A method for carburizing and quenching DC04 steel fastening nuts
By controlling the carbon potential in stages and cooling the temperature before quenching, the problems of insufficient hardness and deformation of DC04 steel fasteners after quenching were solved, achieving a balance between high hardness, wear resistance, and toughness, meeting the requirements for anti-loosening performance and long service life, and reducing costs.
Patent Information
- Application Number
- CN202611309099.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
DC04 steel fasteners have extremely low carbon content and no alloying elements, resulting in poor hardenability. After quenching, ferrite is easily formed in the core, leading to insufficient hardness. The nuts are prone to deformation, and brittle carbides are easily formed on the surface, affecting thread accuracy and assembly performance.
A staged carburizing and quenching method is adopted to control the carbon potential, including strong carburizing and diffusion stages. This is combined with pre-quenching cooling to 820℃ and holding at low temperature to control the carbon concentration gradient and microstructure, avoid the formation of brittle carbides, and ensure the matching of surface hardness and core toughness.
It achieves a good match between the high surface hardness and core toughness of DC04 steel fastening nuts, preventing nut deformation and brittle carbides, meeting the requirements for anti-loosening performance and long service life, and reducing costs.
Smart Images

Figure CN123108470A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of heat treatment technology for metallic materials, specifically to a carburizing and quenching method for DC04 steel fastening nuts. Background Technology
[0002] Locking nuts (also known as anti-loosening nuts) are widely used in critical applications such as fasteners for high-speed trains, aerospace engines, spacecraft structural connections, and automotive engine axles and suspension components. Nut loosening is a global challenge. Nut loosening occurs when a nut, after being tightened to the object according to installation requirements, allows itself to rotate due to long-term vibration and the nut's lack of a locking mechanism, once the prestress has decayed to a certain extent. This situation occurs in automobiles, railways, aircraft, tower cranes, and other fields, posing an extreme danger and easily leading to safety accidents. A single piece of equipment can often suffer irreversible damage due to the loosening of a single nut.
[0003] DC04 steel is a cold-rolled low-carbon steel, belonging to the deep-drawing steel category of the European standard EN10130. It has an extremely low carbon content and does not contain alloying elements such as Cr, Ni, Mo, V, Nb, and Ti, classifying it as a non-alloy steel. The mechanical properties of DC04 steel are: yield strength 130–210 MPa, tensile strength ≥270 MPa, and elongation after fracture ≥34%.
[0004] Because DC04 steel is an ultra-low carbon steel (C≤0.08%) and contains almost no alloying elements, its hardenability is very poor. Ferrite is also prone to form in the quenched core, resulting in insufficient core hardness and low strength. Nuts are annular thin-walled parts, and elliptical deformation and end-face warping are easily generated during carburizing and quenching, directly affecting thread accuracy and assembly performance. Furthermore, due to the extremely low initial carbon content of DC04 steel, the surface carbon concentration gradient is large during carburizing. If the carbon potential is too high or diffusion is insufficient, network or blocky carbides easily form on the surface, leading to increased brittleness and making the threads prone to cracking.
[0005] Therefore, there is an urgent need in this field for a heat treatment method that can achieve high hardness and wear resistance in the threaded part of the nut, while retaining sufficient toughness in the core, and effectively controlling the deformation caused by carburizing and quenching, based on the characteristics of DC04 steel. Summary of the Invention
[0006] In view of the problems in the prior art, such as the poor hardenability of DC04 steel due to its extremely low carbon content and lack of alloying elements, the easy formation of ferrite in the core after quenching, and the easy deformation of the annular thin-walled part of the nut during carburizing and quenching, and the easy formation of network or block carbides on the surface, the present invention provides a carburizing and quenching method for DC04 steel fastening nuts.
[0007] The technical solution adopted by this invention to solve its technical problem is as follows: A method for carburizing and quenching DC04 steel fasteners includes the following steps: S1. Carburizing treatment: Place the DC04 steel fastening nut in a heating furnace and hold it at 820℃ for 30 minutes. The carbon potential in the heating furnace is 0.5%. Then raise the temperature to 900℃ for carburizing treatment. The carburizing treatment includes a strong carburizing stage and a diffusion stage. The carbon potential in the strong carburizing stage is 1.05%, and the carbon potential in the diffusion stage is 0.85%. S2. Quenching treatment: Cool the nut after carburizing in step S1 to 820℃ and keep it at 820℃. During the holding period, the carbon potential in the heating furnace is 0.7%. After the holding period, place it in quenching oil at 100℃ for quenching and stir during the quenching process. S3. Tempering treatment: The nuts after quenching in step S2 are tempered at 165℃ for 2 to 3 hours to obtain DC04 steel fastening nuts.
[0008] Furthermore, in step S1, the strong infiltration stage lasts for 120 minutes, and the diffusion stage lasts for 40 minutes.
[0009] Further, in step S2, the nut after carburizing treatment in step S1 is cooled to 820°C in the heating furnace for 70 minutes.
[0010] Furthermore, in step S2, the heat preservation time is 25 minutes.
[0011] Furthermore, in step S2, the frequency of the stirring motor is 30Hz.
[0012] Further, in step S1, DC04 steel fastening nuts are laid flat in layers in the material basket, with 10 layers in each basket, and then the basket is placed in the heating furnace.
[0013] Furthermore, the DC04 steel fastening nut is made of DC04 steel, with a chemical composition of C≤0.08%, Mn≤0.40%, P≤0.025%, S≤0.020%, Al≥0.025%, and does not contain alloying elements such as Cr, Ni, Mo, V, Nb, and Ti.
[0014] The present invention also provides a DC04 steel fastening nut obtained by any of the methods described above.
[0015] Compared with the prior art, the carburizing and quenching method for DC04 steel fastening nuts provided by the present invention has the following beneficial effects: (1) Due to the phased control of 1.05% strong carburizing potential and 0.85% diffusion carbon potential, the carbon concentration of the surface layer forms a smooth transition gradient, avoiding the sudden change in carbon concentration between the surface layer and the core caused by the extremely low initial carbon content of DC04 steel. This effectively prevents the formation of network or blocky brittle carbides on the surface layer after quenching, and ensures the anti-cracking performance of the threaded part.
[0016] (2) Because the carburized nut is cooled to 820°C and kept warm before quenching, the supercooled austenite pre-precipitates an appropriate amount of uniformly distributed ferrite before quenching, which effectively adjusts the core hardness and overcomes the defects of DC04 steel, which has poor hardenability, resulting in coarse ferrite agglomeration and insufficient strength in the core after quenching. This ensures high surface hardness while maintaining good toughness in the core.
[0017] (3) By cooling the temperature to 820℃ before quenching and controlling the carbon potential to 0.7%, the decarburization of the nut surface during the heat preservation process before quenching is effectively prevented, ensuring the uniformity of the hardness of the carburized layer; combined with the low-temperature tempering treatment at 165℃, the surface layer obtains tempered martensite structure and the core obtains a composite structure of tempered troostite and ferrite, achieving a good match between high surface hardness and wear resistance and sufficient toughness of the core, meeting the dual requirements of anti-loosening performance and long service life.
[0018] (4) Due to the use of special material baskets, each layer of screen is laid flat with a single layer of workpieces, and each material basket is laid flat with 10 layers of workpieces. This ensures that the atmosphere in the furnace flows evenly between each layer of workpieces, avoids uneven local carbon potential and uneven heating caused by stacking or dense placement, effectively controls the elliptical deformation and end face warping of the nut during the carburizing and quenching process, and ensures the thread accuracy and subsequent assembly performance.
[0019] (5) This invention achieves effective carburizing and quenching strengthening of DC04 ultra-low carbon steel without alloying elements such as Cr, Ni, Mo, V, Nb, and Ti. It can obtain fastening nuts that meet the requirements without adding expensive alloying elements, and has significant cost advantages. Attached Figure Description
[0020] Other features, objects, and advantages of this application will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings: Figure 1 This is a metallographic microstructure of the surface of the DC04 steel fastening nut after carburizing and quenching in an embodiment of the present invention. Figure 2 This is a metallographic microstructure of the core of the DC04 steel fastening nut after carburizing and quenching in an embodiment of the present invention. Detailed Implementation
[0021] The present application will now be described in further detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and not intended to limit it. Furthermore, it should be noted that, for ease of description, only the parts relevant to the invention are shown in the accompanying drawings.
[0022] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. This application will now be described in detail with reference to the accompanying drawings and embodiments.
[0023] This invention provides a carburizing and quenching method for DC04 steel fastening nuts, the method comprising the following steps S1 to S3.
[0024] Before carburizing, the DC04 steel fastening nuts should be prepared. Preferably, a stress-relieving annealing step should be added before carburizing to effectively eliminate residual stress generated during the initial cold heading and machining process, and reduce deformation caused by stress release during the subsequent carburizing and quenching heating process.
[0025] As a preferred furnace loading method, DC04 steel fastening nuts are laid flat in layers in a dedicated material basket using a sieve-like method, with each layer of workpieces laid flat on the sieve, and 10 layers laid flat in each basket. The basket containing the DC04 steel fastening nuts is then placed in the heating furnace for subsequent carburizing treatment. This furnace loading method ensures uniform circulation of the furnace atmosphere between each layer of workpieces, making the carburizing environment of each layer of nuts consistent, avoiding uneven carbon potential and uneven heating caused by stacking or dense placement, and effectively controlling the elliptical deformation and end face warping of the annular thin-walled nuts during the carburizing and quenching process.
[0026] S1. Carburizing Treatment: Place the DC04 steel fastening nut in a heating furnace. Raise the furnace temperature from room temperature to 820℃ and hold at this temperature for 30 minutes. During this holding period, the carbon potential inside the furnace is controlled at 0.5%, creating an initial carbon concentration gradient on the nut surface. This lays the foundation for subsequent high-temperature carburizing and avoids abrupt changes in carbon concentration between the surface and core due to the extremely low initial carbon content of the DC04 steel. After holding, continue raising the furnace temperature to 900℃ to enter the carburizing treatment stage. The carburizing treatment includes a strong carburizing stage and a diffusion stage. In the strong carburizing stage, the carbon potential inside the furnace is controlled at 1.05%, allowing active carbon atoms to fully penetrate the nut surface, obtaining sufficient carbon concentration reserves to ensure high surface hardness after quenching. After the strong carburizing stage, the diffusion stage begins. In the diffusion stage, the carbon potential inside the furnace is controlled at 0.85%, allowing the excessively high carbon concentration on the surface to diffuse evenly inward, forming a gentle carbon concentration gradient transition layer. This avoids the formation of network or blocky brittle carbides during subsequent quenching due to an excessively steep concentration gradient. The strong infiltration stage lasts for 120 minutes, the diffusion stage lasts for 40 minutes, and the time ratio of the strong infiltration stage to the diffusion stage is 3:1.
[0027] S2. Quenching Treatment: The nut after carburizing in step S1 is cooled to 820℃ and held at 820℃. Specifically, the nut after carburizing is cooled to 820℃ in the furnace. During the cooling process, the heating power is turned off to achieve a slow cooling inside the furnace, and the cooling time is 70 minutes. In this invention, the cooling rate is controlled during the cooling stage to ensure a smooth transition of surface carbon concentration as the temperature decreases, avoiding the precipitation of carbides along grain boundaries. By appropriately lowering the quenching temperature to 820℃, this invention allows the supercooled austenite to pre-precipitate an appropriate amount of uniformly distributed ferrite during the holding process at this temperature, thereby adjusting the core hardness of the nut and avoiding the formation of coarse or aggregated ferrite in the core after quenching due to the extremely poor hardenability of DC04 steel, which would result in insufficient strength. After the nut is cooled to 820℃, it is held at this temperature for 25 minutes. During the holding period, the carbon potential in the furnace is controlled at 0.7% to prevent decarburization of the nut surface during the holding process before quenching and to ensure the uniformity of the hardness of the carburized layer. After the heat preservation is completed, the nut is placed in quenching oil at a temperature of 100°C for quenching. During the quenching process, the nut is stirred at a motor frequency of 30Hz to obtain a quenched structure with a high-hardness surface layer while maintaining sufficient toughness in the core.
[0028] S3. Tempering Treatment: The nut after quenching in step S2 is tempered at 165℃ for 2-3 hours. As a preferred embodiment, the tempering time is 2.5 hours. This low-temperature tempering treatment eliminates quenching stress, stabilizes the tempered microstructure, and results in a tempered martensitic structure on the surface and a composite structure of tempered troostite and ferrite in the core. The final product is a DC04 steel fastening nut with high surface hardness, high wear resistance, and good core toughness.
[0029] Figure 1 This is a metallographic microstructure image of the surface of a DC04 steel fastening nut after carburizing and quenching, as shown in the embodiment of the present invention. Figure 1 As shown, the surface of the DC04 steel fastening nut treated by the method of the present invention is tempered martensitic structure with uniform metallographic structure and no network or blocky carbide precipitation. This indicates that the present invention effectively avoids the formation of brittle carbides through staged carbon potential control, thus ensuring the anti-cracking performance of the threaded part.
[0030] Figure 2 This is a metallographic microstructure of the core of a DC04 steel fastening nut after carburizing and quenching, as shown in the embodiment of the present invention. Figure 2 As shown, the core of the DC04 steel fastening nut treated by the method of the present invention is a composite structure of tempered troostite and ferrite. The ferrite is evenly distributed and there is no coarse agglomeration. This indicates that the present invention, by cooling to 820℃ and holding before quenching, allows the supercooled austenite to pre-precipitate an appropriate amount of evenly distributed ferrite, which effectively adjusts the core hardness and overcomes the defects of coarse agglomeration of ferrite and insufficient strength in the core after quenching caused by the extremely poor hardenability of DC04 steel. It ensures high surface hardness while maintaining good toughness in the core.
[0031] All the above metallographic images were obtained by etching with 4% nitric acid alcohol solution and then observing them under a 500x metallographic microscope.
[0032] The DC04 steel fastening nut used in this invention is made of DC04 steel, which belongs to the deep-drawing steel category in European standard EN10130. Its chemical composition is C≤0.08%, Mn≤0.40%, P≤0.025%, S≤0.020%, Al≥0.025%, and it does not contain alloying elements such as Cr, Ni, Mo, V, Nb, and Ti, thus belonging to non-alloy steel. Because DC04 steel is an ultra-low carbon steel and contains almost no alloying elements to improve hardenability, its hardenability is very poor. After quenching, ferrite easily forms in the core. This invention achieves high hardness and wear resistance in the threaded portion of the DC04 steel nut through the aforementioned carburizing and quenching method, while retaining sufficient toughness in the core, thereby meeting the dual requirements of anti-loosening performance and long service life.
[0033] The above description is merely a preferred embodiment of this application and an explanation of the technical principles employed. Those skilled in the art should understand that the scope of the invention involved in this application is not limited to technical solutions formed by specific combinations of the above-described technical features, but should also cover other technical solutions formed by arbitrary combinations of the above-described technical features or their equivalents without departing from the above-described inventive concept. For example, technical solutions formed by substituting the above features with (but not limited to) technical features with similar functions disclosed in this application.
Claims
1. A method for carburizing and quenching DC04 steel fastening nuts, characterized in that, Includes the following steps: S1. Carburizing treatment: The DC04 steel fastening nut is placed in a heating furnace and first held at 820℃ for 30 minutes, with a carbon potential of 0.5% in the furnace. Then, the temperature is raised to 900℃ for carburizing treatment. The carburizing treatment includes a strong carburizing stage and a diffusion stage. The carbon potential in the strong carburizing stage is 1.05%, and the carbon potential in the diffusion stage is 0.85%. S2. Quenching treatment: Cool the nut after carburizing in step S1 to 820℃ and keep it at 820℃. During the holding period, the carbon potential in the heating furnace is 0.7%. After the holding period, place it in quenching oil at 100℃ for quenching and stir during the quenching process. S3. Tempering treatment: The nuts after quenching in step S2 are tempered at 165℃ for 2 to 3 hours to obtain DC04 steel fastening nuts.
2. The carburizing and quenching method for DC04 steel fastening nuts according to claim 1, characterized in that: In step S1, the duration of the strong penetration stage is 120 minutes, and the duration of the diffusion stage is 40 minutes.
3. The carburizing and quenching method for DC04 steel fastening nuts according to claim 1, characterized in that: In step S2, the nut after carburizing in step S1 is cooled to 820°C in the heating furnace for 70 minutes.
4. The carburizing and quenching method for DC04 steel fastening nuts according to claim 1, characterized in that: In step S2, the heat preservation time is 25 minutes.
5. The carburizing and quenching method for DC04 steel fastening nuts according to claim 1, characterized in that: In step S2, the frequency of the stirring motor is 30Hz.
6. The carburizing and quenching method for DC04 steel fastening nuts according to claim 1, characterized in that: In step S1, the DC04 steel fastening nuts are laid flat in layers in the material basket, with 10 layers in each basket, and then the material basket is placed in the heating furnace.
7. The carburizing and quenching method for DC04 steel fastening nuts according to claim 1, characterized in that: The DC04 steel fastening nut is made of DC04 steel, with a chemical composition of C≤0.08%, Mn≤0.40%, P≤0.025%, S≤0.020%, Al≥0.025%, and does not contain alloying elements such as Cr, Ni, Mo, V, Nb, and Ti.
8. A DC04 steel fastening nut obtained by the method according to any one of claims 1 to 7.