A bifunctional electrode, its preparation method and application
By growing Co-Mo-S nanosheet arrays in situ on a nickel foam substrate and forming an oxygen vacancy-sulfur vacancy structure, the problems of active sites and electronic structure in the electrode preparation of cobalt-molybdenum-sulfur electrocatalysts were solved, achieving high efficiency in hydrogen evolution and oxygen evolution reactions, suitable for water electrolysis, seawater electrolysis and carbon dioxide electroreduction reactions.
Patent Information
- Application Number
- CN202611468594.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cobalt-molybdenum-sulfur electrocatalysts suffer from problems such as insufficient exposure of active sites, underoptimized electronic structure, complex preparation process, and poor bifunctional catalytic performance during electrode preparation. In particular, it is difficult to achieve high stability and large-scale production under high temperature and high pressure conditions.
Using nickel foam as a conductive substrate, Co-Mo-S nanosheet arrays were grown through cyclic voltammetric electrochemical activation and in-situ electrodeposition, and an oxygen-sulfur vacancy interface dual-vacancy structure was formed by annealing treatment to prepare a Co-Mo-S/NF self-supporting bifunctional electrode.
It improves the utilization rate of active sites of the catalyst, lowers the energy barrier of hydrogen evolution and oxygen evolution reactions, and achieves high efficiency of hydrogen evolution and oxygen evolution reaction performance in alkaline media. It is also suitable for seawater electrolysis and carbon dioxide electroreduction systems.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrocatalytic materials technology, and relates to a bifunctional electrode, its preparation method, and its application. Background Technology
[0002] Hydrogen energy, as a clean and renewable energy source with high energy density, combustion products consisting only of water, and no secondary pollution, is considered the most promising next-generation green energy. Its development and utilization have become a research hotspot in the global energy sector. Hydrogen production through water electrolysis is widely recognized as the core technological path for the future large-scale production of green hydrogen energy due to its outstanding advantages, including high product purity, mild reaction conditions, the ability to utilize renewable energy sources (such as solar and wind power) to achieve "green electricity to green hydrogen," and zero carbon emissions.
[0003] The water electrolysis process mainly includes the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. OER involves a four-electron transfer process with slow reaction kinetics. Developing efficient catalysts and electrodes can lower the reaction energy barrier and accelerate the reaction rate, becoming key to improving the efficiency of hydrogen production through water electrolysis and promoting its industrial application. Noble metals (such as Pt, Ir, Ru, and their oxides) have long been considered the benchmark catalysts for both HER and OER in water electrolysis due to their excellent catalytic activity. However, the scarcity and high price of precious metal resources lead to high catalyst costs, severely restricting the large-scale application of water electrolysis for hydrogen production. Developing low-cost, highly active, and long-term stable non-precious metal electrocatalysts to replace traditional precious metal catalysts has become a current research focus and core direction in the field of electrocatalysis.
[0004] Among numerous non-noble metal electrocatalysts, transition metal sulfides have attracted widespread attention from researchers due to their unique electronic structure, tunable active sites, good conductivity, and environmental compatibility. Cobalt-molybdenum-based sulfides (Co-Mo-S), with their platinum-like hydrogen adsorption free energy, excellent electron transport performance, and tunable component ratios, have become one of the most promising non-noble metal HER electrocatalysts. In recent years, researchers both domestically and internationally have conducted extensive research on the preparation and performance optimization of Co-Mo-S-based electrocatalysts. Regarding preparation methods, various synthetic routes have been developed, including hydrothermal / solvothermal methods, template methods, vapor deposition methods, and electrodeposition methods. Among these, the hydrothermal method has become a commonly used method for preparing Co-Mo-S nanomaterials due to its relatively simple operation and ease of scalability. For example, Zhou et al. prepared hierarchical Co-Mo-S nanoflower catalysts using a hydrothermal method. By constructing nanoflower structures, they increased the exposure of active sites and improved the HER catalytic activity in neutral media. However, this method requires high temperature and high pressure conditions and uses a water-ethylene glycol mixed solvent system, which still suffers from problems such as harsh process conditions, high energy consumption, and insufficient environmental friendliness, making it difficult to meet the needs of green large-scale preparation. (Journal of Alloys and Compounds, 2020, 844:156108). Tang et al. synthesized interconnected porous CoMoS4 nanosheets through hydrothermal and ion exchange methods, achieving efficient total water splitting at 10 mA cm⁻¹. -2 The overpotentials for OER / HER were 306 mV and 162 mV, respectively, with the porous nanosheet structure significantly increasing the exposure of active sites. However, this process requires high-temperature hydrothermal treatment and secondary sulfidation, resulting in a complex process with high energy consumption. Furthermore, the nanosheets are prone to aggregation, leading to the coverage of some active sites. Simultaneously, this system relies solely on intrinsic sulfur vacancies, failing to achieve synergistic regulation with oxygen vacancies, limiting electronic structure optimization and making precise control of sulfur vacancy concentration and distribution difficult. Therefore, the bifunctional catalytic kinetics still face significant bottlenecks. (Inorganic Chemistry Frontiers, 2020, 7(11): 2120-2127.) Furthermore, the bonding method between the catalyst and the conductive substrate also significantly affects its catalytic performance. Loading Co-Mo-S active materials onto conductive substrates such as nickel foam and carbon cloth can effectively improve electron transport efficiency; however, the binders used in traditional coating methods can cover active sites and increase contact resistance, leading to a decrease in catalytic performance. While in-situ growth methods can improve the bonding force between the catalyst and the substrate, existing in-situ growth strategies (such as hydrothermal methods) often require high temperature and high pressure conditions and are difficult to precisely control morphology and defects, resulting in poor catalyst stability. Therefore, how to grow highly stable catalysts in situ on substrates at room temperature and pressure to prepare high-performance electrodes is an urgent problem to be solved. Summary of the Invention
[0005] To overcome the shortcomings of existing technologies, this invention addresses the technical problems of insufficient exposure of active sites, underoptimized electronic structure, complex preparation processes, and poor bifunctional catalytic performance in existing cobalt-molybdenum-sulfur electrocatalysts. This invention provides a bifunctional electrode, its preparation method, and its applications; specifically, it is a cobalt-molybdenum-sulfur nanosheet bifunctional electrocatalyst with interfacial dual-vacancy synergy and its preparation method. This catalyst exhibits excellent hydrogen evolution and oxygen evolution bifunctional activity and long-term stability. The preparation method is simple, environmentally friendly, and suitable for large-scale production.
[0006] Furthermore, to overcome the shortcomings of existing technologies, this invention addresses the problems of insufficient utilization of active sites, limited control of interface electronic structure, complex preparation processes, and the need to improve the hydrogen evolution and oxygen evolution bifunctional properties of existing cobalt-molybdenum-sulfur materials in electrode preparation. It provides a Co-Mo-S / NF self-supporting bifunctional electrode, its preparation method, and its applications. This electrode uses nickel foam as a conductive substrate layer, on which a Co-Mo-S nanosheet array is grown in situ. An annealing treatment is then used to form an oxygen vacancy-sulfur vacancy interface dual-vacancy structure within the Co-Mo-S nanosheet array.
[0007] The above-mentioned objective of this invention is achieved through the following technical solution: A bifunctional electrode, specifically a Co-Mo-S / NF self-supporting bifunctional electrode, is disclosed. A nickel foam substrate is used as the conductive base layer, on which a Co-Mo-S nanosheet array is grown in situ. The conductive base layer thickness is 300 μm to 1 mm. The Co-Mo-S nanosheets have a thickness of 1 to 50 nm and a length of 0.2 to 5 μm. The Co-Mo-S nanosheet loading is 2 to 15 mg / cm³. 2 .
[0008] In Co-Mo-S nanosheets, the relative atomic percentages of Co, Mo, and S are 5%–50%, 5%–50%, and 40%–90%, respectively, and the sum of the three is 100%.
[0009] Co-Mo-S nanosheets are rich in oxygen and sulfur vacancies, forming a synergistic effect of interfacial dual vacancies. By synergistically regulating the electronic structure of the catalyst surface, the energy barrier for hydrogen evolution and oxygen evolution reactions is lowered.
[0010] The present invention also claims protection for the preparation method of the above-mentioned bifunctional electrode. The electrode preparation process includes conductive substrate pretreatment, cyclic voltammetry electrochemical activation, in-situ electrodeposition growth of Co-Mo-S nanosheet array and annealing treatment, to prepare Co-Mo-S / NF self-supporting bifunctional electrode.
[0011] The preparation method specifically includes the following steps: S1. Conductive substrate pretreatment: The nickel foam is compressed into tablets at 0.5 MPa to 3 MPa for 10 to 40 seconds on a tablet press. Then, it is cleaned or soaked in acetone, anhydrous ethanol and 10% to 30% NaOH solution in sequence. The NaOH solution treatment temperature is 60 to 90 °C and the treatment time is 1 to 3 hours. After ultrasonic cleaning for 10 to 40 minutes, the pretreated nickel foam is obtained and is denoted as T-NF. S2. Cyclic voltammetry electrochemical activation: Using the T-NF obtained in step S1 as the working electrode, it is immersed in dilute hydrochloric acid solution, and electrochemical activation and surface modification are performed by cyclic voltammetry scanning to obtain electrochemically activated nickel foam, denoted as E-NF. S3. In-situ electrodeposition growth of Co-Mo-S nanosheet array: The E-NF obtained in step S2 is immersed in an electrolyte containing cobalt salt, molybdenum salt, sulfur source and complexing agent; Co-Mo-S precursor nanosheet array is deposited in-situ on the surface of E-NF using cyclic voltammetric electrodeposition to obtain E-NF / Co-Mo-S precursor. S4: Annealing treatment: The E-NF / Co-Mo-S precursor obtained in step S3 is placed in an inert or reducing atmosphere and annealed at 250~500 ℃ for 1~12 hours to promote the crystallization of the E-NF / Co-Mo-S precursor and generate interfacial oxygen vacancies and sulfur vacancies in situ, while enhancing the bonding force between the Co-Mo-S nanosheet array and the conductive substrate. The annealing heating rate is 1~10℃·min. -1 After annealing, the material was naturally cooled to room temperature to obtain a Co-Mo-S / NF self-supporting bifunctional electrode.
[0012] Furthermore, in step S2, the concentration of the dilute hydrochloric acid solution is 0.01 ~ 1.0 mol·L⁻¹. -1 The preferred concentration is 0.1~0.5 mol·L⁻¹. -1 The potential range of the cyclic voltammetric scan is -1.0 to 0.5 V compared to the Ag / AgCl electrode, the scan rate is 10 mV / s to 60 mV / s, preferably 30 mV / s to 50 mV / s, and the number of scan cycles is 5 to 40, preferably 10 to 30.
[0013] Further, in step S3, the cobalt salt is any one or more of cobalt chloride, cobalt nitrate, cobalt sulfate, or cobalt acetate; the molybdenum salt is any one or more of sodium molybdate, ammonium molybdate, or phosphomolybdic acid; and the sulfur source is any one or more of thiourea, thioacetamide, or sodium sulfide.
[0014] Furthermore, in step S3, the total concentration of cobalt salt and molybdenum salt is 5–30 mmol·L⁻¹. -1Preferably 10 mmol·L -1 The molar ratio of cobalt salt to molybdenum salt is 1:3 to 3:1, preferably 1:1; the concentration of the sulfur source is 100 to 1000 mmol·L⁻¹. -1 The preferred concentration is 700 mmol·L⁻¹. -1 The molar ratio of the sulfur source to the total amount of cobalt salt and molybdenum salt is 10:1 to 100:1, preferably 70:1. The total concentration of cobalt salt and molybdenum salt and the concentration of sulfur source are their concentrations in the electrolyte.
[0015] Further, in step S3, the complexing agent is any one or more of polyvinylpyrrolidone (PVP), hexadecyltrimethylammonium bromide (CTAB), sodium citrate, and urea. The concentration of the complexing agent in the electrolyte is 1 mmol·L⁻¹. -1 ~ 10 mmol·L -1 The preferred concentration is 1 mmol·L⁻¹. -1 ~ 5 mmol·L -1 .
[0016] Further, in step S3, the electrodeposition parameters in the cyclic voltammetric electrodeposition method are as follows: the Ag / AgCl electrode is the reference electrode, and the scanning potential range is -1.0 to 1.5 V; wherein the high potential is 0.8 V to 1.5 V, preferably 1.0 V to 1.2 V, and the low potential range is -1.0 V to 0.2 V, preferably -0.8 V to 0.1 V; the scanning rate is 2 to 60 mV / s, preferably 10 to 50 mV / s; and the number of scan cycles is 4 to 20, preferably 5 to 16.
[0017] Further, in step S4, the inert atmosphere is nitrogen or argon, and the reducing atmosphere is a mixture of hydrogen and argon or a mixture of hydrogen and nitrogen; the volume fraction of hydrogen is 5-10%; the annealing temperature is 300-450℃, and the annealing time is 3-10 hours.
[0018] This invention also claims protection for the application of the bifunctional electrode prepared by the above-described method in hydrogen evolution reaction and oxygen evolution reaction, used in an alkaline medium for hydrogen evolution reaction and oxygen evolution reaction, as a hydrogen evolution electrode for water electrolysis, an oxygen evolution electrode for water electrolysis, or a hydrogen / oxygen evolution bifunctional electrode. The alkaline medium is 1 M KOH or 0.1 M KOH.
[0019] This invention also seeks protection for the application of the bifunctional electrode prepared by the above method in the electrolysis of seawater hydrogen / oxygen evolution system.
[0020] This invention also seeks protection for the application of the bifunctional electrode prepared by the above preparation method in the anodic oxygen evolution reaction in a carbon dioxide electroreduction system.
[0021] The electrode prepared by this invention does not require additional binders such as current collectors, Nafion, and sugar alcohols, which can improve the utilization rate of catalyst active sites. The three-dimensional porous structure of the conductive substrate layer, nickel foam, and the in-situ grown Co-Mo-S nanosheet array can ensure that the electrolyte fully wets the electrode surface and promote the transport of reactants and products. The advantages of this invention compared to the prior art are: This invention provides a bifunctional electrode using three-dimensional porous nickel foam as a conductive substrate. The Co-Mo-S / NF self-supporting bifunctional electrode is prepared through nickel foam pretreatment, cyclic voltammetric electrochemical activation, in-situ electrodeposition of Co-Mo-S nanosheet arrays, and annealing. The cyclic voltammetric electrochemical activation and in-situ electrodeposition of the Co-Mo-S nanosheet arrays allow for direct in-situ growth of the Co-Mo-S nanosheet arrays on the surface of the conductive nickel foam substrate, which improves the bonding force between the Co-Mo-S nanosheet arrays and the conductive substrate. Furthermore, this method eliminates the need for additional current collectors and binders, resulting in relatively simple preparation steps and a wide availability of raw materials, thus possessing potential for large-scale production. This invention constructs oxygen and sulfur vacancies in situ within a Co-Mo-S nanosheet array through annealing, forming an interfacial dual-vacancy synergistic structure. Mo sites facilitate the hydrogen evolution reaction, while Co sites facilitate the oxygen evolution reaction. Sulfur and oxygen vacancies can jointly regulate the electronic structure of the Co and Mo active sites, promoting charge transfer during water electrolysis and lowering the energy barriers for hydrogen and oxygen evolution reactions.
[0022] The electrode provided by this invention can be used simultaneously for hydrogen evolution reaction and oxygen evolution reaction in alkaline medium. It is suitable for preparing hydrogen evolution electrode, oxygen evolution electrode or hydrogen / oxygen evolution bifunctional electrode for water electrolysis. It can also be used for hydrogen / oxygen evolution bifunctional electrode for seawater electrolysis and anodic oxygen evolution electrode in carbon dioxide electroreduction reaction system. Attached Figure Description
[0023] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0024] Figure 1 Hydrogen evolution tests were performed on the electrodes prepared in Examples 1, 2, 3, and 4 at different elemental ratios, i.e., linear voltammetric curves in 1M KOH solution.
[0025] Figure 2 The oxygen evolution test performed on the electrodes prepared in Examples 1, 2, 3, and 4 is shown as a linear voltammetric curve in 1M KOH solution.
[0026] Figure 3Hydrogen evolution tests were performed on the electrodes prepared in Examples 1, 5, 6, and 7 under different deposition conditions, i.e., linear voltammetric curves in 1M KOH solution. Figure 4 The oxygen evolution test performed on the electrodes prepared in Examples 1, 5, 6 and 7 is shown as a linear voltammetric curve in 1M KOH solution. Figure 5 Hydrogen evolution tests were performed on the electrodes prepared in Examples 1, 8, 9, and 10 under different annealing conditions, i.e., linear voltammetric curves in 1M KOH solution; Figure 6 The oxygen evolution test was performed on the electrodes prepared in Examples 1, 8, 9, and 10, i.e., the linear voltammetric curves in 1M KOH solution; Figure 7 Hydrogen evolution tests were performed on the electrodes prepared in Examples 1, 2, 3, 4, and 5, i.e., linear voltammetric curves in 1M KOH solution. Figure 8 The oxygen evolution test was performed on the electrodes prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, and Comparative Example 5, i.e., the linear voltammetric curves in 1M KOH solution. Detailed Implementation
[0027] The present invention is described in detail below through specific embodiments, but this does not limit the scope of protection of the present invention. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can all be obtained commercially.
[0028] This invention provides a Co-Mo-S / NF self-supporting bifunctional electrode with interfacial dual-vacancy synergy, its preparation method, and its applications. The invention increases the active sites on the nickel foam surface through electrochemical activation, promoting the uniform growth of Co-Mo-S nanosheets and enhancing the bonding between the Co-Mo-S nanosheet array and the conductive substrate layer. After annealing, a synergistic structure of oxygen and sulfur vacancies is formed. A Co-Mo-S nanosheet array containing oxygen and sulfur vacancies is grown in situ on the electrode surface, forming a dual-vacancy synergistic structure at the Co-Mo-S nanosheet array interface. This structure can modulate the electronic structure of the Co and Mo active sites, promoting charge transfer during water electrolysis and improving the activity of the electrode in the hydrogen evolution and oxygen evolution reactions. This electrode requires no additional current collector or binder, which improves the utilization rate of the Co-Mo-S nanosheet array on the electrode surface. The conductive substrate layer has a three-dimensional structure that ensures sufficient wetting of the electrolyte, which is beneficial for the transport of reactants and products. Furthermore, the composition, crystallization state, and surface structure of the Co-Mo-S nanosheet array can be controlled by subsequent heat treatment, thereby improving the charge transport and reactant / product transport performance of the electrode and enhancing the electrocatalytic performance of the resulting electrode.
[0029] The method for fabricating a Co-Mo-S / NF self-supporting bifunctional electrode with interfacial dual vacancy synergy provided by this invention includes: Pretreated nickel foam is obtained by pretreating it, denoted as T-NF. Using T-NF as the working electrode, electrochemical activation and surface modification were performed in an acidic solution using cyclic voltammetry scanning to obtain electrochemically activated nickel foam, denoted as E-NF. E-NF was placed in an electrolyte containing cobalt salt, molybdenum salt, sulfur source and complexing agent, and Co-Mo-S precursor nanosheet array was deposited in situ on the surface of E-NF by cyclic voltammetric electrodeposition. The obtained Co-Mo-S precursor nanosheet array was annealed in an inert or reducing atmosphere to crystallize the precursor and form oxygen and sulfur vacancies in situ, thus obtaining the Co-Mo-S / NF self-supporting bifunctional electrode with interfacial dual vacancy synergy.
[0030] Example 1 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0031] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0032] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0033] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF-CV.
[0034] Example 2 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0035] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0036] 0.010 mol·L -1 Cobalt chloride, 0.005 mol·L-1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0037] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the electrode Co. 10 Mo5S 700 / NF-CV.
[0038] Example 3 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0039] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0040] 0.005 mol·L -1 Cobalt chloride, 0.010 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0041] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo electrode. 10 S 700 / NF-CV.
[0042] Example 4 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0043] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0044] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.35 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0045] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 350 / NF-CV.
[0046] Example 5 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0047] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0048] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.4~0.8V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0049] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF-CV(-0.4~0.8V).
[0050] Example 6 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0051] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0052] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 10 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0053] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF-CV(10mV / s).
[0054] Example 7 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0055] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water.-1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0056] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 15 to obtain the E-NF / Co-Mo-S precursor.
[0057] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF-CV(15cycles).
[0058] Example 8 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0059] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0060] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0061] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 300℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF-CV(300℃).
[0062] Example 9 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0063] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0064] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0065] E-NF / Co-Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 10 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF-CV(10h).
[0066] Example 10 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0067] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0068] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo-S precursor.
[0069] E-NF / Co-Mo-S was placed in hydrogen gas at 5 °C·min. -1 The temperature was increased to 350 °C at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF-CV(H 2) .
[0070] Comparative Example 1 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was subjected to ultrasonic treatment in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60°C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. The resulting pretreated nickel foam, denoted as T-NF, was obtained by drying.
[0071] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the T-NF / Co-Mo-S precursor.
[0072] T-NF / Co-Mo-S was placed in argon gas at 5 °C·min. -1 The temperature was increased to 350 °C at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5Mo5S electrode. 700 / NF.
[0073] Comparative Example 2 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0074] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0075] 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Mo-S precursor.
[0076] E-NF / Mo-S was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the electrode Mo5S. 700 / NF-CV.
[0077] Comparative Example 3 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0078] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0079] 0.005 mol·L -1 Cobalt chloride, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-S precursor.
[0080] E-NF / Co-S was placed in argon gas (flow rate 80 mL / min) and heated at 5 °C·min. -1The temperature was increased to 350℃ at a certain rate, held at that temperature for 8 hours, and then allowed to cool naturally to room temperature after annealing to obtain the Co5S electrode. 700 / NF-CV.
[0081] Comparative Example 4 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0082] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0083] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate with 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed and added to deionized water, and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12 to obtain the E-NF / Co-Mo precursor.
[0084] E-NF / Co-Mo was placed under argon gas (flow rate 80 mL / min) at 5 °C·min. -1 The temperature was increased to 350℃ at a certain rate, held for 8 hours, and then naturally cooled to room temperature after annealing to obtain the Co5Mo5 / NF-CV electrode.
[0085] Comparative Example 5 Nickel foam was compressed into tablets at 1.5 MPa for 20 seconds using a tablet press. Subsequently, it was ultrasonically treated in acetone and ethanol solutions for 20 minutes each. The nickel foam was then cleaned in a 15% NaOH alkaline solution at 60 °C for 1 hour. After treatment, it was rinsed with deionized water and ultrasonically cleaned for 10–40 minutes. After drying, the pretreated nickel foam, denoted as T-NF, was obtained.
[0086] Using T-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, the solution was immersed in 0.1 mol·L⁻¹ water. -1 Cyclic voltammetry was performed in a dilute hydrochloric acid solution with a scanning potential range of -1.0 to 0.5 V, a scanning rate of 50 mV / s, and 10 scan cycles. After the scan, the sample was rinsed with deionized water and dried to obtain electrochemically activated nickel foam, denoted as E-NF.
[0087] 0.005 mol·L -1 Cobalt chloride, 0.005 mol·L -1 Ammonium molybdate, 0.70 mol·L -1 Thiourea and 1 mmol·L -1 Stabilizer polyvinylpyrrolidone (PVP) was mixed with deionized water and magnetically stirred until completely dissolved to obtain a clear electrolyte. A standard three-electrode system was used, with E-NF as the working electrode, a platinum sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode. The working electrode was immersed in the electrolyte, and the scanning potential range was -0.8 to 1.2 V, the scanning rate was 50 mV / s, and the number of scans was 12. The electrode Co5Mo5S was obtained after cleaning and drying without annealing. 700 / NF-CV(25℃).
[0088] Application examples Electrolysis performance tests for hydrogen and oxygen evolution in water: Electrodes prepared in Examples 1-10 and Comparative Examples 1-5 were used for electrochemical performance testing. The electrolyte was 1 M KOH solution, and the effective area of the working electrode was 1 cm². 2 The counter electrode was a 1 cm × 1 cm platinum sheet electrode, and the reference electrode was a Hg / HgO electrode. Polarization curves for the hydrogen evolution reaction and oxygen evolution reaction were obtained using linear voltammetry at a scan rate of 10 mV·s. -1 No iR compensation is performed. All potentials in the attached figures are converted to potentials relative to the reversible hydrogen electrode (RHE).
[0089] Figure 1 and Figure 2 Corresponding to Examples 1, 2, 3, and 4. The absolute value of the current density is 10 mA·cm. -2As a comparison point, based on the curves in the attached figures, the hydrogen evolution overpotentials of Examples 1-4 were approximately 130 mV, 180 mV, 245 mV, and 215 mV, respectively, and the oxygen evolution overpotentials were approximately 120 mV, 195 mV, 210 mV, and 250 mV, respectively. The results show that different ratios of Co, Mo, and S raw materials significantly affect the hydrogen evolution and oxygen evolution performance of the obtained Co-Mo-S nanosheet arrays. Example 1 exhibited better overall bifunctional electrocatalytic performance, demonstrating optimal HER and OER catalytic activity, with significantly lower overpotentials than other ratios, proving that this ratio achieves the best synergistic effect in bifunctional catalytic performance.
[0090] Figure 3 and Figure 4 Corresponding to Examples 1, 5, 6, and 7. The absolute value of the current density is 10 mA·cm. -2 As a comparison point, based on curve estimation, the hydrogen evolution overpotentials of Examples 1, 5, 6, and 7 were approximately 130 mV, 185 mV, 220 mV, and 170 mV, respectively; the oxygen evolution overpotentials were approximately 120 mV, 250 mV, 160 mV, and 260 mV, respectively. This shows that changing the scanning potential range, scanning rate, and number of scan cycles in cyclic voltammetric electrodeposition leads to changes in the hydrogen and oxygen evolution performance of the electrode, indicating that electrodeposition conditions have a significant impact on the formation of Co-Mo-S nanosheet arrays and their bifunctional electrocatalytic performance. The electrodeposition parameters used in Example 1 achieve uniform loading and sufficient exposure of the active material, and the catalytic performance is significantly better than other parameter conditions, indicating that these electrodeposition conditions can effectively construct a complete and efficient catalytic interface.
[0091] Figure 5 and Figure 6 Corresponding to Examples 1, 8, 9, and 10. The absolute value of the current density is 10 mA·cm. -2As a comparison point, based on curve estimation, the hydrogen evolution overpotentials of Examples 1, 8, 9, and 10 are approximately 130 mV, 180 mV, 160 mV, and 260 mV, respectively; the oxygen evolution overpotentials are approximately 120 mV, 290 mV, 290 mV, and 100 mV, respectively. Considering the preparation conditions of Example 8 (annealing at 300 °C), Example 9 (annealing at 350 °C for 10 h), and Example 10 (annealing in a hydrogen atmosphere), it can be seen that annealing temperature, annealing time, and annealing atmosphere all affect the hydrogen evolution and oxygen evolution performance of the electrode. Example 10 exhibits a lower oxygen evolution overpotential, but its hydrogen evolution performance is weaker than that of Example 1. Therefore, considering the overall bifunctional performance of HER / OER, Example 1 exhibits a more balanced electrocatalytic performance. The annealing process of Example 1 achieves optimal precursor crystallization and dual-vacancy synergistic effect, significantly reducing the reaction energy barrier, and its catalytic performance is superior to other annealing conditions, proving that this annealing process can effectively improve intrinsic catalytic activity.
[0092] Figure 7 and Figure 8 This is a direct performance comparison between Example 1 and Comparative Examples 1-5. The absolute value of the current density is 10 mA·cm⁻¹. -2 As a comparison point, based on curve estimation, the hydrogen evolution overpotentials of Example 1 and Comparative Examples 1, 2, 3, 4, and 5 were approximately 130 mV, 225 mV, 235 mV, 230 mV, 225 mV, and 170 mV, respectively; and the oxygen evolution overpotentials were approximately 120 mV, 145 mV, 150 mV, 315 mV, 295 mV, and 220 mV, respectively. Compared to Comparative Examples 1-5, the hydrogen evolution overpotential of Example 1 decreased by approximately 95 mV, 105 mV, 100 mV, 95 mV, and 40 mV, respectively, and the oxygen evolution overpotential decreased by approximately 30 mV, 35 mV, 200 mV, 180 mV, and 105 mV, respectively. Comparative Example 1, which did not undergo cyclic voltammetric electrochemical activation, showed weaker hydrogen evolution and oxygen evolution performance than Example 1, indicating that electrochemical activation of nickel foam is beneficial for improving the bifunctional electrocatalytic performance of the electrode. Comparative Example 2, which did not contain Co, and Comparative Example 3, which did not contain Mo, both showed varying degrees of performance degradation, indicating that Co and Mo have different promoting effects on hydrogen evolution and oxygen evolution reactions. Comparative Example 4, which did not add a sulfur source, showed significantly reduced HER and OER performance. Comparative Example 5, which did not undergo annealing treatment, also showed lower hydrogen evolution and oxygen evolution performance than Example 1. These results collectively demonstrate that cyclic voltammetric electrochemical activation, the construction of the Co-Mo-S nanosheet array, and subsequent annealing treatment play crucial roles in obtaining better bifunctional electrocatalytic performance.
[0093] The embodiments described above are merely preferred embodiments of the present invention, and not all feasible embodiments of the present invention. Any obvious modifications made by those skilled in the art without departing from the principles and spirit of the present invention should be considered to be included within the scope of protection of the claims of the present invention.
Claims
1. A bifunctional electrode, characterized in that, Specifically, it is a Co-Mo-S / NF self-supporting bifunctional electrode; using nickel foam as the conductive substrate, an array of Co-Mo-S nanosheets is grown in situ on the surface of the nickel foam, with a conductive substrate thickness of 300 μm to 1 mm; the Co-Mo-S nanosheets have a thickness of 1 to 50 nm and a length of 0.2 to 5 μm; the loading of Co-Mo-S nanosheets is 2 to 15 mg / cm³. 2 .
2. The dual-functional electrode as described in claim 1, characterized in that, In Co-Mo-S nanosheets, the relative atomic percentages of Co, Mo, and S are 5%–50%, 5%–50%, and 40%–90%, respectively.
3. A method for preparing a bifunctional electrode as described in any one of claims 1-2, characterized in that, The electrode fabrication process includes conductive substrate pretreatment, cyclic voltammetry electrochemical activation, in-situ electrodeposition growth of Co-Mo-S nanosheet array, and annealing treatment, to prepare a Co-Mo-S / NF self-supporting bifunctional electrode.
4. The method for preparing a bifunctional electrode as described in claim 3, characterized in that, Specifically, the following steps are included: S1. Conductive substrate pretreatment: The nickel foam is compressed into tablets at 0.5 MPa to 3 MPa for 10 to 40 seconds on a tablet press. Then, it is cleaned or soaked in acetone, anhydrous ethanol and 10% to 30% NaOH solution in sequence. The NaOH solution treatment temperature is 60 to 90 °C and the treatment time is 1 to 3 hours. After ultrasonic cleaning for 10 to 40 minutes, the pretreated nickel foam is obtained and is denoted as T-NF. S2. Cyclic voltammetry electrochemical activation: Using the T-NF obtained in step S1 as the working electrode, it is immersed in dilute hydrochloric acid solution, and electrochemical activation and surface modification are performed by cyclic voltammetry scanning to obtain electrochemically activated nickel foam, denoted as E-NF. S3. In-situ electrodeposition growth of Co-Mo-S nanosheet array: The E-NF obtained in step S2 is immersed in an electrolyte containing cobalt salt, molybdenum salt, sulfur source and complexing agent; Co-Mo-S precursor nanosheet array is deposited in-situ on the surface of E-NF using cyclic voltammetric electrodeposition to obtain E-NF / Co-Mo-S precursor. S4: Annealing treatment: The E-NF / Co-Mo-S precursor obtained in step S3 is placed in an inert or reducing atmosphere and annealed at 250~500 ℃ for 1~12 hours to promote the crystallization of the E-NF / Co-Mo-S precursor and generate interfacial oxygen vacancies and sulfur vacancies in situ, while enhancing the bonding force between the Co-Mo-S nanosheet array and the conductive substrate. The annealing heating rate is 1~10℃·min. -1 After annealing, the material was naturally cooled to room temperature to obtain a Co-Mo-S / NF self-supporting bifunctional electrode.
5. The method for preparing a bifunctional electrode as described in claim 4, characterized in that, In step S2, the concentration of the dilute hydrochloric acid solution is 0.01 ~ 1.0 mol·L⁻¹. -1 The potential range of the cyclic voltammetric scan is -1.0 to 0.5 V compared to the Ag / AgCl electrode, the scan rate is 10 mV / s to 50 mV / s, and the number of scan cycles is 10 to 30.
6. The method for preparing a bifunctional electrode as described in claim 4, characterized in that, In step S3, the cobalt salt is any one or more of cobalt chloride, cobalt nitrate, cobalt sulfate, or cobalt acetate; the molybdenum salt is any one or more of sodium molybdate, ammonium molybdate, or phosphomolybdic acid; the sulfur source is any one or more of thiourea, thioacetamide, or sodium sulfide; and the total concentration of the cobalt and molybdenum salts is 5–30 mmol·L⁻¹. -1 The concentration of the sulfur source is 100–1000 mmol·L⁻¹ -1 .
7. The method for preparing a bifunctional electrode as described in claim 4, characterized in that, In step S3, the complexing agent is any one or more of polyvinylpyrrolidone, hexadecyltrimethylammonium bromide, sodium citrate, and urea; the concentration of the complexing agent in the electrolyte is 1 mmol·L⁻¹. -1 ~ 10 mmol·L -1 .
8. The method for preparing a bifunctional electrode as described in claim 4, characterized in that, In step S3, the electrodeposition parameters in the cyclic voltammetric electrodeposition method are: Ag / AgCl electrode as reference electrode, and scanning potential range of -1.0 to 1.5 V; The high potential ranges from 0.8 V to 1.5 V, the low potential ranges from -1.0 V to 0.2 V, the scan rate ranges from 2 to 60 mV / s, and the number of scans ranges from 4 to 20.
9. The application of the bifunctional electrode prepared by the method of any one of claims 4-8 in the hydrogen evolution reaction and oxygen evolution reaction, characterized in that, It is used in alkaline media for hydrogen evolution and oxygen evolution reactions, serving as a hydrogen evolution electrode, an oxygen evolution electrode, or a hydrogen / oxygen evolution bifunctional electrode in water electrolysis.
10. The application of the bifunctional electrode prepared by the method of any one of claims 4-8 in the anodic oxygen evolution reaction in a carbon dioxide electroreduction system.