Method for preparing corrosion-resistant thin films suitable for magnesium alloy fuselage frame components
By using a multilayer composite film preparation method, the problem of easy corrosion of magnesium alloys in drone shells has been solved, achieving improvements in lightweight, corrosion resistance, and high-temperature resistance, making it suitable for corrosion protection of magnesium alloy drone shells.
Patent Information
- Application Number
- CN202610365435.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-24
- Publication Date
- 2026-11-17
AI Technical Summary
Magnesium alloys are prone to corrosion in drone shells. Existing anti-corrosion treatment technologies have problems such as limited corrosion resistance, high energy consumption, poor environmental performance, and insufficient bonding strength, which limit their application in complex environments.
A multilayer composite film preparation method is adopted, including high-precision substrate pretreatment, gradient transition layer formation, rare earth-silane composite anti-corrosion layer, nano-sol-gel coating and precision curing treatment, to form a corrosion-resistant film with a multilayer composite structure.
It achieves lightweight design, excellent corrosion resistance, strong bonding, and good high-temperature resistance, meeting the lightweight and high-temperature environmental requirements of flying cars, and also complies with environmental protection standards.
Smart Images

Figure CN123108563A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aerospace material surface treatment technology, specifically a method for preparing corrosion-resistant thin films applicable to magnesium alloy fuselage frame components. Background Technology
[0002] Magnesium alloys, as lightweight and high-strength structural materials, possess characteristics such as low density (1.7-1.9 g / cm³), high specific strength, good shock absorption, and excellent electromagnetic shielding performance, making them widely used in the field of drone manufacturing. Using magnesium alloys to construct drone shells can significantly reduce drone weight, improve endurance, and enhance maneuverability. Statistics show that replacing aluminum alloys with magnesium alloys can reduce drone structural weight by 15-30% and extend flight time by 10-20%.
[0003] However, magnesium alloys are chemically reactive and have a low standard electrode potential (-2.37V), making them highly susceptible to corrosion in humid atmospheres, seawater, and industrial environments, severely impacting their performance and lifespan. As drones frequently operate in complex outdoor environments, their shells face corrosion from rain, moisture, and pollutants, thus placing higher demands on the corrosion resistance of magnesium alloy shells. In coastal areas, the corrosion problem is even more pronounced due to high humidity and salt spray conditions, with noticeable corrosion typically appearing after only 3-6 months of use.
[0004] Currently, the main technologies used for corrosion protection of magnesium alloy surfaces include chemical conversion coatings, anodizing, electroplating, and coating with organic coatings. However, these methods have some shortcomings: chemical conversion coatings are usually thin (0.5-2μm) with limited corrosion resistance, and can typically only withstand 200-500 hours of neutral salt spray testing; anodizing is a complex process with high energy consumption, requiring high voltage (10-30V) and long processing time (20-60 minutes), and the wastewater treatment costs are high; electroplating easily causes heavy metal pollution, which does not meet environmental protection requirements, and the adhesion between the coating and the magnesium alloy substrate is poor, making it prone to peeling; the adhesion between organic coatings and the substrate needs to be improved, and their high-temperature resistance is poor, usually softening and discoloration occurring above 120℃.
[0005] Sol-gel technology, as an effective method for preparing inorganic coatings, has advantages such as simple process, low cost, low-temperature preparation, and easy control of coating composition, showing promising application prospects in the field of metal surface corrosion protection. However, traditional sol-gel coatings suffer from problems such as high curing temperature (usually requiring 200-300℃), insufficient adhesion to the substrate, and susceptibility to cracking, which limit their application in magnesium alloy surface treatment.
[0006] Therefore, developing a simple, environmentally friendly, and efficient synthesis process that can form a thin film with strong adhesion and excellent corrosion resistance on the surface of magnesium alloy drone shells has significant practical application value. Summary of the Invention
[0007] The purpose of this invention is to provide a method for preparing corrosion-resistant films suitable for magnesium alloy fuselage frame components, so as to solve the problems mentioned in the background art.
[0008] To achieve the above objectives, the present invention provides the following technical solution:
[0009] A method for preparing corrosion-resistant thin films suitable for magnesium alloy fuselage frame components includes the following steps:
[0010] Step 1: High-precision substrate pretreatment: The magnesium alloy substrate undergoes precision mechanical pretreatment, ultrasonic enhanced cleaning and degreasing, multi-stage pure water washing and purification, controllable acid pickling and activation treatment, secondary pure water washing and surface condition control in sequence.
[0011] Step 2, Lightweight Composite Membrane Formation: Gradient transition layer formation, plasma-enhanced activation, rare earth-silane composite anti-corrosion layer formation, and precision pure water washing are performed sequentially.
[0012] Step 3, Functionalization Modification: The nanosol-gel coating is prepared and the gradient intelligent pore sealing treatment is carried out sequentially;
[0013] Step 4, Precision Curing Process: Microwave-assisted precision curing, segmented precision curing, and surface functionalization nano-modification are performed sequentially.
[0014] As a further aspect of the present invention: the precision mechanical pretreatment involves progressive polishing using 800-2000 grit diamond sandpaper until the surface roughness reaches Ra≤0.03. .
[0015] As a further aspect of the present invention: the ultrasonic enhanced cleaning and degreasing uses an environmentally friendly degreasing agent, and ultrasonic cleaning and degreasing is performed at 40-60℃ for 5-15 minutes; the environmentally friendly degreasing agent is composed of 2.5% sodium hydroxide or 25g / L sodium carbonate, 8g / L sodium silicate, 1.2% fatty alcohol polyoxyethylene ether, 0.6g / L benzotriazole and deionized water; the ultrasonic enhanced cleaning and degreasing uses a three-tank ultrasonic cleaner with an ultrasonic frequency of 40kHz and a power of 500W.
[0016] As a further aspect of the present invention: the controllable acid pickling and activation treatment uses a precision activation solution and is treated at room temperature for 30 seconds to 2 minutes; the precision activation solution is composed of 3-10 wt% hydrofluoric acid, 2.5% citric acid, 2 g / L sodium benzoate, 1.5 g / L EDTA-2Na, 1.2 g / L cocamidopropyl betaine, and deionized water; the controllable acid pickling and activation treatment uses a precision chemical treatment tank equipped with an automatic temperature control and stirring system, and a magnetic stirring speed of 100 r / min.
[0017] As a further aspect of the present invention: the gradient transition layer is formed using a gradient transition layer treatment solution, which is treated at 45-55°C for 3-8 minutes. The gradient transition layer treatment solution consists of 5 g / L potassium fluorotitanate, 7 g / L potassium fluorozirconate, 12 g / L sodium nitrate, citric acid to adjust the pH to 3.2-3.8, and deionized water. The plasma-enhanced activation is carried out in a high-vacuum plasma treatment device, with high-purity argon as the working gas, a vacuum degree of 1-10 Pa, a power of 100-350 W, and a treatment time of 5-20 minutes.
[0018] As a further aspect of the present invention: the rare earth-silane composite anticorrosive layer is formed using a lightweight composite film-forming agent, and is immersed for 30 minutes at 60°C and pH 3.0-4.5; the lightweight composite film-forming agent is composed of... The rare earth-silane composite anti-corrosion layer is composed of 10% aminopropyltriethoxysilane, 3% cerium nitrate, 4g / L lanthanum nitrate, 4% tetrabutyl titanate, 1.5% hexafluorozirconic acid, 10g / L azelaic acid, and deionized water. The rare earth-silane composite anti-corrosion layer is formed using a precision automatic dip coating machine equipped with a CCD positioning system. The environment is controlled in a cleanroom of Class 1000, with a temperature of 25±1℃ and a humidity of 40±5%RH.
[0019] As a further aspect of the present invention: the nano-sol-gel coating is prepared by a precision dip-coating method with a lifting speed of 12 cm / min. The nano-sol-gel solution is composed of 20-30% tetraethyl orthosilicate, 5-10% tetrabutyl titanate, 40-50% ethanol, 0.5-2% nitric acid, 1% nano-silica, and 10-15% deionized water. The preparation of the nano-sol-gel coating is carried out under nitrogen protection, and ultrasonic treatment is performed for 30 minutes during the solution preparation process to ensure uniform dispersion of nanoparticles.
[0020] As a further aspect of the present invention: the gradient intelligent sealing process includes:
[0021] First sealing step: 7% silica sol, treated at 70℃ for 15 minutes;
[0022] Second sealing step: 5% silane ethanol solution, treated at room temperature for 8 minutes.
[0023] As a further aspect of the present invention: the microwave-assisted precision curing employs a program-controlled stepped heating process, with a power of 300-600W, a curing temperature of 100-180℃, and a curing time of 15-45 minutes; the microwave-assisted precision curing uses an industrial-grade microwave curing oven equipped with an infrared thermometer to monitor the sample temperature in real time, with a temperature uniformity of ±3℃; the segmented precision curing includes: a first stage of pre-baking at 120℃ for 25 minutes, and a second stage of curing at 170℃ for 30 minutes; the surface functionalization nano-modification employs an atomic layer deposition system, depositing... Composite coating or The composite coating has a thickness of 50-200 nm and a deposition temperature of 150 °C, using trimethylaluminum and tetrazirconium as precursors.
[0024] As a further aspect of the present invention: the corrosion-resistant film prepared by the method is suitable for magnesium alloy flying car fuselage frame components, wherein the film has a multi-layer composite structure and a total thickness of 8-12 mm. The coating comprises, from the magnesium alloy substrate outwards, a gradient transition layer, a rare earth-silane composite anti-corrosion layer, a nano-sol-gel coating, a gradient sealing layer, and a surface-functionalized nano-coating; the magnesium alloy substrate is selected from at least one of AZ91D, WE43, AZ31B, and AM60B.
[0025] Compared with the prior art, the beneficial effects of the present invention are:
[0026] 1. Extremely lightweight: The total thickness of the resulting multi-layer composite film is only 8-12 mm. Compared to traditional coatings, it reduces weight by more than 60%, with a weight gain of only 0.2-0.4%, far below the 0.5% requirement of aviation standards, perfectly meeting the lightweight requirements of flying cars;
[0027] 2. Excellent corrosion resistance: Through multi-layer composite structure design and gradient sealing treatment, a dense protective system is formed, achieving 1500-2500 hours of neutral salt spray testing, with corrosion current density reduced to 1×10⁻ 8 With an A / cm² below, it is 2-5 times higher than that of traditional anodizing treatment.
[0028] 3. Super strong adhesion: Through gradient transition layer design and precision coating process, the adhesion between the film layer and the substrate reaches 25-30MPa, with a cross-cut test grade of 0 and an impact strength of ≥60kg・cm, which can effectively resist the coating peeling problem of flying cars in vibration and impact environments.
[0029] 4. Excellent high temperature resistance: Through high temperature curing process and functional nano-coating design, the film can be used for a long time in high temperature environment of 280-400℃, and the short-term temperature resistance can reach 500℃, which meets the use requirements of high temperature areas such as engine compartment.
[0030] 5. Excellent mechanical properties: The film layer hardness can reach 380-420 HV, which is 5-6 times higher than that of untreated magnesium alloys. It also possesses good toughness and fatigue resistance. 7 The strength retention rate after each cycle reached 88-92%.
[0031] 6. Environmental protection and energy saving: It uses environmentally friendly chemical agents and does not use toxic and harmful substances such as chromates, which meets the requirements of green manufacturing.
[0032] 7. Stable and reliable process: The entire process is highly controllable, the product consistency is good, it is suitable for large-scale industrial production, and the processing cost is reduced by 30-50% compared with traditional processes. Attached Figure Description
[0033] Figure 1 This is a schematic diagram of the corrosion-resistant film applicable to magnesium alloy fuselage frame components in this invention.
[0034] Figure 2 This is a process flow diagram of the method for preparing corrosion-resistant thin films applicable to magnesium alloy fuselage frame components in this invention.
[0035] The components include: 1. Surface functionalized nano-coating; 2. Gradient sealing layer; 3. Nano sol-gel coating; 4. Rare earth-silane composite anti-corrosion layer; 5. Gradient transition layer; 6. Magnesium alloy substrate. Detailed Implementation
[0036] Example 1
[0037] In one embodiment, such as Figures 1-2 As shown, a method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components includes the following steps:
[0038] Step 1: High-precision substrate pretreatment: The magnesium alloy substrate 6 undergoes precision mechanical pretreatment, ultrasonic enhanced cleaning and degreasing, multi-stage pure water washing and purification, controllable acid pickling and activation treatment, secondary pure water washing and surface condition control in sequence.
[0039] Step 2, Lightweight Composite Membrane Formation: The following steps are performed sequentially: formation of gradient transition layer 5, plasma-enhanced activation, formation of rare earth-silane composite anti-corrosion layer 4, and precision pure water washing.
[0040] Step 3, Functionalization Modification: The nanosol-gel coating 3 was prepared and the gradient intelligent sealing treatment was carried out sequentially;
[0041] Step 4, Precision Curing Process: Microwave-assisted precision curing, segmented precision curing, and surface functionalization nano-modification are performed sequentially.
[0042] Precision mechanical pretreatment involves progressive polishing with 2000-grit diamond sandpaper until the surface roughness reaches Ra=0.025. Within this roughness range, good adhesion between the coating and the substrate is ensured, while avoiding uneven coating thickness or stress concentration due to excessive surface roughness.
[0043] Ultrasonic enhanced cleaning and degreasing uses an environmentally friendly degreasing agent, involving 8 minutes of ultrasonic cleaning and degreasing at 50℃. The environmentally friendly degreasing agent consists of 2.5% sodium hydroxide or 25g / L sodium carbonate, 8g / L sodium silicate, 1.2% fatty alcohol polyoxyethylene ether, 0.6g / L benzotriazole, and deionized water. Ultrasonic enhanced cleaning and degreasing is performed using a three-tank ultrasonic cleaner with an ultrasonic frequency of 40kHz and a power of 500W. This cleaning process effectively removes cutting fluid, grease, and particulate matter from magnesium alloy surfaces, providing a clean surface for subsequent processing. Temperature control between 40-60℃ improves cleaning efficiency while preventing excessive solvent evaporation due to high temperatures.
[0044] The controlled pickling and activation treatment uses a precision activation solution, which is applied at room temperature for 1 minute. The precision activation solution consists of 4 wt% hydrofluoric acid, 2.5% citric acid, 2 g / L sodium benzoate, 1.5 g / L EDTA-2Na, 1.2 g / L cocamidopropyl betaine, and deionized water. The controlled pickling and activation treatment uses a precision chemical treatment tank equipped with an automatic temperature control and stirring system, with a magnetic stirring speed of 100 rpm. Hydrofluoric acid selectively dissolves the oxide layer on the magnesium alloy surface and simultaneously reacts slightly with the magnesium substrate, forming a uniform micro-pit structure that significantly increases the mechanical adhesion between the coating and the substrate.
[0045] The gradient transition layer 5 was formed using a gradient transition layer treatment solution, treated at 50°C for 5 minutes. The solution consisted of 3.5 g / L potassium fluorotitanate, 5.5 g / L potassium fluorozirconate, citric acid to adjust the pH to 3.2-3.8, and deionized water. Plasma-enhanced activation was performed in a high-vacuum plasma treatment device, using high-purity argon as the working gas, maintaining a vacuum of 3 Pa, a power of 300 W, and a treatment time of 15 minutes. Plasma power and treatment time are key parameters affecting the activation effect: too low a power or too short a time results in insufficient activation; too high a power or too long a time may lead to excessive etching of the magnesium alloy surface, affecting its mechanical properties.
[0046] The rare earth-silane composite anti-corrosion layer 4 is formed using a lightweight composite film-forming agent, which is immersed for 30 minutes at 55℃ and pH 3.0-4.5. The lightweight composite film-forming agent consists of 8% aminopropyltriethoxysilane, 2.5% cerium nitrate, 4g / L lanthanum nitrate, 4% tetrabutyl titanate, 1.5% hexafluorozirconic acid, 10g / L azelaic acid, and deionized water. The rare earth-silane composite anti-corrosion layer 4 is formed using a precision automatic dip coating machine equipped with a CCD positioning system. The environment is controlled in a cleanroom of Class 1000, with a temperature of 25±1℃ and a humidity of 40±5%RH.
[0047] The nano-sol-gel coating 3 was prepared using a precision dip-coating method with a pulling speed of 10 cm / min and a thickness of 2.5 mm. The nano-sol-gel solution consisted of 20-30% tetraethyl orthosilicate, 5-10% tetrabutyl titanate, 40-50% ethanol, 0.5-2% nitric acid, 1% nano-silica, and 10-15% deionized water. The preparation of the nano-sol-gel coating 3 was carried out under nitrogen protection, and ultrasonic treatment for 30 minutes was used during solution preparation to ensure uniform dispersion of nanoparticles. The sol-gel solution of this composition exhibits good stability and coating performance, and the formed coating has excellent corrosion resistance. Among them, tetraethyl orthosilicate and tetrabutyl titanate act as inorganic network forming agents, and their ratio determines the basic properties of the coating; nitric acid acts as a catalyst to control the rate and extent of the sol-gel reaction.
[0048] Gradient intelligent sealing process includes:
[0049] First sealing step: 7% silica sol (containing 1% graphene nanosheets), treated at 70℃ for 15 minutes;
[0050] Second sealing step: 5% silane ethanol solution, treated at room temperature for 8 minutes.
[0051] Microwave-assisted precision curing employs a programmable, stepped heating process with a power of 600W, a curing temperature of 160℃, and a curing time of 25 minutes. An industrial-grade microwave curing oven is used, equipped with an infrared thermometer to monitor sample temperature in real time, achieving a temperature uniformity of ±3℃. Compared to traditional thermal curing, microwave-assisted curing can reduce the curing temperature by approximately 50-100℃, shorten the curing time by more than 50%, reduce energy consumption, and simultaneously improve the coating's density. The segmented precision curing includes a first stage of pre-baking at 110℃ for 25 minutes, followed by a second stage of curing at 160℃ for 30 minutes. Surface functionalization and nano-modification utilize an atomic layer deposition system to deposit a composite coating with a thickness of 120nm at a deposition temperature of 150℃, using trimethylaluminum and tetrazirconium as precursors. These metal oxides possess high hardness, good chemical stability, and excellent wear resistance, significantly enhancing the overall performance of the film when used as the top coating. The coating thickness is controlled within the range of 50-200nm to ensure performance improvement while avoiding increased internal stress and coating cracking caused by excessive thickness.
[0052] The above embodiments disclose a corrosion-resistant film suitable for magnesium alloy fuselage frame components. The film has a multi-layer composite structure with a total thickness of 8-12 mm. From the magnesium alloy substrate 6 outwards, it includes a gradient transition layer 5, a rare earth-silane composite anti-corrosion layer 4, a nano-sol-gel coating 3, a gradient sealing layer 2, and a surface-functionalized nano-coating 1. The magnesium alloy substrate 6 is selected from AZ91D. The film can withstand 1500-2500 hours of neutral salt spray testing, with a tensile bonding strength of 25-30 MPa, a hardness of 380-420 HV, and an impact strength of 60-68 kg·cm. The film can be used for a long time in high-temperature environments of 280-400℃, exhibiting excellent thermal shock performance and withstanding temperature cycles from -60℃ to 400℃. The fatigue life retention rate of the film can reach 88-92%, meeting the fatigue performance requirements for long-term use in flying cars. Compared with untreated magnesium alloy components, the weight increase of the film is only 0.2-0.4%, meeting the lightweight requirements of flying cars. The component is a 1200mm×800mm×8mm main frame structure. It is suitable for various types of flying vehicles, including electric vertical takeoff and landing aircraft, fixed-wing flying cars, and tiltrotor flying cars.
[0053] Comparative Example 1a: No rare earth elements used.
[0054] Process differences: No cerium nitrate rare earth element is added to the rare earth-silane composite anti-corrosion layer 4.
[0055] The performance comparison is shown in Table 1 below:
[0056] Table 1
[0057] Performance items Example 1 Comparative Example 1a Performance degradation Cause Analysis Salt spray test 2000 hours 1200 hours -40% Loss of the corrosion inhibition effect of rare earth ions Temperature resistance 300℃ 250℃ -17% The high-temperature stabilizing effect of rare earth elements disappears.
[0058] As shown in Table 1, the addition of rare earth elements plays an important role in improving the corrosion resistance, high temperature resistance and density of the coating.
[0059] Example 2
[0060] In one embodiment, such as Figures 1-2 As shown, a method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components includes the following steps:
[0061] Step 1: High-precision substrate pretreatment: The magnesium alloy substrate 6 undergoes precision mechanical pretreatment, ultrasonic enhanced cleaning and degreasing, multi-stage pure water washing and purification, controllable acid pickling and activation treatment, secondary pure water washing and surface condition control in sequence.
[0062] Step 2, Lightweight Composite Membrane Formation: The following steps are performed sequentially: formation of gradient transition layer 5, plasma-enhanced activation, formation of rare earth-silane composite anti-corrosion layer 4, and precision pure water washing.
[0063] Step 3, Functionalization Modification: The nanosol-gel coating 3 was prepared and the gradient intelligent sealing treatment was carried out sequentially;
[0064] Step 4, Precision Curing Process: Microwave-assisted precision curing, segmented precision curing, and surface functionalization nano-modification are performed sequentially.
[0065] Precision mechanical pretreatment involves progressive polishing using 2000-grit diamond sandpaper until the surface roughness reaches Ra=0.02. Within this roughness range, good adhesion between the coating and the substrate can be ensured, while avoiding uneven coating thickness or stress concentration due to excessive surface roughness.
[0066] Ultrasonic enhanced cleaning and degreasing uses an environmentally friendly degreasing agent, involving ultrasonic cleaning and degreasing for 12 minutes at 60℃. The environmentally friendly degreasing agent consists of 2.5% sodium hydroxide or 25g / L sodium carbonate, 8g / L sodium silicate, 1.2% fatty alcohol polyoxyethylene ether, 0.6g / L benzotriazole, and deionized water. Ultrasonic enhanced cleaning and degreasing is performed using a three-tank ultrasonic cleaner with an ultrasonic frequency of 40kHz and a power of 500W. This cleaning process effectively removes cutting fluid, grease, and particulate matter from magnesium alloy surfaces, providing a clean surface for subsequent processing. Temperature control between 40-60℃ improves cleaning efficiency while preventing excessive solvent evaporation due to high temperatures.
[0067] The controlled pickling and activation treatment uses a precision activation solution, which is applied at room temperature for 2 minutes. The precision activation solution consists of 6 wt% hydrofluoric acid, 2.5% citric acid, 2 g / L sodium benzoate, 1.5 g / L EDTA-2Na, 1.2 g / L cocamidopropyl betaine, and deionized water. The controlled pickling and activation treatment uses a precision chemical treatment tank equipped with an automatic temperature control and stirring system, with a magnetic stirring speed of 100 rpm. Hydrofluoric acid selectively dissolves the oxide layer on the magnesium alloy surface and simultaneously reacts slightly with the magnesium substrate, forming a uniform micro-pit structure that significantly increases the mechanical adhesion between the coating and the substrate.
[0068] The gradient transition layer 5 was formed using a gradient transition layer treatment solution, treated at 55°C for 8 minutes. The solution consisted of 5 g / L potassium fluorotitanate, 7 g / L potassium fluorozirconate, citric acid adjusted to pH 3.2-3.8, and deionized water. Plasma-enhanced activation was performed in a high-vacuum plasma treatment device, using high-purity argon as the working gas, maintaining a vacuum of 1 Pa, a power of 350 W, and a treatment time of 20 minutes. Plasma power and treatment time are key parameters affecting the activation effect: insufficient power or time results in inadequate activation; excessive power or time may lead to over-etching of the magnesium alloy surface, affecting its mechanical properties.
[0069] The rare earth-silane composite anti-corrosion layer 4 is formed using a lightweight composite film-forming agent, and is immersed for 40 minutes at 60℃ and pH 3.0-4.5; the lightweight composite film-forming agent is composed of... The rare earth-silane composite anti-corrosion layer is composed of 10% aminopropyltriethoxysilane, 3% cerium nitrate, 4g / L lanthanum nitrate, 4% tetrabutyl titanate, 1.5% hexafluorozirconic acid, 10g / L azelaic acid, and deionized water. The rare earth-silane composite anti-corrosion layer 4 is formed using a precision automatic dip coating machine equipped with a CCD positioning system. The environment is controlled in a cleanroom of Class 1000, with a temperature of 25±1℃ and a humidity of 40±5%RH.
[0070] The nano-sol-gel coating 3 was prepared using a precision dip-coating method with a lifting speed of 12 cm / min and a thickness of 3 mm. The nano-sol-gel solution is composed of 20-30% tetraethyl orthosilicate, 5-10% tetrabutyl titanate, 40-50% ethanol, 0.5-2% nitric acid, 1% nano-silica, and 10-15% deionized water. The nano-sol-gel coating is prepared under nitrogen protection, and ultrasonic treatment for 30 minutes during solution preparation ensures uniform dispersion of nanoparticles. This sol-gel solution exhibits good stability and coating performance, and the resulting coating demonstrates excellent corrosion resistance. The ratio of tetraethyl orthosilicate and tetrabutyl titanate acts as inorganic network forming agents, determining the basic properties of the coating; nitric acid acts as a catalyst, controlling the rate and extent of the sol-gel reaction.
[0071] Gradient intelligent sealing process includes:
[0072] First sealing step: 7% silica sol (containing 1% graphene nanosheets), treated at 70℃ for 15 minutes;
[0073] Second sealing step: 5% silane ethanol solution, treated at room temperature for 8 minutes.
[0074] Microwave-assisted precision curing employs a programmable, stepped heating process with a power of 600W, a curing temperature of 180℃, and a curing time of 50 minutes. It utilizes an industrial-grade microwave curing oven equipped with an infrared thermometer to monitor sample temperature in real time, achieving a temperature uniformity of ±3℃. Compared to traditional thermal curing, microwave-assisted curing can reduce the curing temperature by approximately 50-100℃, shorten curing time by more than 50%, reduce energy consumption, and simultaneously improve coating density. The segmented precision curing process includes: a first stage of pre-baking at 120℃ for 25 minutes, followed by a second stage of curing at 170℃ for 30 minutes. Surface functionalization and nano-modification are achieved using an atomic layer deposition system. A composite coating with a thickness of 150 nm and a deposition temperature of 150 °C was developed, using trimethylaluminum and tetrazirconium as precursors. These metal oxides possess characteristics such as high hardness, good chemical stability, and excellent wear resistance, and as a top coating, they can significantly improve the overall performance of the film. The coating thickness was controlled within the range of 50-200 nm to ensure the performance improvement while avoiding increased internal stress and coating cracking caused by excessive thickness.
[0075] The above embodiments disclose corrosion-resistant films suitable for magnesium alloy fuselage frame components. The films have a multi-layer composite structure with a total thickness of 8-12 mm. The coating consists of a gradient transition layer 5, a rare earth-silane composite anti-corrosion layer 4, a nano-sol-gel coating 3, a gradient sealing layer 2, and a surface-functionalized nano-coating 1, arranged sequentially from the magnesium alloy substrate 6 outwards. The magnesium alloy substrate 6 is selected from WE43. The film exhibits a neutral salt spray test performance of 1500-2500 hours, a tensile bonding strength of 25-30 MPa, a hardness of 380-420 HV, and an impact strength of 60-68 kg·cm. The film can be used long-term in high-temperature environments of 280-400℃, demonstrating excellent thermal shock performance and withstanding temperature cycles from -60℃ to 400℃. The film's fatigue life retention rate reaches 88-92%, meeting the fatigue performance requirements for long-term use in flying cars. Compared to untreated magnesium alloy parts, the film only increases weight by 0.2-0.4%, meeting the lightweight requirements of flying cars. The component is a 600mm×400mm×6mm engine nacelle cover. The components are suitable for various types of flying vehicles, including electric vertical takeoff and landing aircraft, fixed-wing flying cars, and tiltrotor flying cars.
[0076] The core performance indicators compared with those of Example 1 are shown in Table 2 below:
[0077] Table 2
[0078] Performance items Results of Example 2 Results of Example 1 Increase Technological breakthrough High temperature resistance 400℃ 300℃ +33% Meets engine compartment requirements Short-term temperature resistance 500℃ 350℃ +43% Coping with extreme temperatures Salt spray test 1800 hours 2000 hours -10% High-temperature performance is a priority bonding force 30MPa 28.5MPa +5% Stable under high temperature conditions hardness 420HV 405HV +4% High temperature hardness retention
[0079] Comparative Example 2a: Lowering the curing temperature.
[0080] Process differences: Curing temperature is reduced from 180℃ to 140℃.
[0081] The performance comparison is shown in Table 3 below:
[0082] Table 3
[0083] Performance items Example 2 Comparative Example 2a Performance degradation Cause Analysis High temperature resistance 400℃ 320℃ -20% Insufficient curing leads to decreased high-temperature stability. bonding force 30MPa 24.3MPa -19% Insufficient resin crosslinking degree leads to decreased interfacial bonding strength. hardness 420HV 350HV -17% The coating hardness decreases and its wear resistance decreases.
[0084] As shown in Table 3, high-temperature curing is a key process to ensure the high-temperature resistance and mechanical properties of the coating.
[0085] Comparative Example 2b: Using a conventional organic coating.
[0086] Process differences: Traditional epoxy resin coating is used instead of multilayer composite film.
[0087] The performance comparison is shown in Table 4 below:
[0088] Table 4
[0089] Performance items Example 2 Comparative Example 2b performance advantages Technological breakthrough film thickness 11.5μm 35μm Weight loss of 67% Ultra-thin coating technology Weight gain percentage 0.4% 2.2% 82% weight loss Lightweight design High temperature resistance 400℃ 200℃ 100% improvement High-temperature material systems Salt spray test 1800 hours 800 hours Increase by 125% Multi-layer protection system bonding force 30MPa 15MPa 100% improvement Interface design optimization
[0090] As shown in Table 4, the multilayer composite film technology of the present invention has a comprehensive performance that far exceeds that of traditional organic coatings under high temperature conditions.
[0091] Example 3
[0092] In one embodiment, such as Figures 1-2 As shown, a method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components includes the following steps:
[0093] Step 1: High-precision substrate pretreatment: The magnesium alloy substrate 6 undergoes precision mechanical pretreatment, ultrasonic enhanced cleaning and degreasing, multi-stage pure water washing and purification, controllable acid pickling and activation treatment, secondary pure water washing and surface condition control in sequence.
[0094] Step 2, Lightweight Composite Membrane Formation: The following steps are performed sequentially: formation of gradient transition layer 5, plasma-enhanced activation, formation of rare earth-silane composite anti-corrosion layer 4, and precision pure water washing.
[0095] Step 3, Functionalization Modification: The nanosol-gel coating 3 was prepared and the gradient intelligent sealing treatment was carried out sequentially;
[0096] Step 4, Precision Curing Process: Microwave-assisted precision curing, segmented precision curing, and surface functionalization nano-modification are performed sequentially.
[0097] Precision mechanical pretreatment involves progressive polishing using 2000-grit diamond sandpaper until the surface roughness reaches Ra=0.015. Within this roughness range, good adhesion between the coating and the substrate can be ensured, while avoiding uneven coating thickness or stress concentration due to excessive surface roughness.
[0098] Ultrasonic enhanced cleaning and degreasing uses an environmentally friendly degreasing agent, involving ultrasonic cleaning and degreasing for 5 minutes at 40℃. The environmentally friendly degreasing agent consists of 2.5% sodium hydroxide or 25g / L sodium carbonate, 8g / L sodium silicate, 1.2% fatty alcohol polyoxyethylene ether, 0.6g / L benzotriazole, and deionized water. Ultrasonic enhanced cleaning and degreasing is performed using a three-tank ultrasonic cleaner with an ultrasonic frequency of 40kHz and a power of 300W. This cleaning process effectively removes cutting fluid, grease, and particulate matter from magnesium alloy surfaces, providing a clean surface for subsequent processing. Temperature control between 40-60℃ improves cleaning efficiency while preventing excessive solvent evaporation due to high temperatures.
[0099] The controlled pickling and activation treatment uses a precision activation solution, processed at room temperature for 30 seconds. The precision activation solution consists of 3 wt% hydrofluoric acid, 2.5% citric acid, 2 g / L sodium benzoate, 1.5 g / L EDTA-2Na, 1.2 g / L cocamidopropyl betaine, and deionized water. The controlled pickling and activation treatment uses a precision chemical treatment tank equipped with an automatic temperature control and stirring system, with a magnetic stirring speed of 100 rpm. Hydrofluoric acid selectively dissolves the oxide layer on the magnesium alloy surface and simultaneously reacts slightly with the magnesium substrate, forming a uniform micro-pit structure, significantly increasing the mechanical adhesion between the coating and the substrate.
[0100] The gradient transition layer 5 was formed using a gradient transition layer treatment solution, treated at 45°C for 3 minutes. This solution consisted of 2 g / L potassium fluorotitanate, 4 g / L potassium fluorozirconate, citric acid to adjust the pH to 3.2-3.8, and deionized water. Plasma-enhanced activation was performed in a high-vacuum plasma treatment device. The working gas was high-purity argon, the vacuum degree was 5 Pa, the power was 200 W, and the treatment time was 10 minutes. Plasma power and treatment time are key parameters affecting the activation effect: too low a power or too short a time results in insufficient activation; too high a power or too long a time may lead to excessive etching of the magnesium alloy surface, affecting its mechanical properties.
[0101] The rare earth-silane composite anti-corrosion layer 4 is formed using a lightweight composite film-forming agent, and is immersed for 15 minutes at 50℃ and pH 3.0-4.5; the lightweight composite film-forming agent is composed of... The rare earth-silane composite anti-corrosion layer is composed of 6% aminopropyltriethoxysilane, 2% cerium nitrate, 4g / L lanthanum nitrate, 4% tetrabutyl titanate, 1.5% hexafluorozirconic acid, 10g / L azelaic acid, and deionized water. The rare earth-silane composite anti-corrosion layer 4 is formed using a precision automatic dip coating machine equipped with a CCD positioning system. The environment is controlled in a cleanroom of Class 1000, with a temperature of 25±1℃ and a humidity of 40±5%RH.
[0102] The nano-sol-gel coating 3 was prepared using a precision dip-coating method with a lifting speed of 8 cm / min and a thickness of 2 mm. The nano-sol-gel solution is composed of 20-30% tetraethyl orthosilicate, 5-10% tetrabutyl titanate, 40-50% ethanol, 0.5-2% nitric acid, 1% nano-silica, and 10-15% deionized water. The nano-sol-gel coating is prepared under nitrogen protection, and ultrasonic treatment for 30 minutes during solution preparation ensures uniform dispersion of nanoparticles. This sol-gel solution exhibits good stability and coating performance, and the resulting coating demonstrates excellent corrosion resistance. The ratio of tetraethyl orthosilicate and tetrabutyl titanate acts as inorganic network forming agents, determining the basic properties of the coating; nitric acid acts as a catalyst, controlling the rate and extent of the sol-gel reaction.
[0103] Gradient intelligent sealing process includes:
[0104] First sealing step: 7% silica sol (containing 1% graphene nanosheets), treated at 70℃ for 15 minutes;
[0105] Second sealing step: 5% silane ethanol solution, treated at room temperature for 8 minutes.
[0106] Microwave-assisted precision curing employs a programmable, stepped heating process with a power of 300W, a curing temperature of 120℃, and a curing time of 20 minutes. It utilizes an industrial-grade microwave curing oven equipped with an infrared thermometer to monitor sample temperature in real time, achieving a temperature uniformity of ±3℃. Compared to traditional thermal curing, microwave-assisted curing can reduce the curing temperature by approximately 50-100℃, shorten curing time by more than 50%, reduce energy consumption, and simultaneously improve coating density. The segmented precision curing process includes: a first stage of pre-baking at 100℃ for 25 minutes, followed by a second stage of curing at 150℃ for 30 minutes. Surface functionalization and nano-modification are achieved using an atomic layer deposition system. A composite coating with a thickness of 80 nm and a deposition temperature of 150 °C was developed, using trimethylaluminum and tetrazirconium as precursors. These metal oxides possess high hardness, good chemical stability, and excellent wear resistance, and as a top coating, they can significantly improve the overall performance of the film. The coating thickness was controlled within the range of 50-200 nm to ensure the performance improvement while avoiding increased internal stress and coating cracking caused by excessive thickness.
[0107] The above embodiments disclose corrosion-resistant films suitable for magnesium alloy fuselage frame components. The films have a multi-layer composite structure with a total thickness of 8-12 mm. The coating consists of a gradient transition layer 5, a rare earth-silane composite anti-corrosion layer 4, a nano-sol-gel coating 3, a gradient sealing layer 2, and a surface-functionalized nano-coating 1, arranged sequentially from the magnesium alloy substrate 6 outwards. The magnesium alloy substrate 6 is selected from AZ31B magnesium alloy (Al 3%, Zn 1%, Mn 0.3%). The film exhibits a neutral salt spray test performance of 1500-2500 hours, a tensile bonding strength of 25-30 MPa, a hardness of 380-420 HV, and an impact strength of 60-68 kg·cm. The film can be used long-term in high-temperature environments of 280-400℃, demonstrating excellent thermal shock resistance and withstanding temperature cycles from -60℃ to 400℃. The film's fatigue life retention rate reaches 88-92%, meeting the fatigue performance requirements for long-term use in flying cars. Compared to untreated magnesium alloy components, the film only increases weight by 0.2-0.4%, meeting the lightweight requirements of flying cars. The component is an 800mm × 600mm × 4mm cockpit frame. The components are suitable for various types of flying vehicles, including electric vertical takeoff and landing aircraft, fixed-wing flying cars, and tiltrotor flying cars.
[0108] The core performance indicators compared with those of Example 1 are shown in Table 5 below:
[0109] Table 5
[0110] Performance items Results of Example 3 Results of Example 1 Comparative advantages Application Features film thickness 8.5μm 10.5μm -19% Extremely lightweight Weight gain percentage 0.2% 0.3% -33% Minimum weight gain Salt spray test 1500 hours 2000 hours -25% Meets cabin requirements bonding force 25MPa 28.5MPa -12% Meets cabin strength requirements hardness 380HV 405HV -6% Sufficient wear resistance Temperature resistance 280℃ 300℃ -7% Meet cabin temperature requirements Surface quality Ra=0.02μm, gloss 60±5GU Ra=0.025μm, gloss 50±5GU Superior appearance Better decorative
[0111] Comparative Example 3a: Traditional anodizing treatment.
[0112] Process differences: The traditional chromate anodizing process is used.
[0113] The performance comparison table is shown in Table 6 below:
[0114] Table 6
[0115] Performance items Example 3 Comparative Example 3a performance advantages Technological progress film thickness 8.5μm 18μm Weight loss of 53% Ultra-thin coating technology Weight gain percentage 0.2% 1.2% Weight loss of 83% Lightweight Breakthrough Salt spray test 1500 hours 150 hours 900% increase Corrosion Resistance Revolution bonding force 25MPa 12MPa Increased by 108% Interface design optimization Environmental performance Chromium-free and environmentally friendly Chromium pollution Environmentally friendly Green processes Surface quality High gloss, decorative Grayish white, not suitable for decoration Superior appearance Improved decorative performance Process energy consumption Low high 55% energy saving Energy-saving technology
[0116] As shown in Table 6, the technology of this invention surpasses the traditional anodizing process in terms of lightweighting, corrosion resistance, and environmental friendliness.
[0117] Comparative Example 3b: Simplified process steps.
[0118] Process differences: The nanosol-gel coating and atomic layer deposition steps are omitted.
[0119] The performance comparison table is shown in Table 7 below:
[0120] Table 7
[0121] Performance items Example 3 Comparative Example 3b Performance degradation Cause Analysis Salt spray test 1500 hours 800 hours -47% Loss of the protective effect of the nano-coating hardness 380HV 280HV -26% Nano-reinforcement effect disappears abrasion resistance good generally -40% Decreased surface hardness and wear resistance
[0122] As shown in Table 7, a complete multilayer composite structure is a necessary condition to ensure the overall performance of the coating. Each layer has complementary functions and none can be omitted.
[0123] Through comparative analysis of multiple examples, the following important conclusions can be drawn:
[0124] The importance of process parameter optimization: Key parameters such as plasma activation time and curing temperature have a significant impact on performance, and each parameter needs to be precisely adjusted according to the application scenario;
[0125] Advantages of the material system: The addition of rare earth elements significantly improves corrosion resistance and high temperature resistance, and nano-coating technology is the key to performance breakthrough;
[0126] The necessity of process integrity: The functions of each layer in a multi-layer composite structure are complementary and indispensable. Simplifying the process will lead to a significant decrease in performance.
[0127] Comprehensive technological advantages: Compared with traditional technologies, this invention is comprehensively superior in terms of lightweight, corrosion resistance, and environmental friendliness, with a service life extended by 2-3 times and a significantly improved overall cost performance;
[0128] As can be seen from the above embodiments, the corrosion-resistant film and its preparation method for magnesium alloy flying car fuselage frame components provided by the present invention meet or exceed aerospace-grade standards in terms of lightweighting, corrosion resistance, bonding strength, high temperature resistance, and mechanical properties, and fully meet the stringent requirements of flying cars.
[0129] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the present invention.
Claims
1. A method for preparing corrosion-resistant thin films suitable for magnesium alloy fuselage frame components, characterized in that, Includes the following steps: Step 1: High-precision substrate pretreatment: The magnesium alloy substrate undergoes precision mechanical pretreatment, ultrasonic enhanced cleaning and degreasing, multi-stage pure water washing and purification, controllable acid pickling and activation treatment, secondary pure water washing and surface condition control in sequence. Step 2, Lightweight Composite Membrane Formation: Gradient transition layer formation, plasma-enhanced activation, rare earth-silane composite anti-corrosion layer formation, and precision pure water washing are performed sequentially. Step 3, Functionalization Modification: The nanosol-gel coating is prepared and the gradient intelligent pore sealing treatment is carried out sequentially; Step 4, Precision Curing Process: Microwave-assisted precision curing, segmented precision curing, and surface functionalization nano-modification are performed sequentially.
2. The method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components according to claim 1, characterized in that, The precision mechanical pretreatment involves progressive polishing using 800-2000 grit diamond sandpaper until the surface roughness reaches Ra≤0.
03. .
3. The method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components according to claim 1, characterized in that, The ultrasonic-enhanced cleaning and degreasing process uses an environmentally friendly degreasing agent, and ultrasonic cleaning and degreasing are performed at 40-60℃ for 5-15 minutes. The environmentally friendly degreasing agent is composed of 2.5% sodium hydroxide or 25g / L sodium carbonate, 8g / L sodium silicate, 1.2% fatty alcohol polyoxyethylene ether, 0.6g / L benzotriazole, and deionized water. The ultrasonic-enhanced cleaning and degreasing process uses a three-tank ultrasonic cleaner with an ultrasonic frequency of 40kHz and a power of 500W.
4. The method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components according to claim 1, characterized in that, The controlled acid pickling and activation treatment uses a precision activation solution and is performed at room temperature for 30 seconds to 2 minutes. The precision activation solution consists of 3-10 wt% hydrofluoric acid, 2.5% citric acid, 2 g / L sodium benzoate, 1.5 g / L EDTA-2Na, 1.2 g / L cocamidopropyl betaine, and deionized water. The controlled acid pickling and activation treatment uses a precision chemical treatment tank equipped with an automatic temperature control and stirring system, and a magnetic stirring speed of 100 r / min.
5. The method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components according to claim 1, characterized in that, The gradient transition layer is formed using a gradient transition layer treatment solution, which is applied at 45-55℃ for 3-8 minutes. The gradient transition layer treatment solution consists of 5 g / L potassium fluorotitanate, 7 g / L potassium fluorozirconate, 12 g / L sodium nitrate, citric acid to adjust the pH to 3.2-3.8, and deionized water. The plasma-enhanced activation is carried out in a high-vacuum plasma treatment device, with high-purity argon as the working gas, a vacuum degree of 1-10 Pa, a power of 100-350 W, and a treatment time of 5-20 minutes.
6. The method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components according to claim 1, characterized in that, The rare earth-silane composite anti-corrosion layer is formed using a lightweight composite film-forming agent, and is immersed for 30 minutes at 60°C and pH 3.0-4.5; the lightweight composite film-forming agent is composed of... The rare earth-silane composite anti-corrosion layer is composed of 10% aminopropyltriethoxysilane, 3% cerium nitrate, 4g / L lanthanum nitrate, 4% tetrabutyl titanate, 1.5% hexafluorozirconic acid, 10g / L azelaic acid, and deionized water. The rare earth-silane composite anti-corrosion layer is formed using a precision automatic dip coating machine equipped with a CCD positioning system. The environment is controlled in a cleanroom of Class 1000, with a temperature of 25±1℃ and a humidity of 40±5%RH.
7. The method for preparing a corrosion-resistant thin film suitable for magnesium alloy fuselage frame components according to claim 1, characterized in that, The nano-sol-gel coating is prepared using a precision dip-coating method with a lifting speed of 12 cm / min. The nano-sol-gel solution consists of 20-30% tetraethyl orthosilicate, 5-10% tetrabutyl titanate, 40-50% ethanol, 0.5-2% nitric acid, 1% nano-silica, and 10-15% deionized water. The nano-sol-gel coating is prepared under nitrogen protection, and ultrasonic treatment for 30 minutes is used during solution preparation to ensure uniform dispersion of nanoparticles.
8. The corrosion-resistant thin film for magnesium alloy fuselage frame components according to claim 1, and its preparation method, characterized in that, The gradient intelligent sealing process includes: First sealing step: 7% silica sol, treated at 70℃ for 15 minutes; Second sealing step: 5% silane ethanol solution, treated at room temperature for 8 minutes.
9. The corrosion-resistant thin film suitable for magnesium alloy fuselage frame components according to claim 1, and its preparation method, characterized in that, The microwave-assisted precision curing adopts a program-controlled stepped heating process with a power of 300-600W, a curing temperature of 100-180℃, and a curing time of 15-45 minutes. The microwave-assisted precision curing uses an industrial-grade microwave curing oven equipped with an infrared thermometer to monitor the sample temperature in real time, with a temperature uniformity of ±3℃; the segmented precision curing includes: a first stage of pre-baking at 120℃ for 25 minutes, and a second stage of curing at 170℃ for 30 minutes. The surface functionalization nano-modification is performed using an atomic layer deposition system, depositing... Composite coating or The composite coating has a thickness of 50-200 nm and a deposition temperature of 150 °C, using trimethylaluminum and tetrazirconium as precursors.
10. A corrosion-resistant thin film suitable for magnesium alloy flying car fuselage frame components, prepared by the method according to any one of claims 1-9, characterized in that, The film has a multilayer composite structure with a total thickness of 8-12 mm. The coating comprises, from the magnesium alloy substrate outwards, a gradient transition layer, a rare earth-silane composite anti-corrosion layer, a nano-sol-gel coating, a gradient sealing layer, and a surface-functionalized nano-coating; the magnesium alloy substrate is selected from at least one of AZ91D, WE43, AZ31B, and AM60B.