A method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition

By adding specific metal compounds to the tungstate molten salt system, tungsten-based solid solution alloy coatings are prepared by in-situ electrodeposition, which solves the problems of uneven grain size and poor ductility in existing tungsten coatings and realizes the preparation of high-performance tungsten coatings suitable for high-temperature and corrosion-resistant environments.

CN123108677APending Publication Date: 2026-11-17XINXIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611401233.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing tungsten coating preparation processes are insufficient to produce tungsten coatings with fine grains, high density, and smooth surfaces. Furthermore, the coatings have poor plasticity and toughness, making it difficult to meet the strength and toughness requirements of high-end applications.

Method used

A molten salt system containing tungstate is used, and a metal compound that can form a solid solution or intermetallic compound with tungsten is added. A tungsten-based solid solution alloy coating is prepared by in-situ electrodeposition. Electrolysis parameters are adjusted to achieve co-reduction deposition of tungsten ions, thereby controlling grain refinement and improving adhesion.

Benefits of technology

A tungsten-based solid solution alloy coating with fine grains, high density, smooth surface, high hardness, and good toughness was prepared, which improved the overall performance of the coating. The process is simple and low-cost, and it is suitable for high-temperature or corrosion-resistant protection of heat sink materials such as copper and its alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108677A_ABST
    Figure CN123108677A_ABST
Patent Text Reader

Abstract

This invention relates to the field of surface engineering technology, specifically to a method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition. The method uses a molten salt system composed of tungstate, tungsten trioxide, and a metal compound as the electrolyte. The metal compound is one or more compounds selected from rhenium, chromium, molybdenum, titanium, aluminum, vanadium, potassium, iridium, hafnium, tantalum, or niobium. Under inert gas protection, using a tungsten-containing electrode or an inert electrode as the auxiliary electrode and a conductive plated part as the working electrode, in-situ electrodeposition at 700-1000°C is performed using constant current or constant potential to obtain the tungsten-based solid solution alloy coating. This method, through solid solution strengthening, results in a dense coating structure, fine grains, high bonding strength, and good toughness. This invention is characterized by high efficiency, environmental friendliness, short process, and controllable product quality. It is simple to operate, low in cost, and suitable for high-temperature or corrosion-resistant protection of heat sink materials such as copper and its alloys, with broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of surface engineering technology, and more specifically to a method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition. Background Technology

[0002] Tungsten is valued for its extremely high melting point (3695 K) and extremely low vapor pressure (3695 K, 1.3 × 10⁻ ... 7 With its excellent mechanical strength, high thermal conductivity, and good thermal stability, tungsten has irreplaceable application value in high-end fields such as aerospace, electronics, and nuclear energy. Especially in the field of plasma materials, by depositing a tungsten coating on the surface of a copper substrate, the high temperature resistance of tungsten can be fully utilized to expand its application scenarios.

[0003] Copper is an ideal substrate material for preparing tungsten coatings due to its excellent thermal and electrical conductivity. However, copper itself has a low melting point and poor corrosion resistance, making it difficult to apply directly to high-temperature conditions. Tungsten, on the other hand, has inherent defects such as low fracture toughness and a high ductile-brittle transition temperature (673 K), which severely restricts its machinability and welding performance. Therefore, preparing tungsten coatings on the surface of copper substrates through coating technology and using tungsten as a protective layer for the copper substrate has become a feasible way to solve the above problems and expand the application range of both materials.

[0004] Currently, the mainstream preparation processes for tungsten coatings include vacuum plasma spraying (VPS), physical vapor deposition (PVD), chemical vapor deposition (CVD), and electrodeposition. However, due to the inherent chemical properties of tungsten, the electrochemical window of the aqueous electrolyte system is relatively narrow, and tungsten cannot be electrodeposited independently from aqueous solutions. Therefore, tungsten coatings can only be electrodeposited through molten salt systems. Existing molten salt systems for tungsten electrodeposition are mainly divided into three categories: The first category is halide systems (such as fluoride and chloride molten salts), which have the advantages of low melting point and high current efficiency. However, halide molten salts usually have strong hygroscopicity and corrosiveness, and are prone to volatilization at high temperatures, requiring stringent equipment corrosion resistance and making it difficult to control the operating environment. The second category is halide-oxide composite systems, where the stability of molten salts can be improved by adding oxides to halides. However, this type of system has a complex composition, many side reactions, and an insufficiently wide electrochemical window. In addition, the solubility of oxides is limited, making it difficult to obtain high tungsten ion concentrations. The third category is oxide molten salt systems (such as tungstate-tungsten trioxide systems), which have good stability, relatively low equipment corrosivity, and a wide adjustable range of tungsten source concentration. This is currently the most studied system. However, oxide molten salts have high melting points, usually requiring operation above 700℃, and the molten salt viscosity is high, limiting mass transfer capacity and easily leading to uneven deposition layer growth. To ensure excellent performance and long service life of tungsten coatings, the preparation of tungsten coatings with fine grains, dense structure, and smooth surface has become a key research focus in this field. In existing technologies, researchers have attempted to lower the melting point of molten salt, enhance cathodic polarization, and refine grains by introducing additives (such as rare earth oxides and alkaline earth metal compounds) into the molten salt system. However, the introduction of these additives often makes it difficult to precisely control their dissolution behavior and electrochemical activity in the molten salt. Nodules or coarse grains still exist on the coating surface, resulting in uneven tungsten grain growth, reduced coating density and smoothness, and consequently affecting the mechanical properties and protective effect of the coating. Furthermore, coatings obtained by existing technologies are mostly pure tungsten or composite coatings of tungsten and second-phase particles. Their essence remains pure tungsten as the matrix, and the inherent brittleness of tungsten is not changed. The coatings have poor ductility and toughness, and are prone to cracking or even spalling under thermal cycling or stress loading, making it difficult to meet the comprehensive requirements of high-end applications for coating strength and toughness. Summary of the Invention

[0005] To address the shortcomings of the prior art, the present invention aims to provide a method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition. This method can produce high-strength and high-toughness tungsten-based solid solution alloy coatings with finer grains, higher flatness, and higher density, suitable for high-temperature or corrosion-resistant protection of various heat sink material substrates such as copper and its alloys.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: A method for preparing a tungsten-based solid solution alloy coating by molten salt electrodeposition is disclosed. The method uses a molten salt system containing tungstate as the base electrolyte, and adds a metal compound that can form a solid solution or intermetallic compound with tungsten to prepare the molten salt electrolyte. The molten salt electrolyte is then prepared by in-situ electrodeposition to prepare a solid solution alloy coating with tungsten phase as the main component.

[0007] The metal compound is one or more of the following: rhenium, chromium, molybdenum, titanium, aluminum, vanadium, potassium, iridium, hafnium, tantalum, or niobium.

[0008] In a preferred embodiment of the present invention, the molten salt system is composed of tungstate, tungsten trioxide and the metal compound, wherein the molar ratio of tungstate to tungsten trioxide is 1:0.01~0.6.

[0009] In a preferred embodiment of the present invention, the metal compound is a metal oxide or a metal tungstate, and the amount of the metal compound added to the molten salt system is 1 to 50 mol.

[0010] Furthermore, the amount of metal compound added to the molten salt system is preferably 2 to 20 mol.

[0011] In the tungstate system described in this invention, tungstate mainly acts as a solvent. It can react with added tungsten trioxide to promote the dissolution of tungsten trioxide, thereby increasing the tungsten source concentration in the molten salt medium. Tungsten trioxide of different molar ratios is added as a solute to the molten salt system, increasing the tungsten ion concentration and making the electrodeposition reaction easier to occur. Simultaneously, different molar ratios of molten salt systems will result in differences in the electrodeposited tungsten coating. Higher tungsten source concentrations lead to increased tungsten coating thickness, roughness, and grain size. This invention has found that controlling the amounts of each component in the tungstate system within the aforementioned range is beneficial for balancing electrodeposition reaction efficiency and the performance of the resulting tungsten coating.

[0012] In a preferred embodiment of the present invention, the tungstate is one or more of Na2WO4, K2WO4 and Li2WO4, more preferably Na2WO4.

[0013] In a preferred embodiment of the present invention, the method includes: under inert gas protection, using a soluble tungsten-containing electrode or an inert electrode as an auxiliary electrode and a conductive plated part as a working electrode, heating and melting the molten salt electrolyte and holding it at a certain temperature to perform in-situ electrodeposition.

[0014] In a preferred embodiment of the present invention, in-situ electrodeposition is either constant current electrodeposition or constant potential electrodeposition.

[0015] The current density of the constant current electrodeposition is 5~150 mA / cm².

[0016] The working potential for the constant potential electrodeposition is 0.1~2.0 V.

[0017] In a preferred embodiment of the present invention, the heating and melting temperature and the holding temperature are 700~1000℃.

[0018] In a preferred embodiment of the present invention, the surface roughness of the conductive plating is less than Ra 2.0 μm, and the conductivity is greater than 180 S / cm.

[0019] In a preferred embodiment of the present invention, the inert gas is selected from helium, neon, and argon.

[0020] Compared with the prior art, the beneficial effects of the present invention are: 1. The method provided by this invention involves adding a specific metal compound to a tungstate system and in-situ electrodepositing to obtain a tungsten-based solid solution alloy coating. The formation process involves metal ions in the metal compound that can dissolve with tungsten dissolving into a molten salt electrolyte to form free ions. By adjusting electrolysis parameters such as applied current density, metal compound type and concentration, and external voltage, co-reduction deposition of these ions and tungsten ions is achieved. Specifically, the type and concentration of the metal compound alter the reduction potential of the metal ions, while the current density and applied voltage adjust the electrodeposition parameters. Through the combined effect of multiple deposition conditions, co-deposition of the tungsten-based solid solution alloy coating is achieved. The dragging and suppression of grain boundary migration by solute atoms can refine the grains. Finer grains adhere to the substrate, providing more bonding sites and improving the adhesion between the coating and the substrate. The introduction of solute atoms through solid solution introduces lattice distortion, which enhances atomic diffusion and removes harmful oxide impurities from the substrate, leading to increased density. Simultaneously, the distorted stress field generates a pinning effect, hindering dislocation movement and improving the alloy's hardness and strength. The solute introduced through solid solution treatment modulates the electronic structure, optimizes dislocation slip, captures harmful interstitial impurities, and strengthens grain boundary bonding. This can eliminate the intrinsic brittleness of tungsten metal with a body-centered cubic structure, improve ductility and toughness, and reduce bottom-to-tightness transition temperature (DBTT). In summary, the co-deposition of solid solution alloys results in a denser tungsten coating structure with smaller grains, higher bonding strength, greater hardness, and better overall toughness and strength.

[0021] 2. The method provided by the present invention can obtain a smooth and flat tungsten alloy coating without subsequent processing. Compared with the rough tungsten coating obtained by electrodeposition in the prior art, the tungsten coating obtained by the present invention has superior strength and toughness.

[0022] 3. The method provided by this invention can separate tungsten from other elements in tungsten-containing alloys and directly prepare tungsten coating materials without the need for other means such as hydrometallurgy. Since the method provided by this invention directly prepares tungsten coatings at high temperatures, the resulting tungsten coatings have good thermal shock resistance. The method provided by this invention is characterized by high efficiency, greenness, short process, controllable products, simple process equipment, convenient operation, low cost, and broad prospects for practical application. Attached Figure Description

[0023] Figure 1 The image shows the XRD pattern of the tungsten alloy coating obtained in Example 1 of this invention.

[0024] Figure 2 This is a SEM image of the tungsten alloy coating surface obtained in Example 1 of the present invention.

[0025] Figure 3 This is a SEM-EDS image of the cross-section of the tungsten alloy coating obtained in Example 2 of the present invention.

[0026] Figure 4 The image shows the XRD pattern of the tungsten coating obtained in Comparative Example 1 of this invention.

[0027] Figure 5 This is a SEM image of the tungsten coating obtained in Comparative Example 1 of this invention. Detailed Implementation

[0028] The following detailed description, in conjunction with embodiments of the present invention and accompanying drawings, provides a clear and complete illustration of the technical solutions in these embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0029] It should be noted that all technical terms used in this invention are for the purpose of describing specific embodiments only and are not intended to limit the scope of protection of this invention. Unless otherwise specified, all raw materials, reagents, instruments and equipment used in the following embodiments of this invention can be purchased from the market or prepared by existing methods.

[0030] In one specific embodiment of the present invention, the method for preparing a tungsten alloy coating by in-situ electrodeposition in molten salt includes the following steps: S1. The soluble tungsten alloy or inert electrode after mechanical processing is placed in acetone, alcohol and deionized water for ultrasonic cleaning in sequence, and then dried to obtain the auxiliary electrode for later use.

[0031] S2. After the conductive plated part is processed to a smooth and flat surface, it is ultrasonically cleaned in acetone, alcohol and deionized water in sequence, and then dried to obtain the working electrode for later use.

[0032] S3. Mix the molten salt electrolyte raw materials that have been pre-vacuum dried and dehydrated according to the formula, heat them to 700-1000℃ under inert gas protection, and keep them at the temperature for 2-4 hours to melt them evenly.

[0033] S4. Place the auxiliary electrode and the working electrode in molten salt and deposit them using constant current or constant potential. After the deposition is completed, remove the working electrode and immerse it in alkaline solution. After cleaning, dry it to obtain the final product.

[0034] Example 1 This embodiment provides a method for preparing tungsten-chromium alloy coatings by molten salt electrodeposition, using a pure tungsten electrode (99.99 wt% tungsten content) as an auxiliary electrode and a copper plate as a working electrode, and employing a constant current electrodeposition process.

[0035] Specifically, it includes the following steps: S1. The pure tungsten is mechanically cut to obtain a suitable size, and then mechanically polished to remove dirt and rust. It is then ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and dried for later use.

[0036] S2. The copper plate is mechanically cut, ground and polished until the surface is smooth and has a metallic luster. It is then ultrasonically cleaned in acetone, alcohol and deionized water in sequence, and dried for later use.

[0037] S3. Na2WO4, WO3, and Cr2O3 are pre-dried in a vacuum drying oven at 200℃ for 24 hours to perform dehydration treatment.

[0038] S4. Weigh out a certain amount of Na2WO4 and WO3 molten salt according to the molar percentage, wherein the molar ratio of Na2WO4 to WO3 is 1:0.33, and then add 2% (3.6 mol%) of Cr2O3. After mixing the above drying reagents evenly, place them in an electric resistance furnace, and under the protection of inert gas, raise the temperature to 900℃ at a stable heating rate, and hold at this temperature for 3 hours to allow the molten salt to fully melt.

[0039] S5. Immerse each electrode in the molten salt, connect to the electrochemical workstation, and use constant current deposition technology, setting the cathode current density to 40 mA / cm². 2 Electrodeposition was performed for 3 hours.

[0040] S6. After electrodeposition, remove the working electrode, immerse it in a 5M strong alkaline solution, and then rinse it with water to remove the adhering salt on the coating surface.

[0041] Example 2 A method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition is provided, comprising the following steps: This embodiment provides a method for preparing tungsten-molybdenum alloy coatings by molten salt electrodeposition, using a pure tungsten electrode (99.99 wt% tungsten content) as an auxiliary electrode and a copper plate as a working electrode, and employing a constant potential electrodeposition process.

[0042] Specifically, it includes the following steps: S1. The pure tungsten is mechanically cut to obtain a suitable size, and then mechanically polished to remove dirt and rust. It is then ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and dried for later use.

[0043] S2. The copper plate is mechanically cut, ground and polished until the surface is smooth and has a metallic luster. It is then ultrasonically cleaned in acetone, alcohol and deionized water in sequence, and dried for later use.

[0044] S3. Na2WO4, WO3, Na2MoO4, and MoO3 are pre-dried in a vacuum drying oven at 200℃ for 24 hours to perform dehydration treatment.

[0045] S4. Weigh a certain amount of molten salt according to the molar percentage, wherein the molar ratio of Na2WO4, WO3, Na2MoO4, and MoO3 is 3:1:3:0.6. After mixing the above drying reagents evenly, place them in an electric resistance furnace and, under the protection of an inert gas, raise the temperature to 900℃ at a stable heating rate, and hold at that temperature for 3 hours to allow the molten salt to fully melt.

[0046] S5. Immerse each electrode in molten salt, connect to an electrochemical workstation, and use constant potential deposition technology. Set the cathode potential to -0.5V and perform electrodeposition for 2 hours.

[0047] S6. After electrodeposition, remove the working electrode, immerse it in a 5M strong alkaline solution, and then rinse it with water to remove the adhering salt on the coating surface.

[0048] Example 3 A method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition is provided, comprising the following steps: This embodiment provides a method for preparing a tungsten-rhenium alloy coating by molten salt electrodeposition, using a pure tungsten electrode (99.99 wt% tungsten content) as an auxiliary electrode and a copper plate as a working electrode, and employing a constant current electrodeposition process.

[0049] Specifically, it includes the following steps: S1. The pure tungsten is mechanically cut to obtain a suitable size, and then mechanically polished to remove dirt and rust. It is then ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and dried for later use.

[0050] S2. The copper plate is mechanically cut, ground and polished until the surface is smooth and has a metallic luster. It is then ultrasonically cleaned in acetone, alcohol and deionized water in sequence, and dried for later use.

[0051] S3. K2WO4, WO3, and K2ReO4 are pre-dried in a vacuum drying oven at 200℃ for 24 hours to perform dehydration treatment.

[0052] S4. Weigh out a certain amount of K2WO4, WO3, and K2ReO4 molten salt according to the molar percentage, with a molar ratio of 3:1:1. After mixing the above drying reagents evenly, place them in an electric resistance furnace and, under the protection of an inert gas, raise the temperature to 900℃ at a stable heating rate, and hold at that temperature for 3 hours to allow the molten salt to fully melt.

[0053] S5. Immerse each electrode in the molten salt, connect to the electrochemical workstation, and use potentiostatic deposition technology to set the cathode potential to 50 mA / cm². 2 Electrodeposition was performed for 3 hours.

[0054] S6. After electrodeposition, remove the working electrode, immerse it in a 5M strong alkaline solution, and then rinse it with water to remove the adhering salt on the coating surface.

[0055] Comparative Example 1 This comparative example provides a method for preparing tungsten coatings by in-situ electrodeposition using molten salt. A pure tungsten electrode (99.99 wt% tungsten content) is used as an auxiliary electrode, and a copper plate is used as the working electrode. The coating is prepared using a constant current electrodeposition process.

[0056] Specifically, it includes the following steps: S1. The pure tungsten electrode is mechanically cut to obtain a suitable size, and then mechanically polished to remove dirt and rust. It is then ultrasonically cleaned in acetone, alcohol, and deionized water in sequence, and dried for later use.

[0057] S2. The copper plate is mechanically cut, ground and polished until the surface is smooth and has a metallic luster. It is then ultrasonically cleaned in acetone, alcohol and deionized water in sequence, and dried for later use.

[0058] S3. Na2WO4 and WO3 are pre-dried in a vacuum drying oven at 200℃ for 24 hours to perform dehydration treatment.

[0059] S4. Weigh out a certain amount of Na2WO4 and WO3 molten salt according to the molar percentage, where (n)Na2WO4:(n)WO3 = 1:0.33. Place the well-mixed salt into a resistance furnace, and under the protection of inert gas, raise the temperature to 900℃ at a stable heating rate, and hold for 3 hours to allow the molten salt to fully melt.

[0060] S5. Immerse each electrode in the molten salt, connect to the electrochemical workstation, and use constant current deposition technology, setting the cathode current density to 40 mA / cm². 2 Electrodeposition was performed for 3 hours.

[0061] S6. After electrodeposition, remove the working electrode, immerse it in a 5M strong alkaline solution, and then rinse it with water to remove the adhering salt on the coating surface.

[0062] Results Analysis Figure 1 The image shows the XRD pattern of the tungsten alloy coating obtained in Example 1. It can be seen that there are two phases in the coating: tungsten and chromium.

[0063] Figure 2 The SEM image of the tungsten alloy coating obtained in Example 1 shows that the tungsten coating has a dense structure, with no obvious pores or gaps, complete grains, and a smooth overall surface. The oxygen content of the coating was determined by a nitrogen-oxygen analyzer and was 0.026 wt%. The hardness of the tungsten alloy coating prepared in Example 1 was measured by a microhardness tester. Ten points were taken from the sample, and the average hardness was 492.38 HV. The adhesion strength was measured by the coating scratch method and was 43.57 MPa. The ductility and toughness were measured by a three-point bending test, and the total elongation at break was 14.7%.

[0064] Figure 3 The cross-sectional SEM-EDS image of the tungsten coating obtained in Example 2 shows that the distribution positions of W and Mo elements in the coating are highly consistent, indicating the formation of a W-Mo solid solution alloy coating.

[0065] Figure 4 The image shows the XRD pattern of the tungsten coating prepared in Comparative Example 1. It can be seen that the coating does not contain any impurity phases and is a pure tungsten phase.

[0066] Figure 5 The image shows a SEM image of the tungsten coating prepared in Comparative Example 1. It can be seen that the tungsten coating has no obvious pores or cracks, and the surface has many coarse grains. The average grain size, determined by the scribing method, is 18.68 μm. The oxygen content of the coating was measured using a nitrogen and oxygen analyzer and was 0.048 wt%.

[0067] The hardness of the tungsten coating prepared in Comparative Example 1 was measured by a microhardness tester. Ten points were taken from the sample, and the average hardness was 483.85 HV. The adhesion was measured by the coating scratch method, and the value was 38.83 MPa. The ductility and toughness were measured by the three-point bending test, and the total elongation at break was 7.9%.

[0068] In summary, the method of this invention can prepare high-performance tungsten alloy coatings with a short process and low cost. The prepared coating has fine and complete grains, high density, smooth surface, high hardness, and good toughness, achieving a significant improvement in the performance of tungsten coatings.

[0069] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described here to avoid redundancy. Although preferred embodiments of the invention have been described, those skilled in the art, once they understand the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of this invention.

[0070] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.

Claims

1. A method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition, characterized in that, Using a molten salt system containing tungstate as the base electrolyte, a molten salt electrolyte is prepared by adding a metal compound that can form a solid solution or intermetallic compound with tungsten. The molten salt electrolyte is then prepared by in-situ electrodeposition to create a solid solution alloy coating with tungsten as the main phase. The metal compound is one or more of the following: rhenium, chromium, molybdenum, titanium, aluminum, vanadium, potassium, iridium, hafnium, tantalum, or niobium. The amount of metal compound added to the molten salt system is 1~50 mol.

2. The method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition according to claim 1, characterized in that, The molten salt system consists of tungstate, tungsten trioxide and the metal compound, wherein the molar ratio of tungstate to tungsten trioxide is 1:0.01~0.

6.

3. The method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition according to claim 1, characterized in that, The metal compound is a metal oxide or a metal tungstate.

4. The method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition according to claim 1, characterized in that, Tungstate is one or more of Na2WO4, K2WO4 and Li2WO4.

5. The method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition according to claim 1, characterized in that, The method includes: under inert gas protection, using a soluble tungsten-containing electrode or an inert electrode as an auxiliary electrode and a conductive plated part as a working electrode, heating and melting the molten salt electrolyte and holding it at a certain temperature to perform in-situ electrodeposition.

6. The method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition according to claim 5, characterized in that, In-situ electrodeposition is either constant current electrodeposition or constant potential electrodeposition; the current density of the constant current electrodeposition is 5~150 mA / cm²; the working potential of the constant potential electrodeposition is 0.1~2.0 V.

7. The method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition according to claim 5, characterized in that, The heating and melting temperature and the holding temperature are 700~1000℃.

8. The method for preparing tungsten-based solid solution alloy coatings by molten salt electrodeposition according to claim 5, characterized in that, The surface roughness of the conductive plated part is less than Ra 2.0μm, and the conductivity is greater than 180 S / cm.