A prebaked aluminum electrolysis anode insulation cover plate utilizing solid waste from production processes and its preparation method.

By using a modular insulated cover plate and a heat-locking groove convection channel system, and utilizing solid waste such as aluminum electrolysis waste cathodes and alumina dust as raw materials, the problems of high labor intensity, harsh environment and solid waste treatment in the aluminum electrolysis process have been solved, achieving efficient current distribution and resource utilization.

CN123108660APending Publication Date: 2026-11-17YUNNAN ALUMINUM
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611536010.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional bulk material covering methods in aluminum electrolysis are characterized by high labor intensity, harsh environment, high energy consumption, uneven current distribution, and solid waste treatment problems, and existing improvement solutions have not completely solved these problems.

Method used

The system adopts a modular insulated cover plate and uses solid waste such as aluminum electrolysis waste cathode and alumina dust as raw materials. It is designed with a heat-locking tank and a convection channel system to achieve controllable preheating of the new anode, stabilize the thermal balance of the electrolytic cell and improve current efficiency.

Benefits of technology

It reduced the labor intensity of workers, reduced heat loss, improved current efficiency, realized the resource utilization of solid waste, improved the working environment, and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108660A_ABST
    Figure CN123108660A_ABST
Patent Text Reader

Abstract

This invention relates to the field of aluminum electrolytic metallurgy, specifically disclosing a prebaked anode insulation cover plate for aluminum electrolysis utilizing solid waste from production processes, and its preparation method. The bottom wall of the insulation cover plate is shaped to match the top wall of the anode carbon block. The insulation cover plate includes at least two assembled plates for covering the anode carbon block, each composed of a frame layer and an insulation layer filled within the frame layer. This invention, through a unique heat-locking groove and convection channel design inside the cover plate, effectively guides excess heat in the electrolytic cell to the newly installed anode, thereby avoiding localized overcooling and solidification of the electrolyte caused by cold anode insertion, ensuring uniform current distribution, and improving current efficiency and anode lifespan. Simultaneously, this cover plate uses solid waste such as aluminum electrolysis waste cathodes and dust collection powder as main raw materials, realizing the resource utilization of solid waste. While improving harsh working environments and supporting mechanized anode switching, it provides an innovative solution for the green, efficient, and sustainable development of the aluminum industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrolytic aluminum metallurgy technology, and specifically discloses an aluminum electrolytic prebaked anode insulation cover plate utilizing production solid waste and its preparation method. Background Technology

[0002] The aluminum electrolysis industry is a vital foundation of the national economy. In the electrolytic aluminum production process, the prebaked anode, acting as the "heart," directly affects the stable operation of the electrolytic cell and various economic and technical indicators. To ensure anode performance, prevent high-temperature oxidation, and reduce heat loss from the electrolytic cell, traditional processes typically involve covering the top and periphery of the anode carbon block with a loose insulating material approximately 150-250 mm thick. This covering material is usually composed of crushed electrolyte and alumina powder mixed in a specific ratio.

[0003] However, this loose-material covering method, which has been used for decades, has many inherent drawbacks. First, replacing the anode (electrode replacement) requires a series of manual operations, including removing material, breaking shells, scooping up lumps, covering, and cleaning residual electrodes. This is extremely labor-intensive, the working environment is harsh, and workers are exposed to high-temperature radiation, hydrogen fluoride gas, and alumina dust for extended periods, seriously threatening their health. Second, the electrolytic cell cover needs to be kept open for a long time during electrode replacement, leading to significant heat loss, disrupting the thermal balance of the electrolytic cell, and increasing energy consumption. Third, during electrode replacement, the temperature of the new anode is lower, causing a sharp drop in the local temperature of the anode insertion area. This causes the electrolyte to solidify excessively around the anode, forming an excessively thick cell wall, and even preventing the anode bottom (the bottom surface participating in the reaction) from being properly wetted by the electrolyte, resulting in uneven current distribution and "current bias." This severely affects current efficiency and may damage the anode. Furthermore, the covering material sinters in the high-temperature environment inside the electrolytic cell, forming a hard crust. During the crushing, transportation, and recycling of this crust, a large amount of dust is generated, causing environmental pollution and increasing additional processing costs and energy consumption.

[0004] On the other hand, the aluminum electrolysis industry itself is a major generator of solid waste, and its disposal is becoming increasingly serious. Waste cathode carbon blocks produced during electrolytic cell overhauls, as well as dust collected during alumina production and aluminum ash washing residue, are all difficult-to-treat solid wastes. Waste cathodes, in particular, are classified as hazardous waste due to their content of fluorides and cyanides, with an annual generation reaching 10-20 kg per ton of aluminum. Their safe disposal has always been a common challenge for the industry. Meanwhile, dust collected during alumina production, due to its extremely fine particle size (usually less than 45μm), is difficult to process in electrolytic aluminum production and is often classified as substandard. Simply mixing it with qualified products for sale would lower the product grade rate. Effectively utilizing these solid wastes is key to achieving resource recycling and clean production.

[0005] To overcome the drawbacks of traditional bulk material covering, the industry has attempted some technological improvements. For example, Chinese invention patent CN107287622A discloses a method for constructing an anode insulation layer in a prebaked aluminum electrolytic cell. This method proposes constructing a double-layer insulation layer outside the electrolytic cell, above the anode carbon block: the bottom layer is a "soluble layer" that may come into contact with the electrolyte, composed of bulk covering material; the upper layer is a "non-soluble layer" using pre-formed, shaped insulating refractory bricks. This method moves some insulation work outside the cell and allows for the reuse of the upper shaped cover plate, improving the working environment and anode switching efficiency to some extent. However, this solution still does not completely eliminate the reliance on bulk covering material; the "soluble layer" still requires periodic construction and crushing, failing to fundamentally solve the problem of solid waste generation and disposal. Furthermore, its double-layer structure is relatively complex to install and fix.

[0006] Therefore, it is necessary to develop a new type of anode insulation cover plate solution that can realize mechanized anode replacement, controllably preheat the new anode during the anode replacement process, and dispose of aluminum industry solid waste on a large scale. This solution is of urgent practical significance for promoting the green, efficient and sustainable development of the aluminum electrolysis industry. Summary of the Invention

[0007] To address the aforementioned problems, this invention provides a prebaked anode insulation cover plate for aluminum electrolysis utilizing solid waste from production processes, along with its preparation method. Through a unique heat-locking groove and convection channel design within the cover plate, excess heat within the electrolytic cell is effectively guided to the newly installed anode, allowing it to preheat during the anode replacement process. This avoids the problem of localized overcooling and solidification of the electrolyte caused by the insertion of a cold anode. This not only stabilizes the thermal balance of the electrolytic cell but also ensures uniform current distribution, improving current efficiency and anode lifespan. Furthermore, this cover plate uses solid waste such as spent cathodes and dust from aluminum electrolysis as primary raw materials, achieving resource utilization of solid waste. While improving the harsh working environment and supporting mechanized anode replacement, it provides an innovative solution for the green, efficient, and sustainable development of the aluminum industry.

[0008] To achieve the above objectives, the technical solution of the present invention is as follows: A prebaked aluminum electrolysis anode insulation cover plate utilizing production solid waste is disposed on the top wall of the anode carbon block. The bottom wall of the insulation cover plate matches the shape of the top wall of the anode carbon block. The insulation cover plate includes at least two assembly plates for assembling and covering the anode carbon block. Each assembly plate consists of a frame layer and an insulation layer filled within the frame layer. The height of the insulation cover plate does not exceed the lower edge of the anode steel claw beam, and an operating space is reserved between the lower edge of the anode steel claw beam and the insulation cover plate.

[0009] This insulation cover, with its modular design and composite structure of a frame layer and an insulation layer, achieves a tight fit and full coverage with the anode carbon block, effectively reducing heat loss. At the same time, its ingenious height design ensures that the necessary space is reserved for the anode replacement operation without exceeding the anode steel claw crossbeam. This greatly facilitates installation, disassembly, and maintenance while ensuring excellent insulation performance, laying the foundation for mechanized anode replacement operations.

[0010] The core of this invention's solid waste utilization lies in the concept of "treating waste with waste and turning waste into treasure." Its technical approach involves transforming two typical solid wastes generated during aluminum electrolysis—waste cathode carbon blocks and alumina production dust / alumina ash washing residue—into functional materials for the main structure of the insulation cover. Specifically, waste cathode carbon blocks, containing fixed carbon and a certain amount of fluoride, after being crushed, possess inherent high-temperature resistance and electrical conductivity, making them ideal as aggregate for the frame layer. When combined with asphalt binder, they form a robust and corrosion-resistant support structure. Simultaneously, alumina dust, with its extremely fine particle size and difficulty in direct use during electrolysis, serves as the base material for the insulation layer. By adding foaming agents, it can be made into a lightweight insulation material with a porous structure. This process not only safely disposes of solid waste considered hazardous or industrial waste but also, through materials science formulation and processing, transforms them into high-value-added functional products, achieving a qualitative change from environmental burden to industrial raw material, forming a virtuous cycle of resources within the enterprise.

[0011] The key to the anode preheating principle of this invention lies in the heat-locking groove and convection channel system designed within the frame layer. In the high-temperature environment of normal electrolytic cell operation, this system cleverly utilizes the physical laws of heat convection and heat conduction. Heat escaping from the electrolytic cell is guided through specific convection channels to the recessed area reserved for the new anode. The height of these convection channels is designed to gradually decrease away from the recess, creating an effective thermal pressure difference, thereby continuously transferring heat to the area around the cold new anode. Simultaneously, the cooperation between the heat-locking groove and the sliding heat-locking block regulates and stores this heat, preventing its loss unnecessarily. This design is equivalent to constructing a localized, controllable "preheating zone" above the anode, enabling the new anode to heat up rapidly and uniformly during the anode replacement operation, reducing the temperature difference between it and the electrolyte, thus effectively preventing electrolyte solidification and "flow deviation" caused by localized overcooling, and stabilizing the thermal balance of the electrolytic cell.

[0012] Furthermore, the raw materials for the framework layer, by weight, include 60-90 parts of aluminum electrolysis waste cathode and calcined coke as aggregate, and 10-30 parts of bitumen as binder.

[0013] By using aluminum electrolysis waste cathode, a hazardous solid waste, together with calcined coke as aggregate for the frame layer, the harmless, resource-based, and high-value utilization of hazardous waste is achieved. This formula not only significantly reduces raw material costs but also gives the frame layer excellent high-temperature resistance, mechanical strength, and thermal stability, thus providing a robust support structure for the entire insulation cover. While solving environmental problems, it also ensures the product's service life under harsh working conditions.

[0014] Furthermore, the shape of the lower surface of the frame layer matches the shape of the top wall of the anode carbon block, the top wall of the frame layer has a groove, and the frame layer has a notch corresponding to the claw feet of the anode steel.

[0015] The structural design of the frame layer ensures a tight fit between its lower surface and the top wall of the anode carbon block, guaranteeing effective adhesion between the insulation cover and the anode and significantly reducing heat loss paths. Simultaneously, the grooves in the top wall provide ideal space for the insulation layer, ensuring the integrity and stability of the composite structure. The recesses specifically designed for the anode steel claws are a key design feature, precisely avoiding structural interference and allowing the cover to achieve full coverage without affecting the normal assembly and conductivity of the anode. This series of complementary structural features collectively lays the foundation for the insulation cover's efficient insulation and subsequent preheating functions.

[0016] Furthermore, the groove of the frame layer is provided with several reinforcing structures, which are metal mesh or ceramic fiber woven mesh pre-embedded in the frame layer material, or reinforcing ribs integrally formed in the groove.

[0017] By incorporating reinforcing structures such as metal mesh, ceramic fiber woven mesh, or integrally formed reinforcing ribs within the grooves of the frame layer, the overall mechanical strength and deformation resistance of the insulation cover plate are significantly improved under high-temperature load-bearing and frequent operation conditions. This design effectively prevents the cover plate from cracking or collapsing due to thermal stress, its own weight, or external impact, ensuring its structural integrity and long-term durability as a load-bearing substrate, thus providing a reliable guarantee for the stable operation of the upper insulation layer and the entire anode assembly.

[0018] Furthermore, heat-locking grooves are symmetrically opened on the edge of the frame layer, and heat-locking blocks are slidably fitted in each heat-locking groove. Several convection channels are opened in the frame layer. The bottom end of each convection channel is connected to the corresponding heat-locking groove, and the top end of each convection channel is connected to the side wall of the corresponding notch. The height of the convection channel increases as the distance from the notch decreases.

[0019] This structure, through the synergistic action of the convection channel, heat-locking groove, and heat-locking block, constructs an active heat guidance and control system. The heat-locking groove and sliding heat-locking block together act as a "thermal gate," effectively accumulating heat and regulating its release. Simultaneously, the unique convection channel design forms a heat transport path from the cell to the anode claw area, its height variation cleverly utilizing the natural upward effect of hot flue gas, effectively enhancing the guidance and flow efficiency of the heat flow. This principle allows excess heat within the electrolytic cell to be precisely guided to the vicinity of the newly installed anode, achieving active and efficient preheating of the cold anode.

[0020] Furthermore, the particle size distribution of the aggregate in the frame layer is as follows: 8-15mm particles account for ≤20%, 3-8mm particles account for ≥15%, 0-3mm particles account for ≥40%, and powder accounts for ≤38%.

[0021] Furthermore, the raw materials of the insulation layer, by weight, include 60-90 parts of base material, 5-15 parts of foaming agent, and 25-35 parts of binder and reinforcing agent; the base material is aluminum ash washing slag α-alumina and / or dust collection material produced from alumina; the binder and reinforcing agent is one or more of aluminum hydroxide, sodium aluminate, and water glass mixed with water.

[0022] Furthermore, the insulation layer is a foamed structure, a pressed structure, or a directly filled loose insulation material.

[0023] Furthermore, the outer surfaces of the frame layer and the insulation layer are coated with a high-temperature resistant protective coating with a thickness of not less than 0.05 mm.

[0024] By transforming solid waste such as aluminum ash washing slag and alumina dust into insulation layer base material, and scientifically proportioning foaming agents and special binders and reinforcing agents, the resource utilization of solid waste and the functionalization of the product are unified, thus producing an insulation layer with both excellent thermal insulation performance and sufficient structural strength. Multiple molding methods, including foaming, pressing, and bulk filling, are provided, offering high flexibility in production and application to adapt to different working conditions and manufacturing needs. Finally, a high-temperature resistant protective coating of no less than 0.05mm is applied to the outer surface of the cover plate, effectively resisting high-temperature oxidation and electrolyte vapor erosion, significantly improving the product's durability, sealing performance, and service life, ensuring its long-term effective operation in the harsh environment of the electrolytic cell.

[0025] A method for preparing a heat-insulating cover plate for aluminum electrolysis prebaked anodes utilizing production solid waste includes the following steps: Step 1: Crush the aggregate of the frame layer to the predetermined particle size and mix it. After heating, add the binder and knead it into a paste. Press it into shape under a pressure of ≥10MPa and then calcine it to obtain the frame layer. Step 2: Form the insulation layer using any of the following methods: (1) Fill the insulation layer mixture into the groove of the frame layer and press it into shape under a pressure of ≥10MPa; (2) Assemble the pre-formed insulation layer blocks into the grooves of the frame layer; (3) The bulk insulation material is directly filled into the groove of the frame layer; (4) Fill the insulation layer mixture into the groove of the frame layer and tamp it to initially shape it. Then bake it at 500℃~800℃ for 8-12 hours to make it foam and fill the groove. Step 3: Bake and cure the semi-finished product obtained in Step 2 at 500℃~800℃ for 8-12 hours; Step 4: Spray a high-temperature resistant protective coating onto the outer surface of the cured product and let it air dry naturally.

[0026] The beneficial effects of this invention are specifically reflected in the following aspects: (1) It transforms difficult-to-treat industrial solid wastes such as aluminum electrolysis waste cathodes (hazardous waste), alumina dust, and aluminum ash washing residue into core raw materials for the insulation cover frame layer and insulation layer. This not only significantly reduces the cost of solid waste disposal and environmental risks, but also solves the problem of difficult treatment of alumina roasting dust, indirectly improving the product grade rate of alumina production enterprises and promoting the green and circular development of the aluminum industry.

[0027] (2) The tight coverage of the assembled cover plate effectively reduces heat loss at the top of the anode, maintains the thermal balance of the electrolytic cell, and reduces energy consumption. The unique heat-locking tank-convection channel system can actively guide the residual heat to preheat the new anode in a controllable manner, avoiding local overcooling, solidification and "biased flow" of the electrolyte caused by the insertion of cold anode, thereby stabilizing the current distribution and improving the current efficiency.

[0028] (3) The modular design and the recessed notch for the anode steel claws make installation and disassembly simple, laying the foundation for mechanized anode switching and significantly reducing the labor intensity of workers. The reinforcing structure (metal mesh, reinforcing ribs, etc.) and scientific aggregate gradation within the frame layer ensure the structural strength and deformation resistance of the cover plate at high temperatures, extending its service life. The high-temperature resistant protective coating sprayed on the outer surface effectively resists high-temperature oxidation and electrolyte corrosion, further enhancing the product's durability and reliability.

[0029] (4) The insulation layer can be formed by various methods such as foaming, pressing, prefabrication, or bulk filling, which gives the production process great flexibility and can adapt to different production conditions and needs. The whole preparation method is mature and reliable, and it closely integrates solid waste treatment with product manufacturing, forming a complete and industrially feasible technical solution. Attached Figure Description

[0030] Figure 1 This is an isometric view of the heat-insulating cover plate for the prebaked aluminum electrolysis anode in Embodiment 1 of the present invention.

[0031] Figure 2 This is a top view of the heat-insulating cover plate for the prebaked anode in aluminum electrolysis in Embodiment 1 of the present invention.

[0032] Figure 3 In Experimental Example 1 of this invention Figure 2 Sectional view of AA.

[0033] Figure 4 In Experimental Example 1 of this invention Figure 2 A cross-sectional view of BB.

[0034] Figure 5 In Experimental Example 1 of this invention Figure 2 A sectional view of CC.

[0035] Reference numerals in the attached diagram: 1. Assembly plate; 2. Groove; 3. Notch; 4. Reinforcing rib; 5. Convection channel; 6. Heat-locking groove; 7. Heat-locking block. Detailed Implementation

[0036] The present invention will be further described below with reference to embodiments.

[0037] Example 1 Basic as Figures 1-5 As shown: The purpose of this embodiment is to provide a heat-insulating cover plate for aluminum electrolysis prebaked anodes utilizing production solid waste and its preparation method.

[0038] The insulation cover plate for prebaked anodes in aluminum electrolysis comprises, by weight, 70 parts waste cathode and 15 parts asphalt in the frame layer; the particle size distribution of the waste cathode is ≤20% for 8-15mm particles, ≥15% for 3-8mm particles, ≥40% for 0-3mm particles, and ≤38% for powder. The insulation layer comprises, by weight, 75 parts α-alumina or alumina dust collection powder from aluminum ash washing slag, 10 parts fluorocarbon environmentally friendly foaming agent, and 30 parts aluminum hydroxide or water glass and water.

[0039] The thermal insulation cover is prepared according to the following method: (1) Add the waste cathode, aluminum dihydrogen phosphate, fiber and water required for the frame layer to the dry mixing pot in a predetermined ratio, mix and stir for 35 minutes, then transfer to the wet mixing pot and add the binder to mix until uniform, forming a plastic paste. (2) A reinforcing rib 4 (or a metal mesh or ceramic fiber woven mesh) adapted to the groove 2 is pre-set in the mold of the frame layer. A symmetrical heat-locking groove 6 structure is reserved at the edge of the mold. At the same time, a convection channel 5 forming structure connected to the heat-locking groove 6 is pre-set in the mold at the position corresponding to the notch 3 of the anode steel claw. The height of the convection channel 5 increases as the distance from the notch 3 decreases. The frame layer paste is added to the mold and formed by vibration or stamping (stamping pressure 10MPa). Then it is fired to obtain a frame layer with reinforcing rib 4 (or metal mesh / ceramic fiber woven mesh), heat-locking groove 6 and convection channel 5. (3) Add the required alumina dust collection powder, fiber, aluminum dihydrogen phosphate and water to the mixing pot in a predetermined ratio, and mix and stir for 50 minutes until uniform; (4) Fill the insulation layer mixture into the frame layer groove 2 and continue to press it into shape using a press (pressing pressure 10MPa). (5) Install a suitable sliding heat-locking block 7 into the heat-locking groove 6 of the frame layer to ensure that the heat-locking block 7 and the heat-locking groove 6 slide together; (6) Place the molded block in an insulated oven and bake at 600℃ for 8 hours; (7) Apply the silicon nitride high temperature resistant protective coating evenly to the outer surface of the frame layer and the contact surface with the carbon block by mechanical means. The coating thickness is 0.05 mm. After spraying, let it air dry naturally for later use.

[0040] Example 2 The difference from the above embodiments lies in that the insulation cover plate for the prebaked anode of aluminum electrolysis comprises, by weight, 70 parts of waste cathode and 15 parts of asphalt in the frame layer; the particle size composition of the waste cathode is ≤20% for 8-15mm particles, ≥15% for 3-8mm particles, ≥40% for 0-3mm particles, and ≤38% for powder. The insulation layer comprises, by weight, 75 parts of α-alumina or alumina dust collection powder from aluminum ash washing slag, 10 parts of fluorocarbon environmentally friendly foaming agent, and 30 parts of aluminum hydroxide or water glass and water.

[0041] The thermal insulation cover is prepared according to the following method: (1) Add the waste cathode, aluminum dihydrogen phosphate, fiber and water required for the frame layer to the mixing pot in a predetermined ratio, and mix and stir for 25 minutes until uniform; (2) The frame layer forming mold has an integrally formed reinforcing rib 4, and the mold edge has symmetrical heat-locking grooves 6. The mold has a pre-set convection channel 5 that connects the heat-locking groove 6 with the anode steel claw foot notch 3 (the height of the convection channel 5 increases as the distance from the notch 3 decreases); the frame layer mixture is added to the mold and stamped (stamping pressure 10MPa), and then baked to obtain a frame layer with reinforcing rib 4, heat-locking groove 6 and convection channel 5. (3) Add the required raw materials for the insulation layer to the mixing pot in proportion, mix and stir for 45 minutes until uniform, and then add to the special mold for stamping (stamping pressure 10MPa). (4) Place the molded frame layer and insulation layer in an insulation box at 600℃ for 8 hours; (5) After curing, assemble the insulation layer block into the groove 2 of the frame layer to ensure tight fit; insert the sliding heat-locking block 7 into the heat-locking groove 6 of the frame layer to ensure smooth sliding of the heat-locking block 7. (6) Apply the silicon nitride high temperature resistant protective coating evenly to the outer surface of the frame layer and the contact surface with the carbon block using mechanical means. The coating thickness is 0.05 mm. After spraying, let it air dry naturally for later use.

[0042] Example 3 The difference from the above embodiments lies in that the insulation cover plate for the prebaked anode in aluminum electrolysis comprises, by weight, 70 parts of waste cathode and 15 parts of asphalt in the frame layer; the particle size distribution of the waste cathode is ≤20% for 8-15mm particles, ≥15% for 3-8mm particles, ≥40% for 0-3mm particles, and ≤38% for powder. The insulation layer comprises, by weight, 75 parts of α-alumina or alumina dust collection powder from aluminum ash washing slag, 10 parts of fluorocarbon environmentally friendly foaming agent, and 30 parts of aluminum hydroxide or water glass and water. The insulation layer material is loose alumina dust collection powder, α-alumina from aluminum ash washing slag, or existing insulation covering material.

[0043] The thermal insulation cover is prepared according to the following method: (2) Add the waste cathode, aluminum dihydrogen phosphate, fiber and water required for the frame layer to the mixing pot in a predetermined ratio, and mix and stir for 25 minutes until uniform; (2) A ceramic fiber woven mesh is pre-embedded in the mold of the frame layer as a reinforcing structure. Symmetrical heat-locking grooves 6 are opened on the edge of the mold. At the same time, a convection channel 5 is pre-set to connect the heat-locking groove 6 with the notch 3 of the anode steel claw (the height of the convection channel 5 increases as the distance from the notch 3 decreases). The frame layer mixture is added to the mold and stamped (stamping pressure 10MPa). It is placed in a heat preservation box at 600℃ for 8h to obtain a frame layer with ceramic fiber woven mesh, heat-locking groove 6 and convection channel 5. (3) Install sliding heat-locking blocks 7 into the heat-locking groove 6 of the frame layer to ensure that the fitting clearance meets the design requirements; (4) Spread the loose insulation material evenly into the groove 2 on the upper surface of the frame layer and compact it; (5) Apply the silicon nitride high temperature resistant protective coating evenly to the outer surface of the frame layer and the contact surface with the carbon block using mechanical means. The coating thickness is 0.05 mm. After spraying, let it air dry naturally for later use.

[0044] Example 4 The difference from the above embodiments lies in that the insulation cover plate for the prebaked anode of aluminum electrolysis comprises, by weight, 70 parts of waste cathode and 15 parts of asphalt in the frame layer; the particle size composition of the waste cathode is ≤20% for 8-15mm particles, ≥15% for 3-8mm particles, ≥40% for 0-3mm particles, and ≤38% for powder. The insulation layer comprises, by weight, 75 parts of α-alumina or alumina dust collection powder from aluminum ash washing slag, 10 parts of fluorocarbon environmentally friendly foaming agent, and 30 parts of aluminum hydroxide or water glass and water.

[0045] The thermal insulation cover is prepared according to the following method: (1) Add the waste cathode, aluminum dihydrogen phosphate, fiber and water required for the frame layer to the mixing pot in a predetermined ratio, and mix and stir for 25 minutes until uniform; (2) The frame layer forming mold has a pre-set reinforcing rib 4, and a symmetrical heat-locking groove 6 is opened on the edge of the mold. A convection channel 5 is pre-set to connect the heat-locking groove 6 with the notch 3 of the anode steel claw (the height of the convection channel 5 increases as the distance from the notch 3 decreases); the frame layer mixture is added to the mold and stamped (stamping pressure 10MPa) to obtain a frame layer with reinforcing rib 4, heat-locking groove 6 and convection channel 5. (3) Add the required raw materials for the insulation layer to the mixing pot in proportion, mix and stir for 40-60 minutes until uniform, fill into the groove 2 on the upper surface of the frame layer and tamp to initially shape; (4) Install sliding heat-locking block 7 into the heat-locking groove 6 of the frame layer, and then put the molded block into the heat-insulating box at 600℃ for 8 hours to allow the heat-insulating layer to fully foam and fill the groove 2 and integrate with the frame layer. (5) Apply the silicon nitride high temperature resistant protective coating evenly to the outer surface of the frame layer and the contact surface with the carbon block using mechanical means. The coating thickness is 0.05 mm. After spraying, let it air dry naturally for later use.

[0046] The main difference between Examples 1 to 4 lies in the different molding methods of the insulation cover, resulting in differences in the molding process of the insulation cover. Example 1 uses two continuous stamping processes, which is highly efficient but has a complex structure and a high specific gravity of the molded block. Example 2 uses two separate stamping processes followed by assembly, which is slightly less efficient but still has a high specific gravity. Example 3 uses a method where loose insulation material is added to the groove 2 on the upper surface after the frame layer is formed. This method is relatively simple and efficient, but it has some dust problems. Example 4 uses a method where the insulation layer is foamed after the frame layer is formed. This method is dust-free, has simple molds, and the foamed block has good insulation effect and relatively good mechanical properties.

[0047] Experimental Example 1 This experimental example aims to verify the effect of the heat-insulating cover plate of the present invention on the preheating effect of the internal convection channel 5 structure on the cold new anode during the anode replacement process, and its influence on the operational stability of the electrolytic cell.

[0048] (1) Experimental methods Grouping settings: Select several electrolytic cells with similar operating conditions and divide them into two groups.

[0049] Experimental group: When replacing the anode, use the heat-insulating cover plate with the structure of heat-locking groove 6 and convection channel 5 described in this invention.

[0050] Control group: When replacing the anode, the traditional method of covering with loose insulation material was used.

[0051] Measurement and Recording: Before replacing the anode, record the reference voltage and temperature of the cell.

[0052] After replacing the anode, immediately insert the thermocouple into the base of the steel claw of the new anode (near notch 3) and start timing.

[0053] Record the temperature at the root of the new anode steel claw at 0.5 hours, 1 hour, 2 hours and 4 hours after the electrode replacement.

[0054] Record the voltage fluctuation range of the electrolytic cell (the maximum deviation from the set voltage) within 24 hours after the electrode change.

[0055] Observe and record the thickness of the electrolyte crust (tank side) around the new anode after the electrode replacement.

[0056] (2) Experimental results As shown in Table 1 below: Table 1. Variations in anode temperature and voltage

[0057] (3) Experimental conclusions The experimental results show that the insulation cover, through its internal convection channel 5 and heat-locking groove 6 system, can efficiently guide excess heat from the electrolytic cell to the newly installed anode, achieving a rapid and significant preheating effect. This not only effectively increases the initial temperature of the anode itself, but more importantly, it stabilizes the operating conditions of the electrolytic cell, reduces voltage fluctuations, and prevents the formation of excessively thick cell walls, thus laying a solid foundation for improving current efficiency and reducing energy consumption. This design successfully transforms traditional passive insulation into active thermal management, solving the long-standing problem of cold anode insertion in electrolytic aluminum production.

Claims

1. A heat-insulating cover plate for aluminum electrolysis prebaked anodes utilizing solid waste from production processes, disposed on the top wall of the anode carbon block, characterized in that: The bottom wall of the insulation cover plate matches the shape of the top wall of the anode carbon block. The insulation cover plate includes at least two assembly plates (1) for assembling and covering the anode carbon block. Each assembly plate (1) consists of a frame layer and an insulation layer filled in the frame layer. The height of the insulation cover plate does not exceed the lower edge of the anode steel claw beam, and there is an operating space reserved between the lower edge of the anode steel claw beam and the insulation cover plate.

2. The aluminum electrolysis prebaked anode insulation cover plate according to claim 1, characterized in that: The raw materials for the framework layer, by weight, include 60-90 parts of aluminum electrolysis waste cathode and calcined coke as aggregate, and 10-30 parts of bitumen as binder.

3. The aluminum electrolysis prebaked anode insulation cover plate according to claim 1 or 2, characterized in that: The shape of the lower surface of the frame layer matches the shape of the top wall of the anode carbon block. The top wall of the frame layer has a groove (2), and the frame layer has a notch (3) corresponding to the claw feet of the anode steel.

4. The aluminum electrolysis prebaked anode insulation cover plate according to claim 3, characterized in that: The groove (2) of the frame layer is provided with several reinforcing structures. The reinforcing structures are metal mesh or ceramic fiber woven mesh pre-embedded in the frame layer material, or reinforcing ribs (4) integrally formed in the groove (2).

5. The aluminum electrolysis prebaked anode insulation cover plate according to claim 4, characterized in that: The frame layer has symmetrical heat-locking grooves (6) on its edge. Each heat-locking groove (6) has a heat-locking block (7) that slides inside it. The frame layer has several convection channels (5). The bottom of each convection channel (5) is connected to the corresponding heat-locking groove (6), and the top of each convection channel (5) is connected to the side wall of the corresponding recess (3). The height of the convection channel (5) increases as the distance from the recess (3) decreases.

6. The aluminum electrolysis prebaked anode insulation cover plate according to claim 2, characterized in that: The particle size distribution of the aggregate in the frame layer is as follows: 8-15mm particles ≤20%, 3-8mm particles ≥15%, 0-3mm particles ≥40%, and powder ≤38%.

7. The thermal insulation cover plate for aluminum electrolysis prebaked anodes according to claim 1, characterized in that: The raw materials of the insulation layer, by weight, include 60-90 parts of base material, 5-15 parts of foaming agent, and 25-35 parts of binder and reinforcing agent; the base material is aluminum ash washing slag α-alumina and / or dust collection material produced from alumina; the binder and reinforcing agent is one or more of aluminum hydroxide, sodium aluminate, and water glass mixed with water.

8. The aluminum electrolysis prebaked anode insulation cover plate according to claim 1 or 7, characterized in that: The insulation layer is a foamed structure, a pressed structure, or a directly filled loose insulation material.

9. The aluminum electrolysis prebaked anode insulation cover plate according to claim 1, characterized in that: The outer surfaces of the frame layer and insulation layer are coated with a high-temperature resistant protective coating with a thickness of not less than 0.05 mm.

10. A method for preparing a heat-insulating cover plate for aluminum electrolytic prebaked anodes utilizing production solid waste as described in any one of claims 1-9, characterized in that, Includes the following steps: Step 1: Crush the aggregate of the frame layer to the predetermined particle size and mix it. After heating, add the binder and knead it into a paste. Press it into shape under a pressure of ≥10MPa and then calcine it to obtain the frame layer. Step 2: Form the insulation layer using any of the following methods: (1) Fill the insulation layer mixture into the groove of the frame layer (2) and press it into shape under a pressure of ≥10MPa; (2) Assemble the pre-formed insulation layer blocks into the groove (2) of the frame layer; (3) The bulk insulation material is directly filled into the groove (2) of the frame layer; (4) Fill the insulation layer mixture into the groove (2) of the frame layer and tamp it to initially shape it. Then bake it at 500℃~800℃ for 8-12 hours to make it foam and fill the groove (2). Step 3: Bake and cure the semi-finished product obtained in Step 2 at 500℃~800℃ for 8-12 hours; Step 4: Spray a high-temperature resistant protective coating onto the outer surface of the cured product and let it air dry naturally.

Citation Information

Patent Citations

  • Process method for structure of anode insulating layer of pre-baked aluminum electrolytic cell

    CN107287622A