- CN202611562205.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
The problem of iron oxide scale peeling off during the heating and heat preservation process of existing hot-formed steel is serious, which affects production efficiency and product quality. Existing solutions, such as applying coatings and controlling alloying elements, have problems such as high cost and poor manufacturability.
By regulating the dew point of the heating furnace atmosphere and controlling the temperature and phase transformation, a continuous and dense oxide scale is formed. Combined with composite structures such as equiaxed ferrite and martensite, the bonding force and thermal compatibility between the oxide scale and the substrate are improved, avoiding the use of additional coatings and alloying elements.
It achieves continuous and dense adhesion of oxide scale, reduces cleaning frequency, improves production efficiency and product quality, reduces production costs, and avoids dimensional accuracy problems caused by shot peening.
Smart Images

Figure CN123108469A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hot working technology, and specifically relates to a method for producing oxidation-resistant hot-formed steel. Background Technology
[0002] Hot-formed steel possesses advantages such as ultra-high strength, excellent formability, low springback after forming, and superior impact resistance, making it widely used in automotive safety structural components such as A / B pillars and anti-collision beams. However, during the heating and holding process before hot stamping, even with the introduction of an inert atmosphere in the furnace for protection, significant iron oxide scale growth still occurs due to residual oxygen. This scale has poor adhesion to the substrate, easily peeling off during subsequent stamping, requiring frequent mold cleaning to prevent surface defects. Furthermore, it can affect the dimensional accuracy of hot-formed parts during subsequent shot peening to remove the scale. Therefore, the scale peeling problem of hot-formed steel has become one of the significant bottlenecks affecting its high-end manufacturing.
[0003] To address the problem of oxide scale peeling off hot-formed steel, a conventional solution is to apply an anti-oxidation layer, typically an aluminum-silicon coating. However, this method significantly increases production costs and time, and is prone to problems such as surface nodules on furnace rolls, deterioration of weldability, and hydrogen embrittlement. Another potential solution is alloying element control, which involves adding oxygen-loving elements such as Cr and Si to form a protective oxide film during the heating and holding stage before hot forming, thereby improving high-temperature oxidation resistance. However, low levels of Cr and Si have limited anti-oxidation effects, while high levels can lead to selective oxidation in upstream processes such as hot rolling, deteriorating surface quality and causing manufacturability issues such as hot rolling cracking. Therefore, effectively suppressing the formation and peeling of oxide scale on the surface of hot-formed steel has become a key technical challenge that urgently needs to be overcome in this field.
[0004] Chinese patents CN112703106B and CN114555838A disclose a molding quenching method, proposing to heat-treat pre-coated blanks in an atmosphere with an oxidation energy equal to or greater than that of an atmosphere composed of 1% by volume oxygen and equal to or less than that of an atmosphere composed of 50% by volume oxygen, and with a dew point of -30°C to +30°C, aiming to suppress hydrogen adsorption and enhance resistance to delayed fracture. However, for bare plates without a pre-coated surface, the oxidation energy of this heat treatment atmosphere is too high, causing extremely serious problems of iron oxide scale growth and peeling. In addition, the hot-formed steels in Chinese patents CN112703106B and CN114555838A have microstructures of martensite, martensite + bainite, or equiaxed ferrite (≥75%) + martensite + bainite. However, the thermal compatibility between the first two microstructures and the iron oxide scale is poor, while the ferrite content in the latter microstructure is too high, which significantly degrades the strength of the hot-formed steel.
[0005] Chinese patent CN115747437A discloses a hot forming process for reducing color difference on the surface of hot-dip galvanized steel. This invention involves placing the pre-formed sheet material into a heating furnace with a dew point temperature ≤0℃ for austenitization and heat preservation. During the heat preservation process, the oxygen content in the furnace is controlled to be 10%–40 vol%, thereby improving the uniformity of oxide composition distribution on the surface of the hot-dip galvanized steel. Similarly, for bare sheets without pre-coating, excessively strong oxidizing atmosphere in the heating furnace can cause extremely serious iron oxide scale peeling.
[0006] Chinese patent CN102652177B discloses a method for manufacturing flat steel products with good formability. It proposes annealing in an atmosphere containing 0.1-25% by volume of H2, H2O, and the remainder N2, with the annealing atmosphere having a dew point between -20°C and +60°C, and the H2O / H2 ratio in the atmosphere reaching a maximum of 0.957. However, although reducing H2 can inhibit the growth of iron oxide on the steel surface, high concentrations of H2 are difficult to introduce into hot forming furnaces in industrial production due to limitations in the airtightness and explosion-proof safety of existing hot forming furnaces during the pre-forming heating and holding stage. Summary of the Invention
[0007] To address the aforementioned technical problems, this invention provides a method for preparing antioxidant hot-formed steel, aiming to solve the problem of oxide scale peeling off the surface of hot-formed steel, reduce the frequency of die cleaning, and eliminate the need for subsequent shot peening treatment, thereby improving production efficiency and product quality while taking into account economic efficiency.
[0008] To achieve the above objectives, the technical solution of the present invention is as follows:
[0009] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0010] The sheet metal is heated to 780℃~900℃ in a furnace with a protective atmosphere and held for 1min~10min. The dew point of the protective atmosphere is +15℃ to +40℃. The heated sheet metal is transferred to a hot forming die within 2s~8s for stamping. The stamped component is cooled in the die under controlled temperature, with a quenching rate of 20℃ / s~50℃ / s and a holding time of 10s~30s, to obtain the processed hot-formed component, so as to obtain a microstructure of equiaxed ferrite + martensite or equiaxed ferrite + martensite + bainite in the steel, wherein the equiaxed ferrite accounts for 8%~30% by volume percentage.
[0011] Furthermore, during the heating process, the protective atmosphere uses one or both of Ar and N2 as the carrier gas, and optionally includes H2; when H2 is included, the H2 content in the protective atmosphere is greater than 0 and less than or equal to 0.5% by volume percentage.
[0012] Further, the sheet metal is composed of the following components by weight percentage: C 0.15%~0.40%, Si 0.06%~2.5%, Mn 0.8%~3.0%, Cr≤3.5%, P≤0.025%, S≤0.02%, optionally containing other trace alloying elements in total not exceeding 0.5%, with the remainder being Fe and unavoidable impurities.
[0013] Furthermore, the trace alloying elements include one or more of B, Nb, Ti, Mo, and Al.
[0014] Furthermore, the sheet material is a hot-rolled pickled sheet or a cold-rolled continuously annealed sheet.
[0015] In a preferred embodiment of the present invention, when the sheet material is a cold-rolled continuous annealing sheet, the H2 content in the atmosphere used during the cold-rolled continuous annealing process is 3% to 8% by volume, and the dew point of the atmosphere used is -50°C to -30°C.
[0016] The surface of the processed thermoformed component has a continuous, dense, and highly adhesive iron oxide scale, and there is a continuous oxide layer containing one or more elements of Mn, Si, or Cr between the iron oxide scale and the substrate.
[0017] The main design concept of this invention is:
[0018] 1) Regulating oxidation products to improve oxide scale adhesion: By introducing water vapor (corresponding to an atmosphere dew point of +15℃ to +40℃) into the heating furnace before hot forming, the H2O at high temperature participates in the oxidation reaction, promoting the growth of selective oxides containing Mn, Si, Cr, etc. at the interface between the iron oxide scale and the substrate, forming a high-bonding transition layer, which significantly improves the interfacial bonding and thermal matching between the iron oxide scale and the substrate, and acts as an anti-oxidation barrier layer to a certain extent to inhibit the subsequent oxidation of the substrate; at the same time, the high dew point H2O can also change the growth kinetics mechanism of the oxide scale, changing from the traditional outward diffusion growth of metal ions to the inward diffusion growth of oxygen ions, making the generated oxide scale more continuous and dense; in addition, reducing the heating temperature from the traditional single-phase austenitizing temperature to the two-phase region temperature will reduce oxide scale growth and reduce growth stress. Based on this, the use of 3%~8% H2 and a dew point of -50℃ to -30℃ in the annealing process of cold-rolled continuous annealing sheet is beneficial to obtaining selective oxides on the surface, which can further suppress surface oxidation in subsequent hot forming as an antioxidant layer; while in the hot forming process, a trace amount of reducing H2 (≤0.5 vol.%) is further introduced into the heating furnace atmosphere to reduce the oxidizing properties of the atmosphere in the heating furnace without increasing the safety risks of industrial production.
[0019] 2) Regulating the matrix structure to improve thermal compatibility with oxide scale: To improve the problem of oxide scale cracking and peeling caused by the explosive phase transformation stress of martensite during traditional fully austenitizing quenching, this invention uses two-phase region heating and holding to retain 8%–30% of primary equiaxed ferrite. Combined with subsequent hot stamping temperature-controlled cooling, a composite structure composed of equiaxed ferrite (8%~30%) + martensite, or equiaxed ferrite (8%~30%) + martensite + bainite is constructed. This structure achieves a high strength and toughness combination of "hard phase bearing and soft phase buffering" while utilizing the microscopic plastic rheology of equiaxed ferrite to absorb thermal stress, effectively weakening the local stress concentration and volume change during martensitic transformation. This significantly reduces the thermal mismatch problem at the matrix and oxide scale interface, ensuring the continuous density and firm adhesion of oxide scale during stamping.
[0020] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows:
[0021] 1) Balancing Strength and Manufacturability: Existing anti-oxidation solutions for hot-formed steel mainly include applying coatings (such as aluminum-silicon coatings) and controlling alloy composition (such as adding Si and Cr). However, applying coatings can affect weldability, leading to subsequent welding defects and easily causing hydrogen embrittlement. On the other hand, alloy control techniques that improve oxidation resistance by adding film-forming elements are prone to hot rolling cracking and severe selective surface oxidation in previous processes (hot rolling and annealing), thus deteriorating manufacturability. This invention improves oxide scale adhesion by combining furnace atmosphere control with temperature and phase transformation control, without introducing alloying elements or additional coatings that deteriorate manufacturability. This ensures good manufacturability throughout the entire production process and gives the hot-formed parts a microstructure that balances strength and plasticity with good thermal compatibility with the oxide scale.
[0022] 2) Reduce production costs and improve production efficiency: The current method for oxidation resistance of hot-formed steel in industry mainly involves applying an aluminum-silicon coating, which requires additional coating equipment, coating raw materials, and corresponding processes, resulting in high production costs and low efficiency. The oxidation-resistant hot-formed steel preparation method proposed in this invention can be implemented directly by adjusting the process parameters of the existing hot-formed production line, without adding raw materials or additional coating steps. It can also reduce the frequency of mold cleaning and eliminate the subsequent shot peening process, resulting in significant economic benefits.
[0023] 3) Improved dimensional accuracy of hot-formed parts: Existing bare-plate hot forming technology results in an oxide scale on the steel plate surface that is prone to cracking and peeling, requiring shot peening for removal. However, under the force of shot peening, hot-formed parts are prone to plastic deformation, affecting the dimensional accuracy of the components. This invention, through process control, forms a continuous, dense, highly adhesive, and thermally compatible high-quality oxide scale on the bare plate surface, eliminating the need for subsequent shot peening and enabling direct coating with the oxide scale on, effectively avoiding the dimensional accuracy degradation of hot-formed parts caused by shot peening stress. Attached Figure Description
[0024] Figure 1 A cross-sectional scanning electron microscope image of the hot-formed steel prepared in Example 1;
[0025] Figure 2 The cross-sectional energy dispersive spectroscopy (EDS) diagram of the hot-formed steel prepared in Example 1;
[0026] Figure 3 The surface optical mirror image and white light interference three-dimensional image of the hot-formed steel prepared in Example 7;
[0027] Figure 4 The surface optical mirror image and three-dimensional white light interference image of the hot-formed steel prepared for Comparative Example 1 are shown. Detailed Implementation
[0028] In its specific implementation, this invention provides a method for producing oxidation-resistant hot-formed steel. The sheet metal is heated to 800-900°C in the two-phase region of a furnace with a protective atmosphere (dew point +15°C to +40°C) and held for 3-5 minutes. The heated sheet metal is then rapidly transferred to a hot-forming die for stamping. The stamped component is then quenched and cooled in the die at a rate of 20-40°C / s, resulting in a microstructure of equiaxed ferrite + martensite or equiaxed ferrite + martensite + bainite, wherein the equiaxed ferrite accounts for 8%-28%. This invention can obtain a continuous, dense, and highly adhesive oxide scale on the surface of hot-formed parts, solving the problem of oxide scale peeling on the surface of hot-formed steel, reducing the frequency of die cleaning, and eliminating the need for subsequent shot peening. This improves production efficiency and product quality while maintaining economic efficiency.
[0029] The present invention will now be further described with reference to specific embodiments.
[0030] The chemical composition of the steel used in each embodiment is shown in Table 1. The following description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto.
[0031] Table 1. Chemical composition of the steel used in the examples and comparative examples (unit: weight percentage) steel C Mn Si Cr Al Ti Mo Nb B P S A 0.223 1.321 0.245 0.186 0.035 0.028 / / 0.0035 0.0125 0.0015 B 0.177 2.121 1.804 / 0.041 / / 0.028 0.00032 0.0061 0.0011 C 0.162 2.152 0.313 0.725 0.016 / 0.304 0.043 0.0025 0.0108 0.0016
[0032] Example 1
[0033] In this embodiment, the steel grade is A steel, and the plate material is hot-rolled pickled plate.
[0034] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0035] The sheet metal is heated to 850°C in a furnace with a protective atmosphere (N2 + 0.5 vol.% H2, dew point +15°C) for 3 minutes. The heated sheet metal is then transferred to a hot forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature, with a quenching rate of 35°C / s and a holding time of 10-30 seconds, resulting in a treated hot-formed component with an equiaxed ferrite + martensite microstructure in the steel, wherein the equiaxed ferrite accounts for 18% by volume. The oxide scale adhesion grade on the surface of the treated hot-formed component is grade 0.
[0036] Example 2
[0037] In this embodiment, the steel grade is A steel, and the plate material is hot-rolled pickled plate.
[0038] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0039] The sheet metal is heated to 850°C in a furnace with a protective atmosphere (N2) and a dew point of +30°C for 3 minutes. The heated sheet metal is then transferred to a hot forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature conditions at a quenching rate of 40°C / s and a holding time of 10-30 seconds to obtain a treated hot-formed component with an equiaxed ferrite + martensite microstructure in the steel, wherein the equiaxed ferrite accounts for 18% by volume. The oxide scale adhesion grade on the surface of the treated hot-formed component is grade 0.
[0040] Example 3
[0041] In this embodiment, the steel grade is B steel, and the sheet material is cold-rolled continuous annealing sheet. During the cold rolling continuous annealing process, the atmosphere used is N2 + 5 vol.% H2, and the dew point is -30℃.
[0042] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0043] The sheet metal is heated to 880°C in a furnace with a protective atmosphere (N2 + 0.1 vol.% H2, dew point +25°C) for 5 minutes. The heated sheet metal is then transferred to a hot forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature, with a quenching rate of 30°C / s and a holding time of 10-30 seconds, resulting in a treated hot-formed component with an equiaxed ferrite + martensite microstructure in the steel, wherein the equiaxed ferrite accounts for 12% by volume. The oxide scale adhesion grade on the surface of the treated hot-formed component is grade 0.
[0044] Example 4
[0045] In this embodiment, the steel grade is C steel and the plate material is hot-rolled pickled plate.
[0046] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0047] The sheet metal is heated to 830°C in a furnace with a protective atmosphere (N2) and a dew point of +25°C for 5 minutes. The heated sheet metal is then transferred to a hot forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature conditions at a quenching rate of 40°C / s and a holding time of 10-30 seconds to obtain a treated hot-formed component with an equiaxed ferrite + martensite microstructure in the steel, wherein the equiaxed ferrite accounts for 25% by volume. The oxide scale adhesion grade on the surface of the treated hot-formed component is grade 0.
[0048] Example 5
[0049] In this embodiment, the steel grade is B steel, and the sheet material is cold-rolled continuous annealing sheet. During the cold rolling continuous annealing process, the atmosphere used is N2 + 5 vol.% H2, and the dew point is -30℃.
[0050] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0051] The sheet metal is heated to 900°C in a furnace with a protective atmosphere (N2 + 0.5 vol.% H2, dew point +25°C) for 3 minutes. The heated sheet metal is then transferred to a hot forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature, with a quenching rate of 30°C / s and a holding time of 10-30 seconds, resulting in a treated hot-formed component with an equiaxed ferrite + martensite microstructure in the steel, wherein the equiaxed ferrite accounts for 8% by volume. The oxide scale adhesion grade on the surface of the treated hot-formed component is grade 0.
[0052] Example 6
[0053] In this embodiment, the steel grade is A steel, and the plate material is hot-rolled pickled plate.
[0054] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0055] The sheet metal is heated to 800°C in a furnace with a protective atmosphere (N2) and a dew point of +25°C for 5 minutes. The heated sheet metal is then transferred to a hot-forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature, with a quenching rate of 20°C / s and a holding time of 10-30 seconds, resulting in a treated hot-formed component with a microstructure of equiaxed ferrite, bainite, and martensite in the steel. The equiaxed ferrite comprises 28% and the bainite 30% by volume percentage. The oxide scale adhesion grade on the surface of the treated hot-formed component is grade 0.
[0056] Example 7
[0057] In this embodiment, the steel grade is A steel, and the plate material is hot-rolled pickled plate.
[0058] A method for preparing oxidation-resistant hot-formed steel includes the following steps:
[0059] The sheet metal is heated to 840°C in a furnace with a protective atmosphere (N2) and a dew point of +40°C for 5 minutes. The heated sheet metal is then transferred to a hot forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature conditions at a quenching rate of 40°C / s and a holding time of 10-30 seconds to obtain a treated hot-formed component with an equiaxed ferrite + martensite microstructure in the steel, wherein the equiaxed ferrite accounts for 12% by volume. The oxide scale adhesion level on the surface of the treated hot-formed component is Grade 1.
[0060] Comparative Example 1
[0061] In this comparative example, the steel grade is A steel, and the plate material is hot-rolled pickled plate.
[0062] The sheet metal was heated to 930°C in a furnace with a protective atmosphere (industrial grade N2) and a dew point of -48°C for 3 minutes. The heated sheet metal was then transferred to a hot-forming die within 2-8 seconds for stamping. The stamped component was then cooled in the die under controlled temperature conditions at a quenching rate of 40°C / s and a holding time of 10-30 seconds to obtain a treated hot-formed component with a fully martensitic microstructure. The oxide scale adhesion level on the surface of the treated hot-formed component was grade 4.
[0063] Comparative Example 2
[0064] In this comparative example, the steel grade is B steel, and the sheet material is cold-rolled continuous annealing sheet. During the cold rolling continuous annealing process, the atmosphere used is N2 + 5 vol.% H2, and the dew point is -50℃.
[0065] The sheet metal is heated to 950°C in a furnace with a protective atmosphere (N2) and a dew point of -48°C for 5 minutes. The heated sheet metal is then transferred to a hot-forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature conditions at a quenching rate of 30°C / s and a holding time of 10-30 seconds to obtain a treated hot-formed component with a fully martensitic microstructure. The oxide scale adhesion level on the surface of the treated hot-formed component is grade 3.
[0066] Comparative Example 3
[0067] In this comparative example, the steel grade is A steel, and the plate material is hot-rolled pickled plate.
[0068] The sheet metal is heated to 850°C in a furnace with a protective atmosphere (N2) and a dew point of -48°C for 3 minutes. The heated sheet metal is then transferred to a hot-forming die within 2-8 seconds for stamping. The stamped component is then cooled in the die under controlled temperature conditions at a quenching rate of 40°C / s and a holding time of 10-30 seconds to obtain a treated hot-formed component with a fully martensitic microstructure. The oxide scale adhesion level on the surface of the treated hot-formed component is grade 3.
[0069] The results of the above hot-formed steel oxide scale adhesion performance show that Examples 1-6 all obtained oxide scale with strong adhesion and no peeling. In Example 7, the atmosphere dew point of +40℃ is at the upper limit of the suitable value, and the oxide scale adhesion is good. After the cross-cut test, the peeling area is ≤5%. The difference between Comparative Examples 1-3 and the Examples is that no additional H2O (corresponding to the atmosphere dew point) was introduced into the protective atmosphere. In addition, the heating temperature used in Comparative Examples 1 and 2 is the fully austenitizing temperature commonly used in the industry, and the cooling structure after hot forming is martensite. In order to better compare and reflect the influence of atmosphere dew point, the heating temperature of Comparative Example 3 was also reduced to 850℃, a two-phase temperature. The cooling structure is the same as that of Example 1, which is also equiaxed ferrite + martensite. The oxide scale bonding force of Comparative Examples 1-3 is poor. It is difficult to completely solve the oxide scale adhesion problem by simply adding film-forming elements (such as Si). Although reducing the heating temperature and controlling the thermal regime to form equiaxed ferrite + martensite can improve the oxide scale adhesion to a certain extent, it still needs to be combined with atmosphere dew point control.
[0070] Depend on Figures 1-3 It is evident that the oxide scale of the hot-formed steel prepared in Examples 1 and 7 is dense, continuous, and has strong adhesion to the substrate. Furthermore, in Example 1, a thin, continuous layer of Si- and Cr-rich oxides exists between the oxide scale and the substrate. In Example 7, no cracking or peeling was observed on the oxide scale. Figure 4 It is evident that the oxide scale on the surface of the hot-formed steel in Comparative Example 1 exhibits significant cracking and peeling problems.
[0071] As can be seen from the above embodiments, the hot-formed steel production method of the present invention can obtain a continuous, dense, and highly adhesive oxide scale, significantly improving the oxidation resistance of the hot-formed steel. Therefore, the present invention can solve the problem of oxide scale peeling off the surface of hot-formed steel, reduce the frequency of die cleaning, and eliminate the need for subsequent shot peening, avoiding deformation of parts caused by shot peening force. Furthermore, the hot-formed steel production method provided in this application has the advantages of strong operability, high economy, and high production efficiency.
Claims
1. A method for producing oxidation-resistant hot-formed steel, characterized in that, Includes the following steps: The sheet metal is heated to 780℃~900℃ in a furnace with a protective atmosphere and held for 1min~10min. The dew point of the protective atmosphere is +15℃ to +40℃. The heated sheet metal is transferred to a hot forming die within 2s~8s for stamping. The stamped component is cooled in the die under controlled temperature, with a quenching rate of 20℃ / s~50℃ / s and a holding time of 10s~30s, to obtain the processed hot-formed component, so as to obtain a microstructure of equiaxed ferrite + martensite or equiaxed ferrite + martensite + bainite in the steel, wherein the equiaxed ferrite accounts for 8%~30% by volume percentage.
2. The method for producing oxidation-resistant hot-formed steel according to claim 1, characterized in that, During the heating process, the protective atmosphere uses one or both of Ar and N2 as the carrier gas, and optionally includes H2; when H2 is included, the H2 content in the protective atmosphere is greater than 0 and less than or equal to 0.5% by volume percentage.
3. The method for producing oxidation-resistant hot-formed steel according to claim 1, characterized in that, The sheet metal is composed of the following components by weight percentage: C 0.15%~0.40%, Si 0.06%~2.5%, Mn 0.8%~3.0%, Cr≤3.5%, P≤0.025%, S≤0.02%, optionally containing other trace alloying elements in total not exceeding 0.5%, with the remainder being Fe and unavoidable impurities.
4. The method for producing oxidation-resistant hot-formed steel according to claim 3, characterized in that, The other trace alloying elements include one or more of B, Nb, Ti, Mo, and Al.
5. The method for producing oxidation-resistant hot-formed steel according to claim 1, characterized in that, The sheet material is hot-rolled pickled sheet or cold-rolled continuously annealed sheet.
6. The method for producing oxidation-resistant hot-formed steel according to claim 5, characterized in that, When the sheet material is a cold-rolled continuous annealing sheet, the H2 content in the atmosphere used during the cold-rolled continuous annealing process is 3% to 8% by volume, and the dew point of the atmosphere used is -50°C to -30°C.
7. The method for producing oxidation-resistant hot-formed steel according to claim 1, characterized in that, The surface of the processed thermoformed component has a continuous, dense, and highly adhesive iron oxide scale, and there is a continuous oxide layer containing one or more elements of Mn, Si, or Cr between the iron oxide scale and the substrate.
Citation Information
Patent Citations
Method for producing an easily deformable flat steel product, flat steel product, and method for producing a component from such a flat steel product
CN102652177B
Molding quenching method
CN112703106B
Die quenching method
CN114555838A
Hot forming process for reducing surface color difference of hot-galvanized hot-formed steel
CN115747437A