A hydroxide composite plating electrode for use as an oxygen anode in alkaline water electrolysis, its preparation method and application
By preparing a hydroxide/nickel composite coating on an alkaline water electrolytic oxygen anode, the problems of insufficient coating-substrate bonding strength and catalytic activity were solved, achieving highly efficient electrocatalytic performance and a sustainable production method.
Patent Information
- Application Number
- CN202611621066.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing alkaline water electrolytic oxygen anodes are difficult to balance the bonding strength between the coating and the substrate and the catalytic activity of the electrode. They also have high production costs. Traditional preparation methods result in easy pulverization of the catalyst layer and dissolution of elements, making the plating solution unusable and putting great pressure on the environment.
The preparation method of hydroxide composite plating electrode involves introducing hydroxide slurry and metal salt into the composite plating solution, and forming a hydroxide/nickel composite plating layer on the surface of a conductive substrate by DC electroplating. The hydroxide particles are tightly coated and mechanically fixed by the nickel substrate, achieving metallurgical bonding between the plating layer and the substrate. The problem of plating solution waste is solved by recycling the plating solution.
It significantly improves the bonding strength between the coating and the substrate, provides abundant catalytic active sites, reduces the oxygen evolution overpotential, exhibits excellent electrocatalytic activity and reaction kinetics, and at the same time reduces production costs, meeting the requirements of green manufacturing.
Smart Images

Figure CN123108703A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of water electrolysis hydrogen production technology, and particularly relates to a hydroxide composite plating electrode for alkaline water electrolysis oxygen anode, its preparation method and application. Background Technology
[0002] Electrolysis of water to produce hydrogen is a key technological path for achieving large-scale storage and consumption of renewable energy and building a green hydrogen industry chain. Among these technologies, anion exchange membrane electrolysis (AEMWE) combines the advantages of alkaline water electrolysis (AWE)—its tolerance to non-precious metal catalysts and low system cost—with the high current density and fast dynamic response of proton exchange membrane electrolysis (PEM), making it a significant development direction for low-cost water electrolysis to produce hydrogen. The oxygen evolution reaction (OER) at the anolyte involves a multi-electron transfer process with slow kinetics, making it a critical factor limiting the overall energy conversion efficiency of water electrolysis. Especially under industrial conditions of high current density and long-term operation, developing highly active and stable non-precious metal OER anodes is crucial. Nickel-iron layered double hydroxides (NiFe-LDH) and their derivatives are widely considered among the most promising non-precious metal OER catalyst materials due to their layered structure, large specific surface area, abundant active sites, excellent catalytic activity in alkaline media, and low cost.
[0003] Currently, the main methods for preparing NiFe-LDH-based oxygen evolution anodes include hydrothermal methods, co-precipitation methods, and conventional electrodeposition methods. Hydrothermal and co-precipitation methods typically require the introduction of binders or physical adhesion to load the catalyst onto conductive substrates such as nickel mesh or nickel foam, resulting in weak bonding between the resulting catalyst layer and the substrate. While conventional electrodeposition methods can grow coatings in situ, the homogeneous coating exhibits lattice mismatch and internal stress concentration with the substrate. Under harsh operating conditions such as high temperature, high alkali concentration, high current density, and severe oxygen evolution bubble impact, the catalyst layer is prone to pulverization, elemental dissolution, or complete peeling, leading to rapid performance degradation of the electrolytic cell and failing to meet the lifespan requirements of tens of thousands of hours for industrial-scale stacks. Furthermore, the metal ions in the hydrothermal mother liquor, precipitation mother liquor, or electroplating solution from these methods are often discharged as waste after each batch and cannot be reused. This not only results in significant waste of raw materials such as nickel salts and increased production costs but also introduces environmental problems related to heavy metal wastewater treatment, failing to meet the requirements of green manufacturing and sustainable development. Composite electroplating technology, as a surface engineering method to achieve the co-deposition of metal and solid microparticles, can theoretically improve the adhesion between the catalytic layer and the substrate and enable long-term use of the plating solution through continuous replenishment. However, when applied to the preparation of hydroxide catalytic electrodes, it faces challenges such as the easy reduction of hydroxide microparticles by the cathode during the co-deposition process, which destroys the layered structure and leads to loss of catalytic activity; and the irreversible hard agglomeration of nano-hydroxide powder during drying pretreatment, making it difficult to disperse uniformly in the plating solution and affecting the batch consistency of the coating. Based on this, the present invention provides a hydroxide composite plating electrode for alkaline water electrolytic oxygen anodes, its preparation method, and its application, to solve the problems of existing alkaline water electrolytic oxygen anodes, which struggle to balance the adhesion strength between the coating and the substrate, as well as the electrode catalytic activity and high production costs. Summary of the Invention
[0004] The main objective of this invention is to provide a hydroxide composite plating electrode for alkaline water electrolytic oxygen anode, its preparation method, and its application, aiming to solve the technical problems of existing alkaline water electrolytic oxygen anodes, which are difficult to balance the bonding strength between the plating layer and the substrate and the catalytic activity of the electrode, as well as the high production cost.
[0005] To achieve the above objectives, the present invention provides a method for preparing a hydroxide composite plating electrode for an alkaline water electrolytic oxygen anode, comprising the following steps: S1: Provide a hydroxide slurry, the hydroxide slurry including one of NiFe-LDH slurry and Fe(OH)3 slurry; the solid content is 10~30% based on the total mass of the hydroxide slurry.
[0006] S2: Prepare a composite plating solution, wherein the composite plating solution comprises nickel main salt, boric acid, nickel chloride, nickel nitrate, ferric nitrate and the hydroxide slurry; based on the total volume of the composite plating solution, the concentration of nickel nitrate is 2~6 g / L, the concentration of ferric nitrate is 1~3 g / L, and the hydroxide solid content introduced by the hydroxide slurry is 0.5~2 g / L.
[0007] S3: Using the pretreated conductive substrate as the cathode and the nickel plate as the anode, the substrate is placed in the composite plating solution and composite electroplating deposition is performed using a DC power supply to form a hydroxide / nickel composite plating layer on the surface of the pretreated conductive substrate, thus obtaining the hydroxide composite plating electrode for alkaline water electrolytic oxygen anode.
[0008] The hydroxide / nickel composite coating is a composite coating of hydroxide and pure nickel formed by a pure nickel phase encapsulating a hydroxide phase.
[0009] According to an embodiment of the present invention, the NiFe-LDH slurry is prepared by hydrothermal synthesis.
[0010] The method for preparing the NiFe-LDH slurry includes: Nickel nitrate and iron nitrate were weighed according to a Ni:Fe molar ratio of 2:1 to 4:1, with a total molar amount of 0.9 mmol. 6 mmol CO(NH2)2, 2.2 mmol NH4F and 20 mL water were added, and the mixture was reacted at 100 to 140 °C for 6 to 24 h. After the reaction was completed, the mixture was centrifuged, washed, and concentrated to a solid content of 10 to 30%, without drying.
[0011] According to an embodiment of the present invention, the Fe(OH)3 slurry is prepared by electroplating.
[0012] The method for preparing the Fe(OH)3 slurry includes: Using an iron plate as the anode and a nickel or stainless steel plate as the cathode, a constant current density of 20–200 mA / cm² was applied in an electrolyte solution containing 8–25 mmol Fe(NO₃)₃·9H₂O and 0.2–1 mmol NaNO₃. 2 Electrolyze for 30-300 seconds, stirring during the process. After electrolysis, allow to stand, centrifuge, wash, and concentrate to a solid content of 10-30%, without drying.
[0013] According to an embodiment of the present invention, the nickel main salt comprises nickel aminosulfonate.
[0014] Based on the total volume of the composite plating solution, the composite plating solution comprises: nickel aminosulfonate (Ni(SO3NH2)2·4H2O) at 300~400 g / L, boric acid at 20~40 g / L, nickel chloride at 5~15 g / L, nickel nitrate at 2~6 g / L, and ferric nitrate at 1~3 g / L.
[0015] According to an embodiment of the present invention, the nickel main salt comprises nickel sulfate.
[0016] Based on the total volume of the composite plating solution, the composite plating solution comprises: 300-400 g / L nickel sulfate (NiSO4·6H2O), 30-40 g / L boric acid, 5-15 g / L nickel chloride, 2-6 g / L nickel nitrate, and 1-3 g / L ferric nitrate.
[0017] According to an embodiment of the present invention, the temperature of the composite plating solution is 20~60°C.
[0018] The parameters for the composite electroplating deposition include: an electrode spacing of 10-20 cm, a stirring speed of 200-400 rpm, and a current density of 3-15 A / dm³. 2 The electroplating time is 10~40 minutes.
[0019] This invention provides a hydroxide composite plating electrode for alkaline water electrolytic oxygen anode, which is prepared according to the above-described preparation method for the hydroxide composite plating electrode for alkaline water electrolytic oxygen anode.
[0020] According to an embodiment of the present invention, the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode includes a conductive substrate and a hydroxide / nickel composite plating layer formed on the surface of the conductive substrate.
[0021] In the composite coating, metallic nickel is a continuous phase, hydroxide particles are a discrete phase, and the hydroxide particles are encapsulated and / or anchored inside the metallic nickel matrix.
[0022] The hydroxide includes one of NiFe-LDH and Fe(OH)3.
[0023] According to an embodiment of the present invention, the pretreatment step includes degreasing and acid washing activation.
[0024] The conductive substrate includes one of nickel mesh and nickel foam.
[0025] The Fe element mass fraction in the composite coating is 0.5~1.5%.
[0026] The present invention also provides an electrode prepared by the above-mentioned method for preparing a hydroxide composite plating electrode for alkaline water electrolysis oxygen anode, or the application of the above-mentioned hydroxide composite plating electrode for alkaline water electrolysis oxygen anode in alkaline water electrolysis hydrogen production, wherein alkaline water electrolysis includes one of alkaline water electrolysis (ALK) and anion exchange membrane water electrolysis (AEM).
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: The aforementioned hydroxide composite plating electrode, preparation method, and application for alkaline water electrolytic oxygen anodes utilize a method that directly disperses hydroxide slurry in a composite plating solution. The synthesized hydroxide slurry is then simply washed and concentrated before being added directly to the composite plating solution, completely eliminating the need for drying and grinding processes. This fundamentally avoids the agglomeration problem of hydroxide powder during drying and ensures good dispersion of hydroxide particles in the plating solution. Furthermore, the plating solution can be reused simply by adding hydroxide slurry and necessary metal salts, fundamentally solving the problem of difficult reuse of plating solutions / slurries in traditional electroplating. This one-step composite electroplating method can deposit hydrogen on the surface of a conductive substrate. In the oxide / nickel composite coating process, hydroxide particles are in situ embedded in the growing metallic nickel coating as nickel ions are reduced, forming a particle-reinforced composite coating structure. The hydroxide particles are tightly coated and mechanically fixed by the nickel substrate, which significantly improves the bonding strength between the coating and the conductive substrate. This effectively avoids the problems of easy detachment and peeling of traditional coating and bonding methods, as well as catalyst layers prepared by in-situ growth relying on van der Waals forces and a small number of ionic bonds, under high current density oxygen evolution conditions. At the same time, the continuous and dense nickel coating, as a conductive network and structural support phase, effectively compensates for the low intrinsic conductivity of hydroxide and promotes the rapid transport of charge between the catalytic active sites and the substrate. Furthermore, by synergistically introducing nickel nitrate, iron nitrate, and hydroxide slurry into the composite plating solution, Ni and Fe elements are co-deposited and uniformly distributed in the composite coating during the electroplating process. The resulting hydroxide / nickel composite coating is rich in NiFe-LDH and / or Fe(OH)3 highly active catalytic phases, providing abundant alkaline oxygen evolution reaction active sites, significantly reducing the oxygen evolution overpotential, and exhibiting excellent electrocatalytic activity and reaction kinetics.
[0028] Moreover, the raw materials of this invention are all inexpensive and readily available conventional chemical reagents, the preparation method is simple, the operation is convenient and controllable, it is easy to scale up production, and it has good prospects for industrial application. Attached Figure Description
[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.
[0030] Figure 1 This is a SEM image of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 1 of the present invention. Figure 2 EDS image of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 1; Figure 3 The figure shows the voltage change curves of the hydroxide composite plating electrode prepared in Examples 1-4 for use as an oxygen anode in alkaline water electrolysis, which was continuously operated for 270 hours under constant current conditions in an alkaline electrolytic cell. Figure 4 This is a SEM image of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 2. Figure 5 This is a SEM image of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 3. Figure 6 This is a SEM image of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 4. Figure 7 SEM image of the electrode prepared in Comparative Example 1 for use as an oxygen anode in alkaline water electrolysis. Figure 8 The figure shows the voltage change curves of the small chamber of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 1, and the electrodes for alkaline water electrolysis oxygen anode prepared in Comparative Examples 1 and 3-5, which were continuously operated under constant current conditions in an alkaline electrolytic cell for 270 h. Figure 9 SEM image of the electrode prepared in Comparative Example 3 for use as an oxygen anode in alkaline water electrolysis. Figure 10 SEM image of the electrode prepared in Comparative Example 4 for use as an oxygen anode in alkaline water electrolysis. Figure 11 This is a SEM image of the electrode prepared in Comparative Example 5 for use as an oxygen anode in alkaline water electrolysis.
[0031] The realization of the objective, functional characteristics and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0033] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.
[0034] The applicant discovered that current methods for preparing NiFe-LDH-based oxygen evolution anodes mainly include hydrothermal methods, co-precipitation methods, and conventional electrodeposition methods. These methods have the following serious drawbacks in practical industrial applications (especially for the high-current, long-term operation conditions of ALK / AEM electrolyzers): (1) Poor adhesion between the catalyst and the conductive substrate (nickel mesh / nickel foam). Catalysts prepared by hydrothermal and co-precipitation methods rely on binders or simple physical adhesion, while the uniform composition coating prepared by conventional constant current electrodeposition method has significant lattice mismatch and internal stress concentration with the nickel mesh substrate. In actual operation of alkaline electrolytic cells (high temperature >60℃, high concentration of alkaline solution, and severe oxygen bubble impact under high current density), the catalyst layer is prone to pulverization, element dissolution, and overall peeling, resulting in a sharp decline in the performance of the electrolytic cell, which is far from meeting the life requirements of tens of thousands of hours for industrial ALK / AEM stacks.
[0035] (2) The prepared solution is used only once, resulting in serious waste of raw materials and significant environmental pressure. The reaction mother liquor used in hydrothermal and coprecipitation methods contains a large number of unreacted metal ions and excess precipitates, which are discharged as waste liquid after each batch of reaction and cannot be directly reused. This not only significantly increases the cost of raw materials (especially nickel salts), but also brings huge environmental pressure to the treatment of heavy metal waste liquid, which does not meet the requirements of green manufacturing and sustainable development.
[0036] To address the aforementioned issues of poor adhesion and raw material waste, composite electroplating technology offers a potential solution. Composite electroplating is a process that uses electrodeposition to co-deposit metal and solid particles onto the cathode surface. If NiFe-LDH hydroxide powders can be used as solid particles and co-deposited with metallic nickel on a nickel mesh substrate, a "metal-anchored hydroxide" composite plating structure can theoretically be formed. Since metallic nickel and the nickel mesh substrate are homogeneous materials, metallurgical-grade bonding can be achieved, fundamentally solving the adhesion problem. Simultaneously, the electroplating solution can be recycled and replenished for long-term use, eliminating the problem of one-time waste.
[0037] However, directly applying composite electroplating technology to the preparation of hydroxide catalytic electrodes faces the following unique technical obstacle: hydroxides are easily electrochemically reduced in conventional composite electroplating, leading to the loss of catalytic activity. This is the core bottleneck limiting the application of composite electroplating technology to hydroxide systems. In conventional nickel plating processes, when hydroxide particles such as NiFe-LDH are transported to the cathode surface, the Ni in the particles... 2+ and Fe 3+ Under strong reducing conditions, hydroxides are readily reduced directly to their metallic state. Once reduced, the active phase for hydrogen evolution transforms into the inactive phase, resulting in slow oxygen evolution kinetics. Simultaneously, the loss of specific surface area leads to a significant reduction in active sites, drastically decreasing the electrode's OER catalytic activity. Furthermore, hydroxide powders are prone to hard agglomeration during drying, making subsequent dispersion difficult. Traditional composite electroplating processes typically require pretreatment steps such as drying, grinding, and sieving for solid microparticles. However, for nanoscale hydroxide powders, the strong capillary forces during drying cause irreversible hard agglomeration between particles, forming micron-sized or even larger agglomerates. These agglomerates are difficult to redisperse into original nanoparticles in the plating solution, leading to uneven particle distribution and unstable deposition in the composite coating, severely impacting batch-to-batch consistency of the coating quality.
[0038] Based on this, the present invention provides a hydroxide composite plating electrode for alkaline water electrolytic oxygen anode, its preparation method and application, aiming to solve the technical problems of existing alkaline water electrolytic oxygen anodes, which are difficult to balance the bonding strength between the coating and the substrate and the catalytic activity of the electrode, and have high production costs.
[0039] To achieve the above objectives, the present invention provides a method for preparing a hydroxide composite plating electrode for an alkaline water electrolytic oxygen anode, comprising the following steps: S1: Provide a hydroxide slurry, the hydroxide slurry including one of NiFe-LDH slurry and Fe(OH)3 slurry; the solid content is 10~30% based on the total mass of the hydroxide slurry.
[0040] S2: Prepare a composite plating solution, wherein the composite plating solution comprises nickel main salt, boric acid, nickel chloride, nickel nitrate, ferric nitrate and the hydroxide slurry; based on the total volume of the composite plating solution, the concentration of nickel nitrate is 2~6 g / L, the concentration of ferric nitrate is 1~3 g / L, and the hydroxide solid content introduced by the hydroxide slurry is 0.5~2 g / L.
[0041] S3: Using the pretreated conductive substrate as the cathode and the nickel plate as the anode, the substrate is placed in the composite plating solution and composite electroplating deposition is performed using a DC power supply to form a hydroxide / nickel composite plating layer on the surface of the pretreated conductive substrate, thus obtaining the hydroxide composite plating electrode for alkaline water electrolytic oxygen anode.
[0042] The hydroxide / nickel composite coating is a composite coating of hydroxide and pure nickel formed by a pure nickel phase encapsulating a hydroxide phase.
[0043] In some embodiments, metallic nickel and various hydroxide powders are co-deposited on the surface of a conductive substrate by DC electroplating to form a multi-component hydroxide / nickel composite coating.
[0044] In some embodiments, in step S3, Ni in the composite plating solution 2+ On the cathode surface, the hydroxide is reduced to metallic nickel. Simultaneously, the hydroxide powder suspended in the plating bath is transported to the cathode surface under stirring and electromigration, where it is encapsulated by the deposited metallic nickel lattice and embedded in the coating, forming a composite coating in which hydroxide is uniformly distributed in the metallic nickel substrate. After electroplating, the electrode is removed, rinsed with deionized water, and vacuum dried at 60~80℃.
[0045] The aforementioned method for preparing a hydroxide composite plating electrode for an alkaline water electrolytic oxygen anode involves directly dispersing a hydroxide slurry in a composite plating solution. The synthesized hydroxide slurry is then simply washed and concentrated before being added directly to the composite plating solution, completely eliminating the need for drying and grinding processes. This fundamentally avoids the agglomeration problem of hydroxide powder during drying and ensures good dispersion of hydroxide particles in the plating solution. Furthermore, the plating solution can be reused simply by adding hydroxide slurry and necessary metal salts, fundamentally solving the problem of difficult reuse of plating solutions / slurries in traditional electroplating. This one-step composite electroplating method can deposit hydroxide slurry on the surface of a conductive substrate. In the DC electroplating process, hydroxide / nickel composite coatings involve hydroxide particles being in situ embedded in the growing metallic nickel coating as nickel ions are reduced, forming a particle-reinforced composite coating structure. The hydroxide particles are tightly encapsulated and mechanically fixed by the nickel substrate, significantly improving the bonding strength between the coating and the conductive substrate. This effectively avoids the problems of easy detachment and peeling of traditional coating and bonding methods, as well as catalyst layers prepared by in-situ growth relying on van der Waals forces and a small number of ionic bonds, under high current density oxygen evolution conditions. At the same time, the continuous and dense nickel coating, as a conductive network and structural support phase, effectively compensates for the low intrinsic conductivity of hydroxides, promoting rapid charge transport between the catalytic active sites and the substrate. Furthermore, by synergistically introducing nickel nitrate, iron nitrate, and hydroxide slurry into the composite plating solution, Ni and Fe elements are co-deposited and uniformly distributed in the composite coating during the electroplating process. The resulting hydroxide / nickel composite coating is rich in NiFe-LDH and / or Fe(OH)3 highly active catalytic phases, providing abundant alkaline oxygen evolution reaction active sites, significantly reducing the oxygen evolution overpotential, and exhibiting excellent electrocatalytic activity and reaction kinetics.
[0046] In some embodiments, the present invention introduces nickel nitrate and ferric nitrate as "reduction inhibitors" to utilize free Ni 2+ and Fe 3+ The competitive adsorption and interfacial buffering at the cathode interface fundamentally suppress the electrochemical reduction of hydroxide powder during co-deposition, thus preserving its crystal structure and catalytic activity. Simultaneously, the hydroxide powder, after synthesis, is simply washed and concentrated into a wet slurry before being directly added to the plating bath, completely avoiding the drying process and the resulting hard agglomeration problems. Furthermore, a long-term recycling system for the plating bath enables its continuous reuse. Ultimately, this achieves a synergistic effect of high intrinsic catalytic activity, metallurgical-grade bonding strength, and recyclable plating bath under alkaline OER conditions.
[0047] The technical principles of this invention include: (1) Composite co-deposition and anchoring principle. Under a DC electric field, metallic nickel is continuously deposited and encapsulates and embeds the hydroxide particles that reach the cathode surface into the coating, forming a composite structure in which metallic nickel is the continuous phase and hydroxide is the discrete reinforcing phase. This structure achieves metallurgical-grade bonding with the conductive substrate (nickel mesh), and the hydroxide particles are firmly anchored.
[0048] (2) Wet dispersion principle. The surface of the solid powder in the freshly synthesized slurry has a large number of adsorbed water and hydroxyl functional groups. Under the combined effect of surface tension and electrostatic repulsion, the particles are not easy to agglomerate. After being added directly to the plating solution, a stable suspension system can be formed by stirring and sonication, ensuring that the powder is uniformly dispersed in the plating solution as nano- or submicron-sized particles.
[0049] (3) Hydroxide Reduction Inhibition Principle. In conventional composite electroplating, when hydroxide particles are transported to the cathode surface, due to the extremely negative cathode potential, the metal ions in the particles directly gain electrons and are reduced to a metallic state, leading to the destruction of the hydroxide structure and loss of catalytic activity. This invention introduces a large number of nitrate ions by adding nickel nitrate and iron nitrate to the plating solution. During the electroplating process, nitrate undergoes a reduction reaction on the cathode surface, and its electrochemical behavior plays the following synergistic inhibitory role: Nitrate can undergo a reduction reaction (NO3) on the cathode surface. - + H2O + 2e - → NO2 - + 2OH - This reaction consumes some electron flow at the cathode interface, reducing the effective current density and local overpotential acting on the surface of the hydroxide particles. Simultaneously, NO3... - The reduction product (NO2) - ) and the released OH - An adsorption or diffusion layer is formed on the cathode surface, which physically and chemically blocks the direct injection of electrons into the internal lattice of the hydroxide particles. This also helps maintain the stability of the hydroxide in the alkaline microenvironment. Furthermore, it neutralizes the slight acid erosion caused by the acidity of the plating bath on the hydroxide surface, allowing the Fe in the particles to... 3+ It is difficult for it to gain electrons and be reduced. This makes the hydroxide powder mainly encapsulated and embedded in the nickel matrix in the form of "inert particles".
[0050] In some embodiments, the NiFe-LDH slurry is prepared by hydrothermal synthesis.
[0051] The method for preparing the NiFe-LDH slurry includes: Nickel nitrate and iron nitrate were weighed according to a Ni:Fe molar ratio of 2:1 to 4:1, with a total molar amount of 0.9 mmol. 6 mmol CO(NH2)2, 2.2 mmol NH4F and 20 mL water were added, and the mixture was reacted at 100 to 140 °C for 6 to 24 h. After the reaction was completed, the mixture was centrifuged, washed, and concentrated to a solid content of 10 to 30%, without drying.
[0052] In some embodiments, the reaction is carried out in a hydrothermal reactor at 100-140°C for 6-24 hours. After the reaction, the product is centrifuged and washed repeatedly with deionized water 3-5 times to remove unreacted ions and byproducts. The washed NiFe-LDH precipitate is not dried but directly concentrated to a wet slurry with a solid content of 10-30 wt% for later use.
[0053] In some embodiments, the Fe(OH)3 slurry is prepared by electroplating.
[0054] The method for preparing the Fe(OH)3 slurry includes: Using an iron plate as the anode and a nickel or stainless steel plate as the cathode, a constant current density of 20–200 mA / cm² was applied in an electrolyte solution containing 8–25 mmol Fe(NO₃)₃·9H₂O and 0.2–1 mmol NaNO₃. 2 Electrolyze for 30-300 seconds, stirring during the process. After electrolysis, allow to stand, centrifuge, wash, and concentrate to a solid content of 10-30%, without drying.
[0055] In some embodiments, the method for preparing the Fe(OH)3 slurry includes: using an iron plate as the anode and a nickel plate or stainless steel plate as the cathode, in an electrolyte solution containing 10-20 mmol Fe(NO3)3·9H2O and 0.2-0.8 mmol NaNO3, using a constant current density of 45-55 mA / cm². 2 Electrolyze for 1-2 minutes, stirring during the process. After electrolysis, let stand, centrifuge, wash, and concentrate to a solid content of 10-30%, without drying.
[0056] In some embodiments, an iron plate (purity ≥99%) is used as the anode and a nickel plate or stainless steel plate is used as the cathode. During the electrolysis process of the Fe(OH)3 slurry preparation method, the anode iron dissolves to generate Fe. 2+ / Fe 3+ In the near-cathode region, it reacts with OH- produced by water electrolysis. - The reaction produces Fe(OH)3 precipitate. After electrolysis, the resulting suspension is allowed to stand, the supernatant is removed, and the suspension is repeatedly centrifuged and washed with deionized water 3-5 times. Finally, it is concentrated to a wet Fe(OH)3 slurry with a solid content of 10-30 wt% for later use.
[0057] In some embodiments, the nickel primary salt comprises nickel aminosulfonate.
[0058] Based on the total volume of the composite plating solution, the composite plating solution comprises: nickel aminosulfonate (Ni(SO3NH2)2·4H2O) at 300~400 g / L, boric acid at 20~40 g / L, nickel chloride at 5~15 g / L, nickel nitrate at 2~6 g / L, and ferric nitrate at 1~3 g / L.
[0059] In some embodiments, the nickel main salt includes nickel aminosulfonate. This composite plating solution is characterized by low internal stress in the coating and fast deposition rate, making it suitable for applications requiring high coating density and adhesion.
[0060] In some embodiments, the nickel primary salt comprises nickel sulfate.
[0061] Based on the total volume of the composite plating solution, the composite plating solution comprises: 300-400 g / L nickel sulfate (NiSO4·6H2O), 30-40 g / L boric acid, 5-15 g / L nickel chloride, 2-6 g / L nickel nitrate, and 1-3 g / L ferric nitrate.
[0062] In some embodiments, if the nitrate concentration in the composite plating solution is low, the hydroxide will be reduced. While a high concentration does not present obvious defects, it will significantly reduce the electroplating efficiency. Furthermore, if the hydroxide solid content is too high, it will be difficult to suspend, resulting in excessively fast settling and hindering composite electroplating.
[0063] In some embodiments, the temperature of the composite plating solution is 20~60°C.
[0064] The parameters for the composite electroplating deposition include: an electrode spacing of 10-20 cm, a stirring speed of 200-400 rpm, and a current density of 3-15 A / dm³. 2 The electroplating time is 10~40 minutes.
[0065] In some embodiments, during the composite electroplating deposition process, the continuous stirring speed keeps the hydroxide slurry suspended during the deposition process and prevents significant sedimentation within 1 minute after stirring stops. Stirring ensures that the particles in the plating solution are fully suspended, reducing agglomeration.
[0066] Moreover, the raw materials of this invention are all inexpensive and readily available conventional chemical reagents, the preparation method is simple, the operation is convenient and controllable, it is easy to scale up production, and it has good prospects for industrial application.
[0067] This invention provides a hydroxide composite plating electrode for alkaline water electrolytic oxygen anode, which is prepared according to the above-described preparation method for the hydroxide composite plating electrode for alkaline water electrolytic oxygen anode.
[0068] In some embodiments, the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode includes a conductive substrate and a hydroxide / nickel composite plating layer formed on the surface of the conductive substrate.
[0069] In the composite coating, metallic nickel is a continuous phase, hydroxide particles are a discrete phase, and the hydroxide particles are encapsulated and / or anchored inside the metallic nickel matrix.
[0070] The hydroxide includes one of NiFe-LDH and Fe(OH)3.
[0071] In some embodiments, the pretreatment step includes degreasing and acid washing activation.
[0072] The conductive substrate includes one of nickel mesh and nickel foam.
[0073] The Fe element mass fraction in the composite coating is 0.5~1.5%.
[0074] In some embodiments, nickel mesh or nickel foam is selected as the conductive substrate. Degreasing: Immerse the conductive substrate in a 30 wt% KOH solution at 60-80°C for 10-30 minutes, and then ultrasonically clean it with deionized water. Acid pickling and activation: Immerse the substrate in a 10-15 wt% hydrochloric acid or sulfuric acid solution at room temperature for 10-15 minutes, rinse thoroughly with deionized water, and then quickly transfer it to the electroplating tank.
[0075] The present invention also provides an electrode prepared by the above-mentioned method for preparing a hydroxide composite plating electrode for alkaline water electrolysis oxygen anode, or the application of the above-mentioned hydroxide composite plating electrode for alkaline water electrolysis oxygen anode in alkaline water electrolysis hydrogen production, wherein alkaline water electrolysis includes one of alkaline water electrolysis (ALK) and anion exchange membrane water electrolysis (AEM).
[0076] To further illustrate the present invention, the following examples are provided: It should be noted that the test methods in the embodiments and comparative examples of the present invention specifically include: Ultrasonic weight loss rate test data: The 4×4 cm electrode was placed in deionized water and sonicated for 30 min, dried and weighed, and the result was repeated 4 times and the average value was taken.
[0077] Three-electrode test: The electrolyte was a 6 mol / L KOH solution at 80℃, and the area of the working electrode was 2 × 2 cm². 2 The reference electrode was Hg / HgO, the counter electrode was a nickel sheet, and the recording speed was 500 mA / cm.2 Lower potential.
[0078] ALK electrolytic cell test: The electrolyte was a 30% KOH solution at 80℃, 5000 A / m 2 The changes in cell voltage and potential were recorded under constant current conditions for 270 hours.
[0079] Industrial pure water for deionized water. Potassium hydroxide (tablets), industrial grade, 90% purity, manufacturer: Hunan Huihong. Nickel sulfamate tetrahydrate, industrial grade, 99% purity, manufacturer: Jilin Jien. Boric acid, industrial grade, 99.9% purity, manufacturer: QUIBORAX. Nickel sulfate hexahydrate, electroplating grade, manufacturer: Jinchuan. Nickel chloride hexahydrate, 99% purity, manufacturer: Maclean's. Nickel nitrate hexahydrate, analytical grade, AR, Shanghai Testing. Ferric nitrate nonahydrate, 99.9%, Aladdin. Sodium chloride, 99%, Maclean's.
[0080] Example 1 A method for preparing a hydroxide composite plating electrode for use as an oxygen anode in alkaline water electrolysis includes the following steps: S1: Provide Fe(OH)3 slurry, prepared by using an iron plate as the anode and a stainless steel plate as the cathode in an electrolyte solution containing 15 mmol Fe(NO3)3·9H2O, 0.5 mmol NaNO3, and 20 mL deionized water, using a constant current density of 50 mA / cm². 2 Electrolyze for 2 minutes with vigorous stirring during the process. After electrolysis, let stand for 6 hours, remove the supernatant, and wash repeatedly with deionized water by centrifugation 5 times. Concentrate to a Fe(OH)3 slurry with a solid content of 20 wt%, without drying.
[0081] S2: Prepare the composite plating solution. Based on the total volume of the composite plating solution, add nickel sulfamate (Ni(SO3NH2)2·4H2O) at a concentration of 400 g / L, boric acid at a concentration of 30 g / L, and nickel chloride at a concentration of 10 g / L to deionized water, stirring until completely dissolved. Add nickel nitrate at a concentration of 5 g / L, ferric nitrate at a concentration of 2.5 g / L, and the aforementioned Fe(OH)3 slurry. The hydroxide solid content introduced by the Fe(OH)3 slurry is 2 g / L. The solution is mechanically stirred and ultrasonically dispersed until uniform. The resulting composite plating solution has a pH of 4.0 and is kept at room temperature.
[0082] S3: Take nickel foam (size 10×10 cm) as the conductive substrate, and perform degreasing in sequence (specifically, soak in 30% KOH solution at 70℃ for 15 min, ultrasonically wash with water, and then perform acid washing activation (specifically, soak in 10% hydrochloric acid solution at room temperature for 10 min, and rinse thoroughly with deionized water to obtain pretreated nickel foam).
[0083] Using pretreated nickel foam as the cathode and a nickel plate as the anode, with an electrode spacing of 10 cm, the plates were immersed in a composite plating solution at a stirring speed of 200 rpm. A DC power supply with a current density of 15 A / dm³ was used. 2 The electroplating time is 20 minutes. After electroplating, the electrode is removed, rinsed with deionized water, and then vacuum dried in a vacuum drying oven at 60℃ to obtain a hydroxide composite plating electrode for use as an alkaline water electrolysis oxygen anode.
[0084] See Figure 1 It can be seen that the composite coating of the hydroxide composite plating electrode for alkaline water electrolytic oxygen anode prepared in Example 1 is dense and uniform, with granular Fe(OH)3 uniformly distributed in the foamed nickel substrate. The coating is tightly bonded to the foamed nickel substrate and is free of cracks. See also Figure 2 EDS analysis confirmed that Fe was mainly distributed in the particles, demonstrating the successful co-deposition of Fe(OH)3 with a Fe mass fraction of 0.97%.
[0085] Testing showed that the hydroxide composite plating electrode prepared in Example 1 for use as an oxygen anode in alkaline water electrolysis exhibited an ultrasonic weight loss rate of 1.2%, demonstrating excellent coating adhesion; the vast majority of the coating remained firmly attached to the substrate after ultrasonic treatment. (500 mA / cm) 2 The potential was 0.51 V vs Hg / HgO. ALK stability testing showed that the hydroxide composite plating electrode prepared in Example 1 for alkaline water electrolytic oxygen anode plating increased the cell voltage by approximately 15 mV after 270 h. The steady-state cell voltage was 58 mV lower than that of domestically produced commercially available non-precious metal electrodes. (See [reference]). Figure 3 .
[0086] Example 2 Compared to Example 1, the hydroxide slurry was changed.
[0087] In Example 2, the hydroxide slurry was a NiFe-LDH slurry, prepared as follows: Nickel nitrate (specifically, 0.7 mmol Ni(NO3)2·6H2O) and ferric nitrate (specifically, 0.2 mmol Fe(NO3)3·9H2O) were weighed at a Ni:Fe molar ratio of 3.5:1, with a total molar amount of 0.9 mmol. 6 mmol CO(NH2)2, 2.2 mmol NH4F, and 20 mL deionized water were added, stirred to dissolve, and then transferred to a 100 mL hydrothermal reactor. The reaction was carried out at 120°C for 8 hours. After the reaction, the mixture was centrifuged and washed five times (using a cycle of water followed by ethanol for five cycles). After washing with water, the mixture was concentrated to a NiFe-LDH slurry with a solid content of 20 wt%, without drying. The remaining steps were the same as in Example 1, resulting in a hydroxide composite plating electrode for alkaline water electrolytic oxygen anode.
[0088] See Figure 4 It can be seen that the NiFe-LDH hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 2 is distributed in a spherical / clustered manner in the composite coating. Compared with the Fe(OH)3 particles in Example 1, there is a certain agglomeration phenomenon. However, the hydroxide particles are coated and / or anchored by the nickel matrix, and some active sites are exposed.
[0089] Testing showed that the ultrasonic weight loss rate of the hydroxide composite plating electrode prepared in Example 2 for use as an oxygen anode in alkaline water electrolysis was 3.1%, at 500 mA / cm². 2 The potential was 0.52 V vs Hg / HgO. ALK stability testing showed that the hydroxide composite plating electrode prepared in Example 2 for alkaline water electrolytic oxygen anode plating increased the cell voltage by approximately 18 mV after 270 h. The steady-state cell voltage was 54 mV lower than that of domestically produced commercially available non-precious metal electrodes. (See [reference]). Figure 3 .
[0090] Example 3 Compared to Example 1, the composition and temperature of the composite plating solution were changed.
[0091] In Example 3, based on the total volume of the composite plating solution, 400 g / L of nickel sulfate (NiSO4·6H2O), 35 g / L of boric acid, and 10 g / L of nickel chloride were added sequentially to deionized water and stirred until completely dissolved. Then, 5 g / L of nickel nitrate, 2.5 g / L of ferric nitrate, and the aforementioned Fe(OH)3 slurry were added. The hydroxide solid content introduced by the Fe(OH)3 slurry was 2 g / L. The mixture was mechanically stirred and ultrasonically dispersed until uniform. The resulting composite plating solution had a pH of 4.0 and a temperature of 50°C. The remaining steps were the same as in Example 1, thus obtaining a hydroxide composite plating electrode for alkaline water electrolytic oxygen anode.
[0092] See Figure 5 It can be seen that the coating of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 3 has certain cracks and high stress, but the particles are still tightly bonded to the coating.
[0093] Testing showed that the ultrasonic weight loss rate of the hydroxide composite plating electrode prepared in Example 3 for use as an oxygen anode in alkaline water electrolysis was 5.3%, and the ultrasonic weight loss rate was 500 mA / cm². 2 The potential was 0.54 V vs Hg / HgO. ALK stability testing showed that the hydroxide composite plating electrode prepared in Example 3 for alkaline water electrolytic oxygen anode plating increased the cell voltage by approximately 16 mV after 270 h. The steady-state cell voltage was 53 mV lower than that of domestically produced commercially available non-precious metal electrodes. (See [reference]). Figure 3 .
[0094] Example 4 Compared to Example 1, the conductive substrate was changed.
[0095] In Example 4, the conductive substrate was a nickel mesh with a purity ≥99.99%, 40 mesh, and a wire diameter of 0.19 mm. The remaining steps were the same as in Example 1, and a hydroxide composite plating electrode for alkaline water electrolysis oxygen anode was prepared.
[0096] See Figure 6 It can be seen that the granular Fe(OH)3 of the hydroxide composite plating electrode for alkaline water electrolysis oxygen anode prepared in Example 4 is uniformly distributed in the nickel mesh substrate, the plating layer is relatively tightly bonded to the nickel mesh, and there are a few cracks near Fe(OH)3.
[0097] Testing showed that the ultrasonic weight loss rate of the hydroxide composite plating electrode prepared in Example 4 for use as an oxygen anode in alkaline water electrolysis was 1.9%, and the ultrasonic weight loss rate was 500 mA / cm². 2 The potential was 0.54 V vs Hg / HgO. ALK stability testing showed that the hydroxide composite plating electrode prepared in Example 4 for alkaline water electrolytic oxygen anode plating increased the cell voltage by approximately 15 mV after 270 h. The steady-state cell voltage was 51 mV lower than that of domestically produced commercially available non-precious metal electrodes. (See [reference]). Figure 3 .
[0098] Additionally, see Figure 3 It can be seen that during the 270-hour test period, the voltage change trend of the small chamber of the hydroxide composite plating electrode prepared in Examples 1-4 for the oxygen evolution anode in alkaline water electrolysis is stable, and there is no phenomenon of continuous and rapid voltage rise. This indicates that the hydroxide composite plating electrode has excellent oxygen evolution catalytic activity under the constant current condition of alkaline water electrolysis, and also has good long-term operational stability.
[0099] Comparative Example 1 NiFe-LDH was grown in situ on nickel foam using a conventional hydrothermal method. Specifically, the nickel foam was vertically bent and immersed in a hydrothermal reaction solution with the same composition as in Example 2, then transferred to a 100 mL hydrothermal reactor and reacted at 120°C for 8 h. After the reaction, the nickel foam was removed, rinsed with deionized water, and dried in a vacuum drying oven at 60°C. The composite electroplating of Example 1 was not performed; the remaining steps were the same as in Example 1, thus obtaining an electrode for alkaline water electrolysis oxygen anode.
[0100] See Figure 7 It can be seen that, on the electrode prepared in Comparative Example 1 for the electrolytic oxygen anode in alkaline water, layered NiFe-LDH is uniformly grown on the surface of nickel foam; EDS test results show that the mass fraction of Fe element is 9.3%.
[0101] Testing showed that the ultrasonic weight loss rate of the electrode prepared in Comparative Example 1 for the electrolytic oxygen anode in alkaline water was 87%, and a large amount of lamellar NiFe-LDH on the surface of the nickel foam peeled off after ultrasonication; 500 mA / cm 2 The potential is 0.50 V vs Hg / HgO. See also Figure 8 The ALK stability test showed that the electrode prepared in Comparative Example 1 for the electrolytic oxygen anode in alkaline water showed a rise in chamber voltage of about 144 mV after 270 hours of stability testing, indicating that the electrode stability was significantly insufficient. This is because the active layer of the electrode and the substrate are bonded by in-situ Ni-O-LDH growth, and the interface relies only on a small number of ionic bonds and van der Waals forces to achieve bonding. The interface bonding strength is insufficient and cannot withstand the harsh working environment of high current density, fluid erosion, bubble disturbance and high temperature and strong alkalinity. During long-term operation, the active layer is prone to detachment and failure, resulting in voltage rise.
[0102] Comparative Example 2 Compared with Example 1, no hydroxide slurry was added, and the remaining steps were the same as in Example 1, resulting in an electrode for alkaline water electrolysis oxygen anode.
[0103] Testing revealed that the surface of the nickel foam was a smooth and dense pure nickel plating. Testing also showed that the ultrasonic weight loss rate of the electrode prepared in Comparative Example 2 for use as an oxygen anode in alkaline water electrolysis was 1.1%; 500 mA / cm² 2 The potential was 0.69 V vs Hg / HgO, indicating low electrode activity. ALK stability testing showed that the electrode prepared in Comparative Example 2 for the alkaline water electrolysis oxygen anode, after 270 h of stability testing, had a chamber voltage 128 mV higher than that in Example 1. (See [reference]). Figure 8 This is because the active phase of the electrode is pure metallic nickel, which is a non-oxygen evolution active phase. Compared with nickel-based hydroxides, its intrinsic oxygen evolution catalytic activity is lower and the reaction overpotential is higher.
[0104] Comparative Example 3 Compared to Example 1, the composition of the composite plating solution was changed.
[0105] In Comparative Example 3, nickel nitrate and iron nitrate were not added to the composite plating solution, and the remaining steps were the same as in Example 1, thus obtaining an electrode for alkaline water electrolysis oxygen anode.
[0106] See Figure 9 It can be seen that the electrode prepared in Comparative Example 3 for the oxygen anode of alkaline water electrolysis has a smooth surface. After the iron hydroxide is reduced, it becomes a nickel-iron phase, which does not belong to the composite coating and has no obvious hydroxide / metal interface.
[0107] Tests showed that the ultrasonic weight loss rate of the electrode prepared in Comparative Example 3 for use as an oxygen anode in alkaline water electrolysis was 1.9%; 500 mA / cm 2 The potential was 0.62V vs Hg / HgO. ALK stability testing showed that the electrode prepared in Comparative Example 3 for the alkaline water electrolysis oxygen anode, after 270 h of stability testing, had a chamber voltage 76mV higher than that in Example 1. (See [reference]). Figure 8 This is because in the oxidative environment without nitrate, under the influence of cathodic reduction during electrolysis, a large amount of nickel-based hydroxide active phase on the electrode surface is reduced to metallic elements, resulting in a significant decrease in the content of effective oxygen evolution active phase on the electrode surface and a deterioration in catalytic performance.
[0108] Comparative Example 4 Compared to Example 1, the state of the hydroxide slurry was changed.
[0109] In Comparative Example 4, the Fe(OH)3 slurry from Example 1 was dried at 60°C for 24 h, ground into powder, and then dispersed in the plating solution with a solid content of 2 g / L. The remaining steps were the same as in Example 1, and an electrode for alkaline water electrolytic oxygen anode was obtained.
[0110] It can be observed that the plating solution contains obvious solid particles, which precipitate to the bottom of the electrolytic cell within 1 minute after stirring is stopped. This indicates that the powder particles are relatively large, difficult to disperse, and easily adsorb and precipitate. See also Figure 10 It can be seen that the surface particles of the electrode prepared in Comparative Example 4 for alkaline water electrolysis oxygen anode are larger and the number is significantly reduced compared with Example 1, indicating that the dry powder is difficult to be efficiently deposited on the surface of the conductive substrate during the electroplating process.
[0111] Tests showed that the ultrasonic weight loss rate of the electrode prepared in Comparative Example 4 for the electrolytic oxygen anode in alkaline water was 1.8%; 500 mA / cm 2 The potential was 0.55V vs Hg / HgO. ALK stability testing showed that the electrode prepared in Comparative Example 4 for the alkaline water electrolysis oxygen anode, after 270 h of stability testing, had a chamber voltage 54 mV higher than that in Example 1. (See [reference]). Figure 8 .
[0112] Comparative Example 5 Compared to Example 4, the current density in step S3 was changed.
[0113] In Comparative Example 5, the current density in step S3 is 30 A / dm. 2 The remaining steps are the same as in Example 4, and an electrode for the oxygen anode of alkaline water electrolysis is obtained.
[0114] Reference Figure 11The large-area cracking and peeling of the nickel mesh surface coating indicates that the high current density leads to an excessively fast deposition rate, intensified hydrogen evolution, increased internal stress in the coating, and prevents hydroxide particles from bonding tightly with the nickel coating.
[0115] Testing showed that the ultrasonic weight loss rate of the electrode prepared in Comparative Example 5 for the electrolytic oxygen anode in alkaline water was 68%; 500 mA / cm 2 The potential was 0.60 vs Hg / HgO. Due to severe detachment, large metal slags penetrating the diaphragm could cause a short circuit in the electrolytic cell, therefore it was not used in the cell.
[0116] The aforementioned hydroxide composite plating electrode, preparation method, and application for alkaline water electrolytic oxygen anodes utilize a method that directly disperses hydroxide slurry in a composite plating solution. The synthesized hydroxide slurry is simply washed and concentrated before being added directly to the composite plating solution, completely eliminating the need for drying and grinding processes. This fundamentally avoids the agglomeration problem of hydroxide powder during drying and ensures good dispersion of hydroxide particles in the plating solution. A one-step composite electroplating method can deposit a hydroxide / nickel composite coating on the surface of a conductive substrate. During DC electroplating, the hydroxide and oxygen... Hydroxide particles are in situ embedded in the growing nickel plating layer as nickel ions are reduced, forming a particle-reinforced composite plating structure. The hydroxide particles are tightly coated and mechanically fixed by the nickel substrate, significantly improving the bonding strength between the plating layer and the conductive substrate. This effectively avoids the problem of easy detachment and peeling of catalytic layers prepared by traditional coating or bonding methods under high current density oxygen evolution conditions. At the same time, the continuous and dense nickel plating layer, as a conductive network and structural support phase, effectively compensates for the low intrinsic conductivity of hydroxide, promoting rapid charge transport between the catalytic active sites and the substrate. Moreover, by synergistically introducing nickel nitrate, iron nitrate, and hydroxide slurry into the composite plating solution, Ni and Fe elements are co-deposited and uniformly distributed in the composite plating layer during electroplating. The resulting hydroxide / nickel composite plating layer is rich in NiFe-LDH and / or Fe(OH)3 highly active catalytic phases, providing abundant alkaline oxygen evolution reaction active sites, significantly reducing the oxygen evolution overpotential, and exhibiting excellent electrocatalytic activity and reaction kinetics.
[0117] Moreover, the raw materials of this invention are all inexpensive and readily available conventional chemical reagents, the preparation method is simple, the operation is convenient and controllable, it is easy to scale up production, and it has good prospects for industrial application.
[0118] In summary, the above-described technical solutions of the present invention are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. All equivalent structural transformations made using the contents of the present invention's specification and drawings under the technical concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.
Claims
1. A method for preparing a hydroxide composite plating electrode for an alkaline water electrolysis oxygen anode, characterized in that, Includes the following steps: S1: Provide a hydroxide slurry, wherein the hydroxide slurry includes one of NiFe-LDH slurry and Fe(OH)3 slurry; the solid content is 10-30% based on the total mass of the hydroxide slurry; S2: Prepare a composite plating solution, wherein the composite plating solution comprises nickel main salt, boric acid, nickel chloride, nickel nitrate, ferric nitrate and the hydroxide slurry; based on the total volume of the composite plating solution, the concentration of nickel nitrate is 2~6 g / L, the concentration of ferric nitrate is 1~3 g / L, and the hydroxide solid content introduced by the hydroxide slurry is 0.5~2 g / L; S3: Using the pretreated conductive substrate as the cathode and the nickel plate as the anode, the substrate is placed in the composite plating solution and composite electroplating deposition is performed using a DC power supply to form a hydroxide / nickel composite plating layer on the surface of the pretreated conductive substrate, thus obtaining the hydroxide composite plating electrode for alkaline water electrolytic oxygen anode. The hydroxide / nickel composite coating is a composite coating of hydroxide and pure nickel formed by a pure nickel phase encapsulating a hydroxide phase.
2. The method for preparing a hydroxide composite plating electrode for an alkaline water electrolysis oxygen anode according to claim 1, characterized in that, The NiFe-LDH slurry was prepared by a hydrothermal synthesis method. The method for preparing the NiFe-LDH slurry includes: Nickel nitrate and iron nitrate were weighed according to a Ni:Fe molar ratio of 2:1 to 4:1, with a total molar amount of 0.9 mmol. 6 mmol CO(NH2)2, 2.2 mmol NH4F and 20 mL water were added, and the mixture was reacted at 100 to 140 °C for 6 to 24 h. After the reaction was completed, the mixture was centrifuged, washed, and concentrated to a solid content of 10 to 30%, without drying.
3. The method for preparing a hydroxide composite plating electrode for an alkaline water electrolysis oxygen anode according to claim 1, characterized in that, The Fe(OH)3 slurry was prepared by electroplating. The method for preparing the Fe(OH)3 slurry includes: Using an iron plate as the anode and a nickel or stainless steel plate as the cathode, a constant current density of 20–200 mA / cm² is applied in an electrolyte solution containing 8–25 mmol Fe(NO₃)₃·9H₂O and 0.2–1 mmol NaNO₃. 2 Electrolyze for 30-300 seconds, stirring during the process. After electrolysis, allow to stand, centrifuge, wash, and concentrate to a solid content of 10-30%, without drying.
4. The method for preparing a hydroxide composite plating electrode for an alkaline water electrolysis oxygen anode according to claim 1, characterized in that, The nickel main salt includes nickel aminosulfonate; Based on the total volume of the composite plating solution, the composite plating solution comprises: nickel aminosulfonate (Ni(SO3NH2)2·4H2O) at 300~400 g / L, boric acid at 20~40 g / L, nickel chloride at 5~15 g / L, nickel nitrate at 2~6 g / L, and ferric nitrate at 1~3 g / L.
5. The method for preparing a hydroxide composite plating electrode for an alkaline water electrolysis oxygen anode according to claim 1, characterized in that, The nickel main salt includes nickel sulfate; Based on the total volume of the composite plating solution, the composite plating solution comprises: 300-400 g / L of nickel sulfate (NiSO4·6H2O), 30-40 g / L of boric acid, 5-15 g / L of nickel chloride, 2-6 g / L of nickel nitrate, and 1-3 g / L of ferric nitrate.
6. The method for preparing a hydroxide composite plating electrode for an alkaline water electrolysis oxygen anode according to claim 1, characterized in that, The temperature of the composite plating solution is 20~60℃; The parameters for the composite electroplating deposition include: an electrode spacing of 10-20 cm, a stirring speed of 200-400 rpm, and a current density of 3-15 A / dm³. 2 The electroplating time is 10~40 minutes.
7. A hydroxide composite plating electrode for use as an oxygen anode in alkaline water electrolysis, characterized in that, The hydroxide composite plating electrode for alkaline water electrolysis oxygen anode is prepared according to any one of claims 1 to 6.
8. The hydroxide composite plating electrode for alkaline water electrolysis oxygen anode according to claim 7, characterized in that, The hydroxide composite plating electrode for alkaline water electrolysis oxygen anode includes a conductive substrate and a hydroxide / nickel composite plating layer formed on the surface of the conductive substrate. In the composite coating, metallic nickel is a continuous phase, hydroxide particles are a discrete phase, and the hydroxide particles are encapsulated and / or anchored inside the metallic nickel matrix. The hydroxide includes one of NiFe-LDH and Fe(OH)3.
9. The hydroxide composite plating electrode for alkaline water electrolysis oxygen anode according to claim 7, characterized in that, The pretreatment steps include degreasing and pickling activation; The conductive substrate includes one of nickel mesh and nickel foam. The Fe element mass fraction in the composite coating is 0.5~1.5%.
10. An electrode prepared by the method for preparing a hydroxide composite plating electrode for an oxygen anode in alkaline water electrolysis as described in any one of claims 1 to 6, or an electrode for preparing a hydroxide composite plating electrode for an oxygen anode in alkaline water electrolysis as described in any one of claims 7 to 9, in alkaline water electrolysis for hydrogen production, characterized in that, The alkaline water electrolysis includes one of alkaline electrolyzed water (ALK) and anion exchange membrane water electrolysis (AEM).