A method for rapidly depositing Fe2O3-doped carbon coatings on carbon fibers

By employing cathode plasma electrolytic deposition technology and in-situ generation of catalytic Fe2O3 from iron salts, a network-distributed Fe2O3-doped carbon coating was prepared, which solved the problems of uneven deposition and low carbonization efficiency on the carbon fiber surface and improved the interfacial bonding performance.

CN123108685APending Publication Date: 2026-11-17BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611083683.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to uniformly deposit a doped metal oxide carbon coating on the surface of carbon fibers, and the low carbonization efficiency of organic carbon sources leads to poor interfacial bonding performance.

Method used

A network-distributed Fe2O3-doped carbon coating was prepared by using cathode plasma electrolytic deposition technology, which involves non-electrode mobile deposition and in-situ generation of catalytic Fe2O3 from iron salts, combined with the synergistic control of voltage and mobile speed.

Benefits of technology

The rapid and uniform deposition of Fe2O3-doped carbon coating on the carbon fiber surface was achieved, which improved the interfacial shear strength and interfacial bonding performance between the carbon fiber and the resin matrix.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108685A_ABST
    Figure CN123108685A_ABST
Patent Text Reader

Abstract

This invention relates to a method for rapidly depositing an Fe2O3-doped carbon coating on carbon fibers, belonging to the field of carbon fiber surface modification technology. A mixed aqueous solution containing an organic carbon source and iron salt is used as the electrolyte. A graphite plate is used as the anode, and a copper rod is used as the cathode. The copper rod is positioned above the electrolyte with its lower end face pressed against the electrolyte surface. A voltage of 370-390V is applied between the anode and cathode, generating a plasma micro-arc region on the surface of the copper rod. This arc region covers the lower end face of the cathode and extends downwards into the electrolyte. The carbon fiber moves in the electrolyte at a speed of 2-4 cm / s and continuously passes under the cathode, thus achieving the deposition of the Fe2O3-doped carbon coating on the carbon fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for rapidly depositing Fe2O3-doped carbon coatings on carbon fibers, belonging to the field of carbon fiber surface modification technology. Background Technology

[0002] Carbon / carbon (C / C) composites are widely used in high-end fields such as aerospace thermal structural components, engine blades, and throat liners due to their excellent high-temperature mechanical properties, high specific strength, and low density. As the main reinforcement in C / C composites, carbon fiber's interfacial properties directly determine the overall mechanical properties and oxidation resistance of the composite material.

[0003] To improve the interfacial bonding performance between carbon fibers and the matrix, researchers have developed various surface modification techniques, including sol-gel methods, chemical vapor deposition (CVD), and hydrothermal methods. Among these, cathodic plasma electrolytic deposition (CPED) technology has attracted widespread attention in recent years due to its advantages such as simple equipment, convenient operation, high deposition efficiency, and the ability to be performed at room temperature. Existing studies have shown that depositing Al2O3, Cr-C, and other coatings on the surface of carbon fibers using CPED technology can significantly improve their oxidation resistance.

[0004] However, existing methods for depositing metal oxide-doped carbon coatings on carbon fiber surfaces often struggle to achieve uniformly distributed and morphologically controllable network structures. Furthermore, conventional carbon sources (such as glucose) are difficult to carbonize rapidly at low temperatures, lacking effective catalytic mechanisms, resulting in low deposition rates and low carbonization efficiency. Therefore, how to rapidly deposit uniform, functional metal oxide-doped carbon coatings on carbon fibers using plasma electrolysis technology without damaging the fibers, and how to improve the interfacial bonding between the carbon fibers and the subsequent resin matrix, has become a pressing technical problem. Summary of the Invention

[0005] In view of this, the object of the present invention is to provide a method for rapidly depositing Fe2O3-doped carbon coatings on carbon fibers.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] A method for rapidly depositing Fe2O3-doped carbon coatings on carbon fibers, the method comprising the following steps:

[0008] (1) Prepare a mixed aqueous solution containing organic carbon source and iron salt; (2) Using the mixed aqueous solution as the electrolyte, a graphite plate as the anode and a copper rod as the cathode, the copper rod is located above the electrolyte and its lower end face is close to the electrolyte surface. A voltage of 370~390V is applied between the anode and cathode to generate a plasma micro-arc region on the surface of the copper rod. The arc region covers the lower end face of the cathode and extends downward into the electrolyte. The carbon fiber moves in the electrolyte at a speed of 2~4cm / s and continuously passes under the cathode, thereby achieving the deposition of Fe2O3 doped carbon coating on the carbon fiber.

[0009] Preferably, in step (1), the carbon source is glucose.

[0010] Preferably, in step (1), the iron salt is FeCl3·6H2O.

[0011] Preferably, in step (1), the concentration of the organic carbon source in the mixed aqueous solution is 8~12wt%.

[0012] Preferably, in step (1), the concentration of iron salt in the mixed aqueous solution is 12~15 g / L.

[0013] Preferably, in step (2), the diameter of the carbon fiber is 2~10μm.

[0014] Preferably, in step (2), the diameter of the copper rod is 20~40mm.

[0015] Preferably, in step (2), when the carbon fiber passes under the cathode, the vertical distance between the carbon fiber and the center of the lower end face of the copper rod is 8~12mm.

[0016] A carbon fiber with a deposited Fe2O3-doped carbon coating was prepared by the above method.

[0017] Preferably, the carbon coating is distributed in a mesh pattern, with Fe2O3 embedded in the carbon coating.

[0018] Beneficial effects This invention solves the problem of thermal damage to carbon fibers through "non-electrode mobile deposition"; it solves the problem of low carbonization efficiency and slow deposition rate of organic carbon sources (such as glucose) through "in-situ generation of catalytic Fe2O3 from iron salts"; it solves the problem of coating uniformity and morphology controllability through "coordinated control of voltage and mobile speed"; and it significantly improves the interfacial shear strength between carbon fibers and resin matrix through the comprehensive mechanism of "composite morphology of cauliflower-like particles + network carbon" and "mechanical interlocking + interface wetting regulation + graphitization induction". Attached Figure Description

[0019] Figure 1 This is a schematic diagram of the device structure used in the method described in this invention.

[0020] Figure 2This is a surface morphology diagram of the modified carbon fiber in Example 1.

[0021] Figure 3 XPS spectra of the modified carbon fiber in Example 1: (a) full XPS spectrum; (b) peaks of the fine carbon spectrum; (c) fine iron spectrum.

[0022] Figure 4 This is a comparison diagram of the interfacial shear properties of carbon fiber before and after modification in Example 1.

[0023] Figure 5 Comparison of pyrolysis components before and after carbon fiber modification in Example 1: (a) Comparison of Raman spectroscopy results; (b) Comparison of XPS results; (c) C1s peak diagram of pyrolysis carbon on the surface of unmodified carbon fiber; (d) C1s peak diagram of pyrolysis carbon on the surface of modified carbon fiber. Detailed Implementation

[0024] The present invention will be further described in detail below with reference to specific embodiments.

[0025] like Figure 1 As shown, a method for rapidly depositing an Fe2O3-doped carbon coating on carbon fibers includes the following steps: (1) Prepare a mixed aqueous solution containing organic carbon source and iron salt; (2) Using the mixed aqueous solution as the electrolyte, a graphite plate as the anode and a copper rod as the cathode, the copper rod is located above the electrolyte and its lower end face is close to the electrolyte surface. A voltage of 370~390V is applied between the anode and cathode to generate a plasma micro-arc region on the surface of the copper rod. The arc region covers the lower end face of the cathode and extends downward into the electrolyte. The carbon fiber moves in the electrolyte at a speed of 2~4cm / s and continuously passes under the cathode, thereby achieving the deposition of Fe2O3 doped carbon coating on the carbon fiber.

[0026] In some embodiments, in step (1), the carbon source is glucose.

[0027] In some embodiments, in step (1), the iron salt is FeCl3·6H2O.

[0028] In some embodiments, in step (1), the concentration of the organic carbon source in the mixed aqueous solution is 8-12 wt%, and the concentration of the iron salt is 12-15 g / L.

[0029] In some embodiments, in step (2), the diameter of the carbon fiber is 2~10μm.

[0030] In some embodiments, in step (2), the diameter of the copper rod is 20~40mm.

[0031] In some embodiments, in step (2), when the carbon fiber passes under the cathode, the vertical distance between the carbon fiber and the center of the lower end face of the copper rod is 8~12mm.

[0032] Example 1 (1) Prepare a mixed aqueous solution containing a carbon source and a metal salt, wherein the carbon source is glucose with a concentration of 10 wt%; the metal salt is FeCl3·6H2O with a concentration of 13 g / L. The acidity of the electrolyte is adjusted by the hydrogen ions generated by the hydrolysis of the iron salt, and no additional acid is required.

[0033] (2) such as Figure 1 As shown, a graphite plate serves as the anode; a copper rod (30 mm in diameter) acting as the cathode is placed above the electrolyte, close to the liquid surface. An external power supply is turned on, and the voltage is adjusted to 380V, creating a plasma arc region on the surface of the copper rod. This arc region covers the lower end face of the cathode and extends downwards into the electrolyte. An external motor is activated, driving a roller to move the T800 carbon fiber (HF40S, 12K, 5 μm in diameter) wound on the roller. A limiting device ensures the carbon fiber accurately passes through the plasma arc region (the vertical distance between the carbon fiber and the center of the lower end face of the copper rod is 10 mm), with a moving speed of 2.8 cm / s, achieving the deposition of an Fe2O3-doped carbon coating on the carbon fiber. This non-electrode plasma electrolysis deposition method allows the carbon fiber to pass continuously through the plasma electrolysis zone. The carbon fiber does not directly act as the cathode but moves through the plasma arc region, thus avoiding direct damage to the carbon fiber from the high-temperature plasma.

[0034] from Figure 2 It can be seen that the method successfully deposited a carbon coating on the surface of carbon fiber. The prepared carbon coating consists of a network of carbon layers and embedded microparticles.

[0035] from Figure 3 (a) It can be seen that the deposited carbon coating is doped with iron. Figure 3 (b) This indicates that the carbon in the coating is mainly bonded by carbon-carbon single bonds and partially by carbon-carbon double bonds, further proving the presence of Fe2O3 in the coating. Figure 3 (c) Prove that the iron in the coating exists in the form of Fe2O3.

[0036] Micro-debonding tests were conducted on carbon fibers before and after modification using phenolic resin, and the interfacial shear properties were obtained as follows: Figure 4 As shown, the average interfacial shear strength of the modified carbon fiber increased by 40 MPa.

[0037] A layer of phenolic resin was cured on the surface of carbon fiber and then pyrolyzed to obtain a carbon fiber sample containing pyrolyzed carbon. The effect of the coating on the pyrolysis of phenolic resin was studied. Figure 5(a) This demonstrates that the presence of the coating promotes the ordered transformation of the phenolic resin after pyrolysis; Figure 5 (c) and Figure 5 (d) The comparison shows that the presence of the coating increases the carbon-carbon double bond content in the cracked carbon, which is consistent with... Figure 5 The result of (a) is consistent.

[0038] The results above demonstrate that this method can successfully and rapidly prepare Fe2O3-doped carbon coatings on the surface of carbon fibers, thereby improving the interfacial shear strength of the carbon fibers. Furthermore, the presence of the coating also induces a more ordered transformation of the pyrolysis products of phenolic resin.

[0039] In summary, the invention includes, but is not limited to, the above embodiments. Any equivalent substitutions or partial improvements made under the spirit and principles of this invention shall be considered to be within the protection scope of this invention.

Claims

1. A method for rapid deposition of Fe203-doped carbon coating on carbon fibers, characterized by: The method steps include: (1) Prepare a mixed aqueous solution containing organic carbon source and iron salt; (2) Using the mixed aqueous solution as the electrolyte, a graphite plate as the anode and a copper rod as the cathode, the copper rod is located above the electrolyte and its lower end face is close to the electrolyte surface. A voltage of 370~390V is applied between the anode and cathode to generate a plasma micro-arc region on the surface of the copper rod. The arc region covers the lower end face of the cathode and extends downward into the electrolyte. The carbon fiber moves in the electrolyte at a speed of 2~4cm / s and continuously passes under the cathode, thereby achieving the deposition of Fe2O3 doped carbon coating on the carbon fiber.

2. A method for rapid deposition of Fe203 doped carbon coating on carbon fiber as claimed in claim 1 wherein: In step (1), the carbon source is glucose.

3. A method for rapid deposition of Fe203 doped carbon coating on carbon fiber as claimed in claim 1 wherein: In step (1), the iron salt is FeCl3·6H2O.

4. The method for rapidly depositing an Fe2O3-doped carbon coating on carbon fibers as described in claim 1, characterized in that: In step (1), the concentration of the organic carbon source in the mixed aqueous solution is 8~12wt%.

5. The method for rapidly depositing an Fe2O3-doped carbon coating on carbon fibers as described in claim 1, characterized in that: In step (1), the concentration of iron salt is 12~15 g / L.

6. The method for rapidly depositing an Fe2O3-doped carbon coating on carbon fibers as described in claim 1, characterized in that: In step (2), the diameter of the carbon fiber is 2~10μm.

7. The method for rapidly depositing an Fe2O3-doped carbon coating on carbon fibers as described in claim 1, characterized in that: In step (2), the diameter of the copper rod is 20~40mm.

8. The method for rapidly depositing an Fe2O3-doped carbon coating on carbon fibers as described in claim 1, characterized in that: In step (2), when the carbon fiber passes under the cathode, the vertical distance between the carbon fiber and the center of the lower end face of the copper rod is 8~12mm.

9. A carbon fiber with a deposited Fe2O3-doped carbon coating, characterized in that: It is prepared by the method described in any one of claims 1 to 7.

10. The carbon fiber with a deposited Fe2O3-doped carbon coating as described in claim 9, characterized in that: The carbon coating is distributed in a mesh pattern, with Fe2O3 embedded in the carbon coating.