A mixed-crystalline black stone glaze coating and its preparation method

The multi-layered mixed-crystalline black stone glaze coating solves the problems of low bonding strength and poor protective effect of the boiler heating surface coating, achieving high-strength bonding and improved protective performance, thus ensuring the safe and stable operation of the boiler.

CN123108565APending Publication Date: 2026-11-17QIYU (ZHENGZHOU) TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611358573.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-09-01
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing boiler heating surface coatings suffer from problems such as low bonding strength, rough and dense surface, and poor protective effect in terms of high-temperature corrosion and coking/slagging. In particular, tube ruptures frequently occur under complex coal quality conditions.

Method used

The mixed-crystalline black stone glaze coating with a multi-layer structure includes an activated metal layer, a transitional bonding layer, a nano-ceramic layer, and a glaze layer. Through the combination of materials such as silane coupling agents, composite binders, and fluorine-modified nano-titanium sol, a three-dimensional titanium dioxide network structure is formed, which encapsulates glassy materials and ceramic particles, achieving low-temperature sintering and high-strength bonding.

Benefits of technology

It improves the bonding strength and cohesive strength between the coating and the substrate, and has a smooth and dense surface. It has excellent resistance to high-temperature sulfur corrosion, erosion and wear, and anti-coking and anti-slagging properties, thus improving the safe and stable operation of the boiler.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of surface modification technology, specifically relating to a mixed-crystalline black stone glaze coating and its preparation method. This invention solves the problems of low bonding strength between conventional coatings and substrates, low cohesive strength due to the inability of the coating to effectively sinter at operating temperatures, and rough, dense surfaces by designing a multi-layered, multi-phase mixed sintering coating (in specific applications, it can undergo self-catalytic sintering at the operating temperature of the boiler heating surface). It also addresses the problem that conventional anti-coking and slag-forming coatings rely solely on adding low-surface-energy particles, but these particles cannot effectively self-sinter and connect into sheets at the coating's operating temperature, remaining in point contact or isolated states within the coating and failing to form a low-surface-energy surface, resulting in poor anti-coking and slag-forming effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of surface modification technology, specifically relating to a mixed-crystal black stone glaze coating and its preparation method. Background Technology

[0002] With significant fluctuations in coal prices, the quality of coal fed into large power plant coal-fired boilers has become increasingly complex and variable. The large-scale blending of high-sulfur and high-alkali metal coal results in flue gas containing substantial amounts of sulfur and alkali metals, while the ash contains high levels of sulfates and sulfites. These substances adhere to the boiler's heating surfaces and, under the influence of the high-temperature flue gas, cause severe high-temperature corrosion, coking, and slagging. Especially with the increasing frequency of flexible peak-shaving in thermal power units, the operating conditions of boilers are constantly deteriorating, exacerbating the thinning of boiler heating surface tubes and leading to frequent tube ruptures, seriously threatening the safe and stable operation of the boilers.

[0003] To protect boiler heating surfaces from corrosion by high-temperature sulfur and alkali metals, as well as from the erosion by flue gas ash, a common technique is to form a protective coating on the tube surface. This coating resists or absorbs the erosion by corrosive media and the erosion by flue gas ash, preventing direct damage to the tubes. Currently used protective methods include supersonic arc spraying alloy coatings, tube screen cladding welding alloy layers, and cold spraying nano-ceramic coatings, all of which have achieved certain protective effects. However, supersonic arc spraying alloy coatings have high internal porosity, allowing corrosive media to easily penetrate, and their large surface roughness exacerbates coking and slagging. Tube screen cladding welding technology offers excellent protective performance, but it requires prefabricated components and on-site welding installation, which is cumbersome and costly. Its large surface roughness also makes it prone to coking and slagging. While cold-sprayed nano-ceramic coatings are easy to apply, they require rigorous pretreatment of the substrate and involve high sintering temperatures. However, the actual surface temperature during tube panel operation often fails to reach the required sintering temperature, resulting in poor sintering performance and difficulty in achieving the desired surface hardness and adhesion. To address these issues, a novel protective coating needs to be developed that features simple application, high bonding strength with the heated substrate, low-temperature sintering capability, a smooth and dense surface, and resistance to high-temperature corrosion, wear, and coking / slag formation. Summary of the Invention

[0004] The purpose of this invention is to provide a mixed-crystalline black stone glaze coating and its preparation method.

[0005] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing a mixed-crystalline black stone glaze coating, comprising the following steps: After sequentially preparing an activated metal layer, a transition bonding layer, a nano-ceramic layer, and a glaze layer on the substrate surface, sintering is performed to obtain the mixed-crystal black stone glaze layer. The raw materials for the transition bonding layer include silane coupling agent, sodium carboxymethyl cellulose and ceramic whiskers; The raw materials for the nano-ceramic layer include composite binders, ceramic powder, and metal powder; The raw materials for the glaze include fluorine-modified nano-titanium sol, glass powder, metal powder, nano-boron carbide, and cobalt green powder.

[0006] Preferably, the raw material for the activated metal layer includes at least one of aluminum, titanium, and silicon; The thickness of the activated metal layer is 20~60μm.

[0007] Preferably, the silane coupling agent includes at least one of KH550, KH560 and KH570; The ceramic whiskers include at least one of potassium titanate whiskers, silicon carbide whiskers, and alumina whiskers.

[0008] Preferably, the raw materials of the transition adhesive layer, by mass parts, include 1-3 parts of silane coupling agent, 25-70 parts of sodium carboxymethyl cellulose, and 10-30 parts of ceramic whiskers; The thickness of the transition adhesive layer is 20~50μm.

[0009] Preferably, the composite binder comprises an aqueous organosilicon-modified inorganic binder; the inorganic binder in the aqueous organosilicon-modified inorganic binder comprises at least one of potassium silicate, sodium silicate, and potassium-sodium silicate. The ceramic powder includes at least one of nepheline powder, silicon carbide powder, and transition metal oxide powder; the transition metal oxide powder includes at least one of chromium trioxide, cobalt oxide, manganese oxide, and molybdenum oxide. The metal powder in the nano-ceramic layer includes at least one of chromium powder, nickel powder, and titanium powder.

[0010] Preferably, by mass parts, the raw materials of the nano-ceramic layer include 20-50 parts of composite binder, 5-30 parts of ceramic powder and 5-10 parts of metal powder; The thickness of the nano-ceramic layer is 50~100μm.

[0011] Preferably, the glass powder is a low-melting-point glass powder, and the initial softening temperature of the low-melting-point glass powder is 400°C. The metal powder in the glaze includes at least one of aluminum powder and bismuth powder.

[0012] Preferably, by mass parts, the raw materials of the glaze layer include 30-50 parts of fluorine-modified nano-titanium sol, 10-30 parts of glass powder, 5-10 parts of metal powder, 3-10 parts of nano-boron carbide and 5-15 parts of cobalt green powder; The thickness of the glaze layer is 50~150μm.

[0013] Preferably, the sintering temperature is 350~600℃ and the holding time is 2~4h.

[0014] The present invention also provides a mixed-crystalline black stone glaze coating prepared by the preparation method described above, wherein the mixed-crystalline black stone glaze coating uses a three-dimensional network structure of titanium dioxide as a skeleton, in which glassy substances, metals and ceramic particles are encapsulated.

[0015] Compared with the prior art, the beneficial effects of the present invention include: This invention solves the problems of low bonding strength between conventional coatings and substrates, low cohesive strength, and rough, dense surfaces caused by the inability of the coating to sinter effectively at operating temperatures, by designing a multi-layered, mixed-crystal coating (in specific applications, it can undergo self-catalytic sintering at the operating temperature of the boiler heating surface). At the same time, it solves the problem that conventional anti-coking and slag-forming coatings rely solely on adding low surface energy particles, but the particles cannot effectively self-sinter and connect into sheets at the coating's operating temperature. Instead, the particles remain in point contact or exist in isolation within the coating and cannot form a low surface energy surface, resulting in poor anti-coking and slag-forming effects. Detailed Implementation

[0016] This invention provides a method for preparing a mixed-crystalline black stone glaze coating, comprising the following steps: After sequentially preparing an activated metal layer, a transition bonding layer, a nano-ceramic layer, and a glaze layer on the substrate surface, sintering is performed to obtain the mixed-crystal black stone glaze layer. The raw materials for the transition bonding layer include silane coupling agent, sodium carboxymethyl cellulose and ceramic whiskers; The raw materials for the nano-ceramic layer include composite binders, ceramic powder, and metal powder; The raw materials for the glaze include fluorine-modified nano-titanium sol, glass powder, metal powder, nano-boron carbide, and cobalt green powder.

[0017] In this invention, the substrate preferably includes carbon steel, low alloy steel or stainless steel; before preparation, the invention also preferably includes sandblasting and rust removal pretreatment of the substrate.

[0018] In this invention, the raw material of the activated metal layer preferably includes at least one of aluminum, titanium, and silicon. The thickness of the activated metal layer is preferably 20-60 μm, specifically 20 μm, 30 μm, 40 μm, 50 μm, or 60 μm. The activated metal layer is preferably prepared by supersonic flame spraying or arc spraying. This invention does not impose any particular limitation on the supersonic flame spraying or arc spraying process; any process well-known to those skilled in the art can be used. In this invention, the layer contains a large amount of active metal, which can form a high-strength metallurgical bond with the substrate.

[0019] In this invention, the raw materials of the transition bonding layer include a silane coupling agent, sodium carboxymethyl cellulose, and ceramic whiskers; the silane coupling agent preferably includes at least one of KH550, KH560, and KH570; the ceramic whiskers preferably include at least one of potassium titanate whiskers, silicon carbide whiskers, and alumina whiskers. In this invention, by mass parts, the raw materials of the transition bonding layer preferably include 1-3 parts of silane coupling agent (specifically 1 part, 2 parts, or 3 parts), 25-70 parts of sodium carboxymethyl cellulose (specifically 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, or 70 parts), and 10-30 parts of ceramic whiskers (specifically 10 parts, 15 parts, 20 parts, 25 parts, or 30 parts). In this invention, the thickness of the transition adhesive layer is preferably 20~50μm, specifically 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, or 50μm.

[0020] In this invention, the preferred method for preparing the transition bonding layer includes: spraying a slurry containing a silane coupling agent, sodium carboxymethyl cellulose, and ceramic whiskers onto the surface of the activated metal layer, followed by drying and curing. In this invention, the solvent of the slurry preferably includes ethanol and water; the volume ratio of ethanol to water is preferably 1:5 to 10, specifically 1:5, 1:6, 1:7, 1:8, 1:9, or 1:10; the solid content of the slurry is preferably 50 to 70%, specifically 50%, 55%, 60%, 65%, or 70%. In this invention, the spraying is preferably performed using a high-pressure airless sprayer. This invention does not impose any special limitations on the drying and curing process; any process well-known to those skilled in the art can be used. In this invention, before spraying, it is also preferred to spray a layer of hydrogen peroxide solution onto the surface of the activated metal layer; the mass concentration of the hydrogen peroxide is preferably 20 to 40%, specifically 20%, 25%, 30%, 35%, or 40%, and the spraying amount is sufficient to completely cover the surface; by applying the hydrogen peroxide solution, a large number of active hydroxyl groups are further promoted to form on its surface.

[0021] In this invention, the transitional adhesive layer acts as a bridge. After the silane coupling agent in the layer is hydrolyzed, the hydroxyl groups at one end undergo a silanol condensation reaction with the hydroxyl groups of the activated metal layer to form strong silicon-oxygen bonds. The organic groups at the other end undergo a copolymerization reaction with the aqueous organosilicon in the nano-ceramic layer to form an interwoven three-dimensional network structure. In this invention, the raw materials of the nano-ceramic layer preferably include a composite binder, ceramic powder, and metal powder; the composite binder preferably includes an aqueous organosilicon-modified inorganic binder. In this invention, by weight, the raw materials of the nano-ceramic layer include 20-50 parts of composite binder (specifically 20, 25, 30, 35, 40, 45, or 50 parts), 5-30 parts of ceramic powder (specifically 5, 10, 15, 20, 25, or 30 parts), and 5-10 parts of metal powder (specifically 5, 6, 7, 8, 9, or 10 parts). In this invention, the thickness of the nano-ceramic layer is preferably 50-100 μm (specifically 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm).

[0022] In this invention, the waterborne organosilicon modified inorganic binder preferably contains acrylic-modified silicone resin; the acrylic-modified silicone resin preferably includes Wacker SILRES M 51 E waterborne organosilicon, Wacker SILRES BS 338 waterborne organosilicon, or Wacker SILRES MPF 52 E waterborne organosilicon; the inorganic binder preferably includes at least one of potassium silicate, sodium silicate, and potassium-sodium silicate; the potassium silicate is preferably of the type Foshan Zhongfa silicate ZFK29-44A.

[0023] In this invention, the preferred method for preparing the waterborne organosilicon-modified inorganic binder includes: adding waterborne organosilicon to an inorganic binder under stirring conditions, and sequentially dispersing, settling, and activating to obtain the waterborne organosilicon-modified inorganic binder. In this invention, the mass ratio of the waterborne organosilicon to the inorganic binder is 1:5~10, specifically 1:5, 1:6, 1:7, 1:8, 1:9, or 1:10; the stirring speed is preferably 500~1000 rpm, specifically 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, or 1000 rpm; the dispersion is preferably carried out under stirring conditions; the dispersion speed is preferably the same as the stirring speed specified above; the dispersion time is preferably 10~15 min; the settling time is preferably 30 min; the activation is preferably carried out under ultrasonic conditions; and the activation time is preferably 10~20 min.

[0024] In this invention, the ceramic powder preferably includes at least one selected from nepheline powder, silicon carbide powder, and transition metal oxide powder; the transition metal oxide powder preferably includes at least one selected from chromium trioxide, cobalt oxide, manganese oxide, and molybdenum oxide. In this invention, the metal powder preferably includes at least one selected from chromium powder, nickel powder, and titanium powder.

[0025] In this invention, the preferred method for preparing the nano-ceramic layer includes: mixing a composite binder, ceramic powder, metal powder, defoamer, wetting and dispersing agent, and water to obtain a slurry; and spraying the slurry onto the surface of the transition bonding layer for drying and curing. In this invention, the defoamer preferably includes Tuyile® acetylenic diol diluted surfactant, specifically preferably FS-204X acetylenic diol solution additive, and the content of the defoamer is preferably 0.5~1.5 parts (specifically, 0.5 parts, 0.8 parts, 1.0 parts, 1.2 parts, or 1.5 parts); the wetting and dispersing agent preferably includes Tuyile® HD-2202 wetting and dispersing agent, and the content of the wetting and dispersing agent is preferably 0.5~1.5 parts (specifically, 0.5 parts, 0.8 parts, 1.0 parts, 1.2 parts, or 1.5 parts); the water is preferably deionized water, and the content of the water is preferably 20~50 parts (specifically, 20 parts, 30 parts, 40 parts, or 50 parts). In this invention, the mixing is preferably carried out under stirring conditions. In this invention, the spraying is preferably performed using a high-pressure airless sprayer. This invention does not impose any particular limitations on the drying and curing process; any process well-known to those skilled in the art can be used.

[0026] In this invention, the composite binder undergoes chemical cross-linking after blending (referring to the use of water-based organosilicon-modified inorganic binder) to form silicon-oxygen covalent bonds, and organic groups are grafted onto these silicon-oxygen bonds, increasing the toughness and density of the binder. This, in turn, improves the toughness and density of the nano-ceramic layer, preventing coating cracking. Simultaneously, the organosilicon coats the surface of the inorganic binder gel, hindering gel grain growth, increasing the particle surface area of ​​the composite binder, and improving bonding strength. Furthermore, the water-based organosilicon copolymerizes with the organic groups of the silane coupling agent in the transition adhesive layer, forming an interwoven three-dimensional network structure. The ceramic whiskers in the transition adhesive layer possess high strength and good fracture toughness, forming an interwoven three-dimensional network, further enhancing the bridging effect of the transition adhesive layer. That is, through the transition bonding effect of the second layer, the third nano-ceramic layer is firmly connected to the first activated metal layer, thereby indirectly improving the bonding strength between the nano-ceramic coating and the substrate, and the cohesive strength of the entire composite coating.

[0027] In this invention, the raw materials of the glaze layer preferably include fluorine-modified nano-titanium sol, glass powder, metal powder, nano-boron carbide, and cobalt green powder. In this invention, by mass parts, the raw materials of the glaze layer preferably include 30-50 parts of fluorine-modified nano-titanium sol (specifically 30, 35, 40, 45, or 50 parts), 10-30 parts of glass powder (specifically 10, 15, 20, 25, or 30 parts), 5-10 parts of metal powder (specifically 5, 6, 7, 8, 9, or 10 parts), 3-10 parts of nano-boron carbide (specifically 3, 4, 5, 6, 7, 8, 9, or 10 parts), and 5-15 parts of cobalt green powder (specifically 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts). In this invention, the thickness of the glaze layer is preferably 50~150μm (specifically, it can be 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, or 150μm).

[0028] In this invention, the fluorine-modified nano-titanium sol is preferably obtained through preparation. The preparation method preferably includes: mixing a silane coupling agent and a titanium sol for surface modification to obtain a modified titanium sol; and adding an aqueous fluorocarbon resin to the modified titanium sol for grafting to obtain the fluorine-modified nano-titanium sol. In this invention, the silane coupling agent preferably includes at least one of KH550, KH560, and KH570; the titanium sol is preferably of type CY-T30R (Hangzhou Jiupeng New Materials); the aqueous fluorocarbon resin is preferably of type HLR-WR02 (Shandong Huafu Chemical Co., Ltd.); and the mass of the silane coupling agent is preferably 2-5% of the mass of the titanium sol (specifically, it can be 2%, 3%, 4%, or 5%). In this invention, the surface modification is preferably performed under ultrasonic conditions, with the ultrasonic temperature preferably being 50-80°C (specifically, 50°C, 60°C, 70°C, or 80°C) and the time preferably being 0.5-1 h (specifically, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, or 1 h). In this invention, the mass ratio of waterborne fluorocarbon resin to modified titanium sol is preferably 1:3-10 (specifically, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, or 1:10); the grafting is preferably performed under ultrasonic conditions, with the ultrasonic temperature preferably being 40-60°C (specifically, 40°C, 50°C, or 60°C). In this invention, a silane coupling agent is used to modify the surface of the titanium sol. The hydroxyl groups of the silane coupling agent condense with the hydroxyl groups on the surface of the titanium dioxide particles, thereby grafting organic groups onto the surface of the titanium dioxide particles. Furthermore, an aqueous fluorocarbon resin is slowly added to the titanium sol modified with the silane coupling agent. The main chain of the fluorocarbon resin entangles with the organic groups of the silane coupling agent, thereby attaching fluorine atoms to the surface of the titanium dioxide particles.

[0029] In this invention, the glass powder is preferably a low-melting-point glass powder, and the initial softening temperature of the low-melting-point glass powder is preferably 400℃ (close to the surface working temperature of the tube screen); the type of the low-melting-point glass powder is preferably SAMASOGW-6350 (Foshan Kedeli Chemical Technology Co., Ltd., whose product description states a glass transition temperature of 300℃, but in actual use it has been found that it needs to reach 400℃ to begin softening) or 1140 low-melting-point glass powder from Foshan Youhe Chemical Technology Co., Ltd. In this invention, the metal powder preferably includes at least one of aluminum powder and bismuth powder.

[0030] In this invention, the preferred method for preparing the glaze layer includes: mixing fluorine-modified nano-titanium sol, glass powder, metal powder, nano-boron carbide, cobalt green powder, defoamer, wetting and dispersing agent and water to obtain a slurry; and spraying the slurry onto the surface of the nano-ceramic layer for drying and curing. In this invention, the defoamer preferably includes Tuyile® acetylenic diol diluted surfactant, specifically preferably FS-204X acetylenic diol solution additive, and the content of the defoamer is preferably 0.5~1.5 parts (specifically 0.5 parts, 0.8 parts, 1.0 parts, 1.2 parts, or 1.5 parts); the wetting and dispersing agent preferably includes Tuyile® HD-2202 wetting and dispersing agent, and the content of the wetting and dispersing agent is preferably 0.5~1.5 parts (specifically 0.5 parts, 0.8 parts, 1.0 parts, 1.2 parts, or 1.5 parts); the water is preferably deionized water, and the content of the water is preferably 20~50 parts (specifically 20 parts, 30 parts, 40 parts, or 50 parts). In this invention, the mixing is carried out under stirring conditions; the spraying is preferably carried out using a high-pressure airless sprayer. This invention does not have special limitations on the drying and curing process; any process well known to those skilled in the art can be used.

[0031] In this invention, fluorine-modified nano-titanium sol exhibits extremely high catalytic activity, forming hydrogen bonds or covalent bonds with metal powder, thus improving the toughness and density of the three-dimensional network formed after the titanium sol solidifies. Simultaneously, fluorine atoms in the fluorine-modified nano-titanium sol replace some oxygen atoms. Due to the extremely high electronegativity of fluorine atoms, the resulting titanium fluoride compound has very low polarity and surface energy. The dense three-dimensional network formed after solidification possesses extremely high chemical stability and extremely low surface energy, acting like a dense insulating net, preventing ash and slag from adhering and taking root on its surface. Combined with the smooth and flat surface structure of the glaze layer, it exhibits extremely high anti-ash and slag adhesion performance. This solves the problem of traditional anti-coking coatings relying solely on the addition of low surface energy fillers, where filler particles cannot effectively sinter and connect into sheets below the tube wall temperature of 700℃, remaining essentially in physical point contact or even existing in isolated particle form, significantly reducing the anti-ash and slag adhesion effect.

[0032] In this invention, the metal powder and glass powder in the glaze layer undergo a solid solution reaction to form a multiphase structure in which the amorphous glass phase encapsulates the metal phase, exhibiting high toughness. Cobalt green powder promotes the dissolution of oxides formed from the oxidation of the metal powder within the amorphous glass phase. The spinel structure of the cobalt green powder exhibits good compatibility with the three-dimensional network formed after the titanium sol in the nano-ceramic layer solidifies, improving the strength and density of the coating. Simultaneously, the oxidation of nano-boron carbide to form boron oxide promotes the softening and flow of the glass powder, enhancing mass transfer sintering within the coating.

[0033] In this invention, the substrate is preferably a boiler heating surface, preferably a tube screen, and more preferably a 15CrMoG tube screen. In this invention, the sintering temperature is preferably 350~600℃ (specifically preferably 350℃, 400℃, 450℃, 500℃, 550℃, or 600℃), and the holding time is preferably 2~4h (specifically 2h, 3h, or 4h). In this invention, the sintering is preferably carried out during the use of the boiler; that is, after preparing the activated metal layer, transition bonding layer, nano-ceramic layer, and glaze layer on the boiler heating surface, sintering can be completed during the subsequent heating process of the boiler, forming a mixed-crystalline black stone glaze layer on the surface of the heating surface.

[0034] In this invention, as the boiler heating surface heats up, the low-melting-point glass powder begins to soften, while the metal powder (glaze layer) begins to melt. Nano-boron carbide reacts in situ with oxygen in the flue gas to form nano-boron oxide, which acts as a flux for the low-melting-point glass powder, further promoting its softening, flow, and mass transfer. After melting, the metal powder partially dissolves in the glass powder and undergoes a complex solid solution reaction, forming fine crystalline dendrites. The microstructure consists of a glassy amorphous phase encapsulating a metallic phase. During heating and cooling, the uniformly distributed metallic phase can induce multiple local shear bands, dispersing thermal stress. The metallic phase can also block or deflect microcrack propagation paths, improving the toughness of the glaze layer and preventing cracking during long-term high-temperature application. The high coefficient of thermal expansion of nepheline powder, combined with the addition of the metal powder (ceramic layer), effectively adjusts the coefficient of thermal expansion of the ceramic layer, bringing it close to that of the tube screen, further reducing thermal stress. Simultaneously, nano-boron carbide undergoes solid-liquid phase mixing and sintering with low-melting-point glass powder, metal powder (ceramic layer and glaze layer), and titanium sol, ultimately forming a smooth and dense glaze layer in situ that encapsulates the glass phase, metal phase, and crystalline phase with titanium sol as a network, thus forming a mixed-crystalline black stone glaze coating.

[0035] Meanwhile, the softened, flowing glass phase, under capillary action, partially fills the capillary pores remaining in the third nano-ceramic coating due to the curing and dehydration of the composite binder and water evaporation. It reacts with the metal powder in the third layer, raising the softening temperature and achieving in-situ solidification within the capillary pores. This also promotes the in-situ sintering of the third nano-ceramic layer, improving its density. In the fourth glaze layer, cobalt green powder promotes the dissolution of oxides formed after the oxidation of the metal powder in the third layer within the glaze. Furthermore, its spinel crystal structure exhibits good compatibility with the three-dimensional network formed after the titanium sol solidifies, improving the network's strength and density. This further enhances the bonding strength and density between the third and fourth layers. Simultaneously, cobalt can adjust the electrode potential of the glaze layer, reducing its activity in corrosive environments and improving the high-temperature corrosion resistance of the composite coating.

[0036] In summary, through the interaction of the first, second, third, and fourth layers, a mixed-crystalline black stone glaze coating composed of ceramic crystalline phase, metallic phase, and glass amorphous phase is finally formed on the substrate surface. This coating is smooth and dense, with high chemical inertness and low surface energy, high bonding strength with the substrate, high cohesive strength, high surface hardness, and a certain degree of toughness. It exhibits excellent resistance to high-temperature sulfur corrosion, erosion wear, and anti-coking and slagging properties. Its high emissivity can greatly improve the flue gas radiative heat absorption capacity of the tube screen, resulting in energy saving and efficiency improvement.

[0037] The present invention also provides a mixed-crystalline black stone glaze coating prepared by the preparation method described above, wherein the mixed-crystalline black stone glaze coating uses a three-dimensional network structure of titanium dioxide as a skeleton, in which glassy substances, metals and ceramic particles are encapsulated.

[0038] Unless otherwise specified, the materials and equipment used in this invention are all commercially available products in the field.

[0039] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0040] In the following examples, the defoamer is FS-204X acetylenic diol solution additive, and the wetting and dispersing agent is preferably Tuyile® HD-2202 wetting and dispersing agent; The tube screen is a 15CrMoG tube screen.

[0041] The model number of the potassium silicate is: Foshan Zhongfa Water Glass ZFK29-44A; The model of the titanium sol is: CY-T30R (Hangzhou Jiupeng New Materials). The model of the waterborne fluorocarbon resin is: HLR-WR02 (Shandong Huafu Chemical Co., Ltd.). The model number of the low melting point glass powder is: SAMASOGW-6350 (Foshan Kedeli Chemical Technology Co., Ltd.).

[0042] Example 1 The surface of the tube screen is pretreated by sandblasting to remove rust, and a 40μm thick aluminum activated metal layer is sprayed by supersonic flame. A layer of hydrogen peroxide solution (mass concentration of 25%) was uniformly sprayed onto the surface of the activated metal layer. 50 parts of sodium carboxymethyl cellulose, 1.5 parts of KH550 silane coupling agent, 15 parts of silicon carbide whiskers, and a mixture of ethanol and water were placed in a high-speed mixer and stirred into a slurry (the volume ratio of ethanol to water was 1:5, and the solid content of the slurry was 60%). The slurry was then sprayed onto the surface of the activated metal layer using a high-pressure airless sprayer. After drying, a transition bonding layer with a thickness of 30 μm was formed. Potassium silicate was modified using Wacker SILRES M 51 E water-based silicone (potassium silicate was weighed and placed in a container, a high-speed disperser was turned on at 600 rpm, Wacker SILRES M 51 E water-based silicone was slowly added, dispersed at high speed for 10 min, allowed to stand for 30 min, and then activated by ultrasound for 10 min, wherein the mass ratio of water-based silicone to potassium silicate was 1:8) to form a composite binder. 25 parts of the composite binder, 10 parts of nepheline powder, 5 parts of silicon carbide powder, 5 parts of chromium trioxide powder, 10 parts of a mixture of cobalt oxide powder and manganese oxide powder (where the mass ratio of cobalt oxide powder to manganese oxide powder was 5:1), 5 parts of nano nickel powder, 20 parts of deionized water, 1 part of defoamer, and 0.5 parts of wetting and dispersing agent were put into a high-speed mixer and stirred into a slurry. The slurry was sprayed onto the surface of the transition adhesive layer using a high-pressure airless sprayer. After drying and curing, a nano-ceramic layer with a thickness of 80 μm was formed. 30 parts of fluorine-modified titanium sol (2 parts of KH550 silane coupling agent and 80 parts of titanium sol were mixed and surface modified under ultrasonic conditions to obtain modified titanium sol, where the temperature was 50℃ and the time was 0.5h; 10 parts of water-based fluorocarbon resin were slowly added to the modified titanium sol and grafted under ultrasonic conditions to obtain fluorine-modified titanium sol, where the temperature was 40℃), 20 parts of low melting point glass powder (initial softening temperature of 400℃), 10 parts of nano aluminum powder, 5 parts of nano boron carbide powder, 8 parts of cobalt green powder, 30 parts of deionized water, 1.5 parts of defoamer, and 1 part of wetting and dispersing agent were added to a high-speed mixer and stirred into a slurry. The slurry was sprayed onto the surface of the nano-ceramic layer, and after drying, curing and sintering, a glaze layer with a thickness of 100μm was formed. Then, sintering is carried out at 400℃ for 2 hours to form a mixed-crystalline black stone glaze coating with a thickness of 250μm.

[0043] Example 2 The surface of the tube screen is pretreated by sandblasting to remove rust, and a layer of aluminum-silicon (mass ratio of 3:1) activation metal layer with a thickness of 50μm is applied by supersonic arc spraying. A layer of hydrogen peroxide solution (mass concentration of 30%) was uniformly sprayed onto the surface of the activated metal layer. 30 parts of sodium carboxymethyl cellulose, 2 parts of KH560 silane coupling agent, 15 parts of alumina whiskers, and a mixture of ethanol and water were placed in a high-speed mixer and stirred into a slurry (the volume ratio of ethanol to water was 1:8, and the solid content of the slurry was 70%). The slurry was then sprayed onto the surface of the activated metal layer using a high-pressure airless sprayer. After drying, a transition bonding layer with a thickness of 50 μm was formed. A composite binder was formed by modifying potassium silicate with Wacker SILRES BS 338 waterborne silicone (potassium silicate was weighed and placed in a container, a high-speed disperser was turned on at 700 rpm, Wacker SILRES BS 338 waterborne silicone was slowly added, the mixture was dispersed at high speed for 15 min, allowed to stand for 30 min, and then activated by ultrasound for 15 min, wherein the mass ratio of waterborne silicone to potassium silicate was 1:6). 30 parts of the composite binder, 10 parts of nepheline powder, 5 parts of silicon carbide powder, 5 parts of chromium trioxide powder, 10 parts of a mixture of cobalt oxide powder and molybdenum oxide powder (where the mass ratio of cobalt oxide powder to molybdenum oxide powder was 6:1), 5 parts of nano-chromium powder, 40 parts of deionized water, 0.8 parts of defoamer, and 1.3 parts of wetting and dispersing agent were put into a high-speed mixer and stirred into a slurry. The slurry was sprayed onto the surface of the transition adhesive layer using a high-pressure airless sprayer. After drying and curing, a nano-ceramic layer with a thickness of 60 μm was formed. 35 parts of fluorine-modified titanium sol (3 parts of KH560 silane coupling agent and 80 parts of titanium sol were mixed and surface modified under ultrasonic conditions to obtain modified titanium sol, with a temperature of 50℃ and a time of 0.5h; 15 parts of waterborne fluorocarbon resin were slowly added to the modified titanium sol and grafted under ultrasonic conditions to obtain fluorine-modified titanium sol, with a temperature of 50℃), 20 parts of low melting point glass powder (initial softening temperature of 400℃), 10 parts of nano bismuth powder, 8 parts of nano boron carbide powder, 10 parts of cobalt green powder, 30 parts of deionized water, 0.8 parts of defoamer, and 1.5 parts of wetting and dispersing agent were added to a high-speed mixer and stirred into a slurry. The slurry was sprayed onto the surface of the nano-ceramic layer, and after drying, curing, and sintering, a glaze layer with a thickness of 100μm was formed. Then, sintering was carried out at 450℃ for 3 hours to form a mixed-crystalline black stone glaze coating with a thickness of 260μm.

[0044] Example 3 The surface of the tube screen is pretreated by sandblasting to remove rust, and a 30μm thick aluminum-titanium (mass ratio 2:1) activated metal layer is sprayed by supersonic flame. A layer of hydrogen peroxide solution (40% by mass) was uniformly sprayed onto the surface of the activated metal layer. 25 parts of sodium carboxymethyl cellulose, 1.5 parts of KH570 silane coupling agent, 10 parts of potassium titanate whiskers, and a mixture of ethanol and water were placed in a high-speed mixer and stirred into a slurry (the volume ratio of ethanol to water was 1:5, and the solid content of the slurry was 65%). The slurry was then sprayed onto the surface of the activated metal layer using a high-pressure airless sprayer. After drying, a transition bonding layer with a thickness of 40 μm was formed. A composite binder was formed by modifying potassium silicate with Wacker SILRES MPF 52 E aqueous silicone (potassium silicate was weighed and placed in a container, a high-speed disperser was turned on at 800 rpm, Wacker SILRES BS 338 aqueous silicone was slowly added, the mixture was dispersed at high speed for 15 min, allowed to stand for 30 min, and then activated by ultrasound for 15 min, wherein the mass ratio of aqueous silicone to potassium silicate was 1:6). 35 parts of the composite binder, 15 parts of nepheline powder, 3 parts of silicon carbide powder, 5 parts of chromium trioxide powder, 5 parts of cobalt oxide powder, molybdenum oxide powder and manganese oxide powder mixture (where the mass ratio of cobalt oxide powder, molybdenum oxide powder and manganese oxide powder was 1:1:1), 5 parts of nano titanium powder, 40 parts of deionized water, 1 part of defoamer, and 1 part of wetting and dispersing agent were put into a high-speed mixer and stirred into a slurry. The slurry was sprayed onto the surface of the transition adhesive layer using a high-pressure airless sprayer. After drying and curing, a nano-ceramic layer with a thickness of 50 μm was formed. 45 parts of fluorine-modified titanium sol (3 parts of KH570 silane coupling agent and 80 parts of titanium sol were mixed and surface modified under ultrasonic conditions to obtain modified titanium sol, with a temperature of 50℃ and a time of 0.5h; 20 parts of waterborne fluorocarbon resin were slowly added to the modified titanium sol and grafted under ultrasonic conditions to obtain fluorine-modified titanium sol, with a temperature of 60℃), 15 parts of low melting point glass powder (initial softening temperature of 400℃), 5 parts of nano bismuth powder, 8 parts of nano boron carbide powder, 8 parts of cobalt green powder, 30 parts of deionized water, 1 part of defoamer, and 1 part of wetting and dispersing agent were added to a high-speed mixer and stirred into a slurry. The slurry was sprayed onto the surface of the nano-ceramic layer, and after drying, curing, and sintering, a glaze layer with a thickness of 150μm was formed. Then, sintering is carried out at 500℃ for 3 hours to form a mixed-crystalline black stone glaze coating with a thickness of 270μm.

[0045] Comparative Example 1 A mixed-crystalline black stone glaze coating was prepared according to the method of Example 1, excluding the active metal layer.

[0046] Comparative Example 2 A mixed-crystalline black stone glaze coating was prepared according to the method of Example 1, excluding the transition bonding layer.

[0047] Comparative Example 3 A mixed-crystalline black stone glaze coating was prepared according to the method of Example 1, excluding the glaze layer.

[0048] Performance testing The performance of the coating obtained above was tested, and the test results are shown in Table 1. Table 1 Performance test results of the coatings obtained in the examples and comparative examples

[0049] As shown in Table 1, compared with Comparative Example 1, the adhesion of the coating was significantly improved after using the active adhesive layer in Example 1, and the resistance to molten salt corrosion was also improved to some extent. Compared with Comparative Example 2, the adhesion of the coating was significantly improved after using the transition adhesive layer in Example 1, and the resistance to molten salt corrosion was also improved to some extent. Compared with Comparative Example 3, the adhesion of the coating was improved to some extent after using the glaze layer in Example 1, and the hardness and resistance to molten salt corrosion of the coating were greatly improved, while the wetting angle and hemispherical emissivity were also improved to some extent.

[0050] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a mixed-crystalline black stone glaze coating, characterized in that, Includes the following steps: After sequentially preparing an activated metal layer, a transition bonding layer, a nano-ceramic layer, and a glaze layer on the substrate surface, sintering is performed to obtain the mixed-crystal black stone glaze layer. The raw materials for the transition bonding layer include silane coupling agent, sodium carboxymethyl cellulose and ceramic whiskers; The raw materials for the nano-ceramic layer include composite binders, ceramic powder, and metal powder; The raw materials for the glaze include fluorine-modified nano-titanium sol, glass powder, metal powder, nano-boron carbide, and cobalt green powder.

2. The preparation method according to claim 1, characterized in that, The raw material for the activated metal layer includes at least one of aluminum, titanium, and silicon; The thickness of the activated metal layer is 20~60μm.

3. The preparation method according to claim 1, characterized in that, The silane coupling agent includes at least one of KH550, KH560 and KH570; The ceramic whiskers include at least one of potassium titanate whiskers, silicon carbide whiskers, and alumina whiskers.

4. The preparation method according to claim 1 or 3, characterized in that, The raw materials of the transition adhesive layer, by mass parts, include 1-3 parts of silane coupling agent, 25-70 parts of sodium carboxymethyl cellulose, and 10-30 parts of ceramic whiskers; The thickness of the transition adhesive layer is 20~50μm.

5. The preparation method according to claim 1, characterized in that, The composite binder includes an aqueous organosilicon-modified inorganic binder; the inorganic binder in the aqueous organosilicon-modified inorganic binder includes at least one of potassium silicate, sodium silicate, and potassium-sodium silicate. The ceramic powder includes at least one of nepheline powder, silicon carbide powder, and transition metal oxide powder; the transition metal oxide powder includes at least one of chromium trioxide, cobalt oxide, manganese oxide, and molybdenum oxide. The metal powder in the nano-ceramic layer includes at least one of chromium powder, nickel powder, and titanium powder.

6. The preparation method according to claim 1 or 5, characterized in that, The raw materials of the nano-ceramic layer, by weight, include 20-50 parts of composite binder, 5-30 parts of ceramic powder, and 5-10 parts of metal powder; The thickness of the nano-ceramic layer is 50~100μm.

7. The preparation method according to claim 1, characterized in that, The glass powder is a low-melting-point glass powder, and the initial softening temperature of the low-melting-point glass powder is 400℃. The metal powder in the glaze includes at least one of aluminum powder and bismuth powder.

8. The preparation method according to claim 1 or 7, characterized in that, The raw materials of the glaze layer, by mass, include 30-50 parts of fluorine-modified nano-titanium sol, 10-30 parts of glass powder, 5-10 parts of metal powder, 3-10 parts of nano-boron carbide and 5-15 parts of cobalt green powder; The thickness of the glaze layer is 50~150μm.

9. The preparation method according to claim 1, characterized in that, The sintering temperature is 350~600℃, and the holding time is 2~4h.

10. The mixed-crystalline black stone glaze coating prepared by the preparation method according to any one of claims 1 to 9, characterized in that, The mixed-crystal black stone glaze coating uses a three-dimensional network structure of titanium dioxide as its framework, which encapsulates glassy substances, metals, and ceramic particles.