A method for preparing heterogeneous interface membranes to improve the performance of alkaline electrolyzers

By constructing a ruthenium dioxide and zirconium dioxide heterostructure on the anode side of the membrane in an alkaline electrolyzer, the problem of balancing electrolysis efficiency and safety under high current density was solved, thus improving the stability and safety of the catalyst layer.

CN123108642APending Publication Date: 2026-11-17HUANENG CLEAN ENERGY RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611190503.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Under high current density operating conditions in alkaline water electrolyzers, it is difficult to balance electrolysis efficiency and operational safety. Traditional catalyst preparation processes damage the physical pore structure of the membrane, resulting in weak interfacial bonding strength and easy agglomeration and detachment, which affects the long-term stability and safety of the electrolyzer.

Method used

A room-temperature in-situ conversion deposition process was used to construct a heterostructure of ruthenium dioxide and zirconium dioxide on the anode side of a porous composite membrane. Ruthenium dioxide nanoparticles were formed by selective infiltration of ruthenium precursor solution and generation of ruthenium hydroxide colloidal precipitate at room temperature, thus avoiding the collapse of the pore structure caused by high-temperature treatment. Zirconium dioxide was used as a carrier to enhance the interfacial bonding strength.

Benefits of technology

Maintaining the integrity of the membrane pore structure enhances the structural stability and interfacial bonding strength of the catalyst layer, reduces the hydrogen concentration on the anode side, and achieves simultaneous improvement in the safety and electrolysis efficiency of the electrolyzer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108642A_ABST
    Figure CN123108642A_ABST
Patent Text Reader

Abstract

This application relates to the field of alkaline water electrolysis technology and discloses a method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer. The method includes: selectively applying a ruthenium precursor solution to the surface layer of a porous composite membrane containing zirconium dioxide inorganic filler on the anode-facing side during assembly, causing ruthenium ions to be adsorbed into the pores and between the zirconium dioxide inorganic filler; placing the porous composite membrane with adsorbed ruthenium ions in an alkaline solution for a room-temperature precipitation reaction to generate ruthenium hydroxide colloidal precipitate in situ; washing and then subjecting it to natural oxidation in air to convert it into ruthenium dioxide nanoparticles, with the ruthenium dioxide growing on a zirconium dioxide carrier to form a heterogeneous interface. This application employs room-temperature in-situ deposition, avoiding high-temperature damage to the porous composite membrane structure; the heterogeneous interface improves the bonding strength of the catalyst layer, preventing catalyst detachment; the dispersed catalyst layer effectively recombines hydrogen without increasing ohmic impedance, achieving a synergistic improvement in electrolyzer safety and efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of alkaline water electrolysis technology, specifically to a method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer. Background Technology

[0002] Alkaline water electrolysis has become the main technical route for industrial green hydrogen production due to its mature technology, low equipment cost, and stable operation. It is gradually developing towards higher current density, lower energy consumption, and longer lifespan. Under high current density operating conditions, a large amount of hydrogen can easily diffuse through the diaphragm to the anode side. When the hydrogen concentration at the anode outlet exceeds the lower explosive limit, it will affect the safe operation of the electrolyzer. At present, improving the hydrogen production efficiency of the electrolyzer usually involves methods such as thinning the diaphragm or increasing the diaphragm porosity. However, this will increase the rate at which hydrogen permeates through the diaphragm, resulting in an increase in the hydrogen concentration on the anode side. There is a contradiction between electrolysis efficiency and operational safety that is difficult to balance. If a catalyst is conventionally loaded on the diaphragm surface for gas recombination, the continuous coverage of the catalyst will often block the original micropores of the diaphragm, leading to an increase in the ohmic resistance of the electrolyzer.

[0003] Conventional metal oxide catalyst preparation processes typically require high-temperature calcination. The composite membranes used in alkaline electrolyzers usually contain a polymer skeleton. High-temperature heat treatment can cause thermal shrinkage of the polymer within the membrane and collapse of the physical pore structure. This directly leads to a decrease in the hydrophilicity of the membrane and damages its original ion conduction properties.

[0004] Catalysts loaded onto the membrane surface using traditional physical coating or adhesion methods have weak interfacial bonding strength with the membrane substrate material. During long-term operation of alkaline electrolyzers, under the conditions of a strongly alkaline electrolyte environment and continuous gas-liquid scouring, the catalyst on the membrane surface is prone to agglomeration, detachment, and deactivation. Insufficient stability of the catalyst layer structure leads to a rapid decline in gas recombination efficiency, making it difficult to maintain the long-term stable and safe operation of the electrolyzer. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this application provides a method for preparing a heterogeneous interface membrane to improve the performance of alkaline electrolyzers. This method solves the problem of balancing electrolysis efficiency and operational safety in alkaline electrolyzers under high current density operating conditions. It also solves the problems of traditional high-temperature catalyst preparation processes damaging the physical pore structure of the membrane, and the weak interfacial bonding strength and easy agglomeration and detachment of conventional physically coated catalyst layers under strong alkaline and gas-liquid scouring environments.

[0006] To achieve the above objectives, this application provides the following technical solution: The first aspect of this application provides a method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer, comprising the following steps: selectively applying a ruthenium precursor solution to the surface layer of a porous composite membrane containing zirconium dioxide inorganic filler on the anode-facing side during assembly, so that ruthenium ions in the ruthenium precursor solution are adsorbed into the pores inside the porous composite membrane containing zirconium dioxide inorganic filler and between the zirconium dioxide inorganic filler; placing the porous composite membrane containing zirconium dioxide inorganic filler with adsorbed ruthenium ions in an alkaline solution for a room temperature precipitation reaction, so that the ruthenium ions react with hydroxide ions in the alkaline solution. Ruthenium hydroxide colloidal precipitate was generated in situ on the surface of a porous composite membrane containing zirconium dioxide inorganic filler. The porous composite membrane containing zirconium dioxide inorganic filler with ruthenium hydroxide colloidal precipitate was treated with deionized water to remove impurities. The porous composite membrane containing zirconium dioxide inorganic filler after impurity removal and washing was placed in air for dehydration and natural oxidation treatment, so that the ruthenium hydroxide colloidal precipitate was transformed into ruthenium dioxide nanoparticles. The ruthenium dioxide nanoparticles grew on the zirconium dioxide inorganic filler as a carrier to form a heterogeneous interface structure of ruthenium dioxide and zirconium dioxide.

[0007] In one optional embodiment, the preparation process of the ruthenium precursor solution is as follows: dissolving a water-soluble ruthenium salt in deionized water or a dilute acid solution to prepare a ruthenium precursor solution with a concentration of 0.01 to 0.10 mol / L; the water-soluble ruthenium salt is hydrated ruthenium trichloride, and the dilute acid solution is dilute hydrochloric acid solution.

[0008] In one optional embodiment, the ruthenium precursor solution is selectively applied to the surface layer facing the anode during the assembly of a porous composite membrane containing zirconium dioxide inorganic filler by either drop coating or single-sided immersion. The processing time for either drop coating or single-sided immersion is controlled to be 1 to 10 minutes, so that the penetration depth of ruthenium ions into the porous composite membrane containing zirconium dioxide inorganic filler is defined as between 5 and 15 μm.

[0009] In one alternative embodiment, the alkaline solution is a sodium hydroxide solution with a concentration between 0.1 and 1.0 mol / L; the temperature conditions for the room temperature precipitation reaction are controlled between 25 and 50°C.

[0010] In one optional embodiment, the porous composite membrane containing zirconium dioxide inorganic filler is repeatedly rinsed with deionized water, and the washing endpoint is controlled to ensure that no free chloride ions are detected in the eluent.

[0011] In one optional embodiment, the dehydration and natural oxidation process is as follows: the porous composite membrane containing zirconium dioxide inorganic filler, after impurity removal and washing, is placed in air to air dry naturally, causing the ruthenium hydroxide colloid to precipitate, dehydrate, and react with oxygen in the air, transforming into ruthenium dioxide hydrate and amorphous ruthenium dioxide nanoparticles. Further, after air drying, the porous composite membrane containing zirconium dioxide inorganic filler is transferred to an oven set at 60°C for heat drying.

[0012] In one optional embodiment, by adjusting the concentration of the ruthenium precursor solution and the selectively applied treatment time, the areal loading of ruthenium dioxide nanoparticles generated on the surface of the porous composite membrane containing zirconium dioxide inorganic filler is controlled within the range of 0.02 to 0.20 mg / cm², so that the ruthenium dioxide nanoparticles are distributed in a discontinuous dispersion state on the surface of the porous composite membrane containing zirconium dioxide inorganic filler.

[0013] The second aspect of this application provides a method for assembling an alkaline electrolytic cell, comprising the following steps: preparing a heterogeneous interface membrane using the aforementioned method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolytic cell; placing the heterogeneous interface membrane between the cathode and the anode; and assembling the cathode, the anode, and the heterogeneous interface membrane to form an alkaline electrolytic cell.

[0014] In one optional embodiment, the cathode is a NiMo cathode and the anode is a nickel mesh anode; the step of disposing a heterogeneous interface membrane between the cathode and the anode and assembling the cathode, the anode and the heterogeneous interface membrane to form an alkaline electrolytic cell specifically involves: disposing a heterogeneous interface membrane between the NiMo cathode and the nickel mesh anode, and assembling the NiMo cathode, the nickel mesh anode and the heterogeneous interface membrane to form a zero-gap alkaline electrolytic cell.

[0015] This application provides a method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer. It has the following beneficial effects: 1. This application adopts a room temperature in-situ conversion deposition process to complete the construction of the recombinant catalyst layer without high temperature calcination. This avoids the thermal shrinkage of the polymer inside the membrane and the collapse of the pore structure caused by high temperature treatment. This process maintains the original pore size, porosity and hydrophilicity of the porous composite membrane, ensuring that the ion conduction performance of the membrane does not decrease.

[0016] 2. This application utilizes the zirconium dioxide inorganic filler inside the porous composite membrane as a growth carrier, so that the generated ruthenium dioxide nanoparticles form a ruthenium dioxide and zirconium dioxide heterostructure. This heterostructure enhances the interfacial bonding strength between the catalyst layer and the membrane, inhibits the agglomeration and shedding of the catalyst under strong alkaline environment and gas-liquid scouring conditions, and improves the structural stability of the catalyst layer during long-term operation.

[0017] 3. This application achieves a non-discontinuous dispersion of the recombinant catalyst layer on the membrane surface by selectively impregnating the anode side and controlling the surface loading of the catalyst. The catalyst distributed on the anode side surface can promptly catalyze the hydrogen permeating the membrane to undergo a recombinant reaction, reducing the hydrogen concentration on the anode side to a safe range. At the same time, it avoids the blockage of membrane channels and the increase of ohmic impedance caused by continuous coverage, thus achieving a simultaneous improvement in the safety of electrolyzer operation and electrolysis efficiency. Attached Figure Description

[0018] Figure 1 This is a flowchart of the method in this application; Figure 2 Here is a scanning electron microscope image of the microstructure of ruthenium dioxide nanoparticles in this application; Figure 3 This is a graph showing the 150-hour long-term stability data of the electrolyzer in this application; Figure 4 This is a graph showing the hydrogen content in the anolyte at different times according to this application. Detailed Implementation

[0019] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0020] Please see Figure 1 This application provides a method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer. The method uses a porous composite membrane containing zirconium dioxide (ZrO2) inorganic filler as a carrier and employs a room-temperature in-situ conversion deposition process to construct a recombinant catalyst layer on the anode side of the porous composite membrane. The specific substructure of the porous composite membrane mentioned above includes currently commercially available Zirfon composite membrane materials. The overall workflow of this preparation method includes the following steps: S100, selective impregnation of Ru precursor, this step is intended to make Ru 3+ Ions selectively penetrate the anode side surface of the porous composite membrane and preferentially adsorb between the zirconium dioxide inorganic filler particles, providing reaction sites for the subsequent in-situ formation of the catalyst layer.

[0021] S110, prepare Ru precursor solution, specifically by dissolving hydrated ruthenium trichloride (RuCl3·xH2O) in deionized water or dilute hydrochloric acid to prepare Ru precursor solution with a concentration of 0.01-0.10 mol / L.

[0022] S120, porous composite membrane anode side surface permeation control, specifically using drop coating or single-sided impregnation methods, treating only the anode side of the Zirfon composite membrane, controlling the impregnation time to 1~10 min, so that Ru 3+ Ions selectively penetrate into the anode-side surface of the Zirfon composite membrane at a depth of approximately 5–15 μm and preferentially adsorb between the zirconium dioxide (ZrO2) particles inside the Zirfon composite membrane, providing reaction sites for the subsequent in-situ formation of the catalyst layer.

[0023] S200, room temperature in-situ precipitation. This step aims to allow Ru adsorbed inside the membrane to precipitate without damaging the original polymer framework and physical pore structure of the porous composite membrane. 3+ Ions undergo in-situ precipitation reaction.

[0024] S210, in-situ formation of colloidal precipitate, specifically involves placing the impregnated Zirfon composite membrane in a 0.1–1.0 mol / L sodium hydroxide (NaOH) solution and reacting it at room temperature (25–50°C) to allow Ru to... 3+ Ions and hydroxide ions (OH-) - The reaction occurs, and ruthenium hydroxide (Ru(OH)3) colloidal precipitate is formed in situ.

[0025] S220, impurity removal washing, specifically involves thoroughly washing the Zirfon composite membrane with deionized water to remove residual chloride ions (Cl). - ) and sodium ions (Na) + This is to avoid residual chloride ions causing localized corrosion to the anode electrode.

[0026] S300, room temperature in-situ oxidation to form RuO2 recombination layer. This step aims to transform colloidal precipitate into recombination catalytic layer with gas recombination activity through natural dehydration oxidation process, and simultaneously construct a stable heterogeneous interface structure.

[0027] S310, air drying and natural oxidation, specifically involves placing the washed Zirfon composite membrane in the air to air dry naturally, allowing ruthenium hydroxide (Ru(OH)3) to gradually dehydrate and oxidize in the air to form ruthenium dioxide hydrate (RuO2·xH2O) or amorphous ruthenium dioxide (RuO2) nanoparticles. The entire preparation process does not require high-temperature calcination, which can effectively avoid polymer shrinkage, pore structure collapse and decrease in hydrophilicity in the Zirfon composite membrane caused by heat treatment, thereby maintaining the original pore size, porosity and ion transport performance of the Zirfon composite membrane.

[0028] S320, an in-situ constructed ruthenium dioxide and zirconium dioxide heterostructure, specifically, ruthenium dioxide nanoparticles grow directly between zirconium dioxide particles, forming a stable ruthenium dioxide and zirconium dioxide heterostructure. Utilizing the good interfacial compatibility and high bonding strength of the two metal oxides, the ruthenium dioxide particles can be firmly anchored to the zirconium dioxide support surface, significantly improving the catalyst layer's resistance to erosion, agglomeration, and shedding.

[0029] S400, Catalyst loading regulation: This step aims to control the dispersion state of the catalyst by adjusting process variables, thereby achieving synergistic optimization of electrochemical reaction and mass transport.

[0030] S410, parameter coordinated control, specifically controls the ruthenium dioxide loading by adjusting the precursor concentration, impregnation times, and impregnation time, with the preferred ruthenium dioxide surface loading being 0.02–0.20 mg·cm³. -2 .

[0031] S420 achieves a balance between catalytic and transport performance by controlling the ruthenium dioxide particles to be sparsely and uniformly distributed. This ensures high gas recombination catalytic activity while avoiding an increase in ohmic resistance caused by continuous coverage of the Zirfon composite membrane channels, thus achieving a balance between catalytic and transport performance.

[0032] To verify the actual technical effect of the aforementioned preparation method, Example 1 is given below for specific illustrative purposes.

[0033] Example 1 provides a method for preparing a high-performance heterogeneous interface membrane for an alkaline electrolyzer. The specific preparation process is as follows: Ruthenium trichloride hydrate is weighed and dissolved in a 0.05 mol / L dilute hydrochloric acid solution to prepare a 0.05 mol / L Ru precursor solution. The solution is then magnetically stirred for 30 minutes to dissolve the hydrated ruthenium trichloride, resulting in a uniform and transparent precursor solution. A commercial Zirfon composite membrane is selected as the porous composite membrane substrate material. A drop-coating process is used, treating only the anode side surface of the Zirfon composite membrane. The standard dosage is 40 μL of precursor solution per square centimeter, and the impregnation time is controlled to be 5 minutes to allow the Ru in the precursor solution to dissolve. 3+ Ions fully penetrate the anode-side surface of the Zirfon composite membrane, with the penetration depth controlled to approximately 10 μm. 3+ Ions preferentially adsorb onto the zirconium dioxide particles and interparticle pores within the Zirfon composite membrane. After impregnation, the membrane is allowed to stand under natural conditions for approximately 2 minutes to allow the precursor solution to fully distribute on the anode side surface. The impregnated Zirfon composite membrane is then immersed in a 1 mol / L sodium hydroxide solution and reacted at room temperature for 20 minutes. 3+The ruthenium hydroxide reacts with hydroxide ions in the solution, forming a colloidal precipitate of ruthenium hydroxide in situ on the anode side of the Zirfon composite membrane. Since the precipitation process occurs within the pores of the Zirfon composite membrane and between the zirconium dioxide particles, the ruthenium precursor is uniformly fixed on the anode side of the Zirfon composite membrane. Subsequently, the Zirfon composite membrane after the precipitation reaction is repeatedly rinsed with a large amount of deionized water until no free chloride ions are detected in the eluent, avoiding corrosion of the electrolytic cell by residual chloride ions during long-term operation. The cleaned Zirfon composite membrane is then allowed to air dry naturally for 24 hours, followed by drying in a 60°C oven for 2 hours. During the dehydration and drying process, the ruthenium hydroxide gradually dehydrates and reacts with oxygen in the air, ultimately forming ruthenium dioxide hydrate and some amorphous ruthenium dioxide nanoparticles. Example 1 uses a single impregnation process, resulting in a final ruthenium dioxide surface loading of approximately 0.08 mg·cm³. -2 The ruthenium dioxide particles are sparsely and uniformly dispersed, which ensures good catalytic activity without affecting the ion transport performance of the Zirfon composite membrane channels.

[0034] See attached document Figure 2 , Figure 2 The image shows a scanning electron microscope (SEM) image of the microstructure of ruthenium dioxide nanoparticles according to an embodiment of this application. Combined with the results of the SEM test, the ruthenium dioxide nanoparticles are uniformly distributed on the anode side surface of the Zirfon composite membrane and between the zirconium dioxide particles. No continuous dense covering layer is formed. The pore structure of the Zirfon composite membrane remains intact, and the pore size and porosity are basically the same as those of the original Zirfon composite membrane. This indicates that the room temperature in-situ conversion process effectively avoids the pore structure collapse and polymer shrinkage caused by traditional high temperature treatment.

[0035] See attached document Figure 3 , Figure 3 Based on the 150-hour long-term stability data of an electrolyzer according to an embodiment of this application, a zero-gap alkaline water electrolyzer was assembled by combining a Zirfon composite diaphragm loaded with ruthenium dioxide with a NiMo cathode and a nickel mesh anode. The electrolyzer was operated at 30 wt.% KOH, 80°C, and 0.5 A·cm⁻¹. -2 Under operating conditions, through long-term operation tests, the electrolytic cell voltage remained stable at around 1.65V for 150 hours.

[0036] See attached document Figure 4 , Figure 4Based on an embodiment of this application, the hydrogen content curves in the anolyte at different times are used to test the gas components using gas chromatography. The anolyte gas collected at different time periods is detected. The ruthenium dioxide catalyst layer can perform real-time recombination catalysis on the trace amounts of hydrogen passing through the Zirfon composite membrane, so that the hydrogen concentration on the anolyte side is kept below 0.5% for a long time. Due to the excellent structural stability of the ruthenium dioxide heterostructure, the catalyst layer maintains high catalytic activity under long-term alkaline environment and gas-liquid scouring conditions, thereby achieving a simultaneous improvement in the safety and durability of the electrolyzer.

[0037] Although embodiments of this application have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer, comprising the following steps: S100, a ruthenium precursor solution is selectively applied to the surface layer of the porous composite membrane containing zirconium dioxide inorganic filler on the side facing the anode during assembly, so that ruthenium ions in the ruthenium precursor solution are adsorbed into the pores inside the porous composite membrane containing zirconium dioxide inorganic filler and between the zirconium dioxide inorganic filler. S200 involves placing a porous composite membrane containing zirconium dioxide inorganic filler, which has been treated by S100, into an alkaline solution for a room temperature precipitation reaction. This allows ruthenium ions to react with hydroxide ions in the alkaline solution, resulting in the in-situ generation of ruthenium hydroxide colloidal precipitate on the surface of the porous composite membrane containing zirconium dioxide inorganic filler. S300 uses deionized water to remove impurities from the porous composite membrane containing zirconium dioxide inorganic filler after S200 treatment. S400 involves placing a porous composite membrane containing zirconium dioxide inorganic filler, which has been washed by S300, into air for dehydration and natural oxidation. This process transforms ruthenium hydroxide colloidal precipitate into ruthenium dioxide nanoparticles, which then grow using zirconium dioxide inorganic filler as a carrier, forming a heterogeneous interface structure between ruthenium dioxide and zirconium dioxide.

2. According to claim 1, the method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer, in S100, the preparation process of the ruthenium precursor solution is as follows: dissolving a water-soluble ruthenium salt in deionized water or a dilute acid solution to prepare a ruthenium precursor solution with a concentration of 0.01 to 0.10 mol / L; the water-soluble ruthenium salt is hydrated ruthenium trichloride, and the dilute acid solution is dilute hydrochloric acid solution.

3. According to claim 1, the method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer, in step S100, the ruthenium precursor solution is selectively applied to the surface layer of the porous composite membrane containing zirconium dioxide inorganic filler on the side facing the anode during assembly by either drop coating or single-sided impregnation; the processing time for drop coating or single-sided impregnation is controlled to be 1 to 10 min, so that the penetration depth of ruthenium ions into the porous composite membrane containing zirconium dioxide inorganic filler is defined as between 5 and 15 μm.

4. The method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer according to claim 1, wherein in S200, the alkaline solution is a sodium hydroxide solution with a concentration between 0.1 and 1.0 mol / L; and the temperature conditions for the room temperature precipitation reaction are controlled between 25 and 50°C.

5. According to claim 1, a method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer is provided, wherein in S300, deionized water is used to repeatedly rinse the porous composite membrane containing zirconium dioxide inorganic filler after S200 treatment, and the washing endpoint is controlled so that no free chloride ions and sodium ions can be detected in the eluent.

6. According to the method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer as proposed in claim 1, the specific process of dehydration and natural oxidation treatment in S400 is as follows: the porous composite membrane containing zirconium dioxide inorganic filler after being washed in S300 is placed in the air to dry naturally, so that ruthenium hydroxide colloid precipitate dehydrates and reacts with oxygen in the air to be converted into ruthenium dioxide hydrate and amorphous ruthenium dioxide nanoparticles.

7. The method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer according to claim 6 further includes the following specific steps in the dehydration and natural oxidation treatment: After being air-dried, the porous composite membrane containing zirconium dioxide inorganic filler is transferred to an oven set at 60°C for heat drying.

8. The method for preparing a heterogeneous interface membrane to improve the performance of an alkaline electrolyzer according to claim 1, wherein the areal loading of ruthenium dioxide nanoparticles generated on the surface of a porous composite membrane containing zirconium dioxide inorganic filler is controlled within the range of 0.02 to 0.20 mg / cm² by adjusting the concentration of the ruthenium precursor solution and the selectively applied treatment time, so that the ruthenium dioxide nanoparticles are distributed in a discontinuously dispersed state on the surface of the porous composite membrane containing zirconium dioxide inorganic filler.

9. A method for assembling an alkaline electrolytic cell, comprising the following steps: A heterogeneous interface membrane for improving the performance of an alkaline electrolyzer is prepared using any one of claims 1 to 8. A heterogeneous interface membrane is placed between the cathode and the anode, and the cathode, anode, and heterogeneous interface membrane are assembled to form an alkaline electrolytic cell.

10. The method for assembling an alkaline electrolytic cell according to claim 9, wherein the cathode is a NiMo cathode and the anode is a nickel mesh anode; the step of disposing a heterogeneous interface membrane between the cathode and the anode and assembling the cathode, the anode, and the heterogeneous interface membrane to form an alkaline electrolytic cell specifically comprises: disposing a heterogeneous interface membrane between the NiMo cathode and the nickel mesh anode, and assembling the NiMo cathode, the nickel mesh anode, and the heterogeneous interface membrane to form a zero-gap alkaline electrolytic cell.