Nanowires, methods for preparing nanowires and electronic devices

By forming metal nanoparticle alloying sites on a semiconductor substrate and using laser-induced redox reactions, the problems of monodispersity and directional growth of nanowires have been solved, achieving efficient and low-cost nanowire fabrication suitable for sensors and field-effect devices.

CN123108714APending Publication Date: 2026-11-17SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510606381.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing liquid-phase growth methods produce nanowires with poor monodispersity, making it difficult to achieve directional and localized growth. Furthermore, the high vacuum and high cost limit mass production.

Method used

Metal nanoparticle alloying sites are formed on a semiconductor substrate. Laser irradiation is used to initiate a redox reaction of the complex to generate single-crystal nanowires. The alloying sites are used as growth sites to induce vertical growth of the nanowires, avoiding subsequent arrangement and assembly processes.

Benefits of technology

Single-crystal nanowires with high crystallinity and high collimation, good monodispersity and tunable geometry, are suitable for applications such as sensors and field-effect devices, while reducing reaction temperature and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108714A_ABST
    Figure CN123108714A_ABST
Patent Text Reader

Abstract

This invention provides nanowires, a method for preparing nanowires, and an electronic device. The method involves forming alloying sites on the surface of a semiconductor substrate using metal nanoparticles, which serve as growth sites for confined nanowire growth. The nanowire growth process then proceeds by irradiating the semiconductor substrate with a laser to initiate a redox reaction of a complex in a precursor solution. The resulting atoms dissolve in molten metal droplets. The alloying sites are used as growth sites to induce the growth of single-crystal nanowires. This reduces the reaction temperature of the system and avoids the subsequent arrangement and assembly processes required for conventional solution-phase nanowire growth. This method enables the production of single-crystal nanowires with high crystallinity and collimation on a semiconductor substrate. The resulting nanowires exhibit good monodispersity and tunable geometric dimensions, and the reaction conditions are mild.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing low-dimensional materials, and in particular to a nanowire and its preparation method. Background Technology

[0002] Nanowires are a typical type of nanomaterial. Nanowires composed of silicon and germanium, due to their high specific surface area, quantum size effect, enhanced field emission and photoluminescence properties, and tunable band gaps, have broad application prospects in sensors and field-effect devices. Currently, nanowire growth methods are mainly divided into two categories based on the type of precursor: vapor-liquid-solid (VLS) and solution-liquid-solid (SLS) growth methods. The VLS method for growing nanowires is a mature technology, primarily used for growing vertical nanowire arrays on substrates. Through decades of continuous research, it has become possible to grow nanowires in systems with significantly optimized reaction temperatures using the VLS method. VLS nanowire growth can achieve high crystallinity, collimation, and perpendicularity, and even allows for a degree of diversified growth control. However, the high vacuum required remains a technical bottleneck limiting its application to mass production. The solution-phase SLS method can also achieve high-quality semiconductor nanowire growth.

[0003] Nevertheless, current solutions-based SLS methods for growing nanowires have the following limitations:

[0004] 1) Since the precursor / target in the VLS reaction system still participates in the reaction in gaseous form, process parameters such as reaction temperature have been optimized, but the high vacuum required by the system is still a technical bottleneck that limits the application of this method to mass production. At the same time, due to the instrument precision limitations, it is difficult to obtain nanowire arrays of 10 nm and smaller sizes by etching method, and the cost is too high and the process is complicated.

[0005] 2) Compared to the VLS method, nanowires grown by the SLS method are usually dispersed in solution and require subsequent arrangement and assembly, making it impossible to achieve directional and localized growth of nanowires.

[0006] 3) Conventional SLS methods for generating nanowires are time-consuming and the final samples are prone to agglomeration. The nanowires also suffer from poor monodispersity and the formation of polycrystalline nanowires. Even when combined with laser technology, it remains difficult to introduce the nanowires into a substrate, making it impossible to obtain nanowire arrays.

[0007] 4) The technical challenges of the SLS method revolve around the upper limit growth of nanowires on the substrate, thereby inducing the directional growth of nanowires on the substrate. In addition, most current hydrothermal / solvothermal methods for growing semiconductor nanowires still require inert gases (N2, Ar, etc.) as protective gases.

[0008] 5) In some cases, it is necessary to fabricate arrayed nanowires on a substrate. At present, nanowire arrays are commonly prepared using templates based on nanoimprinting or styrene templates. The former method is difficult to achieve a regular array with micron-level spacing, while the latter method requires the prior arrangement of microspheres to obtain a regular array of nanowires, which has poor repeatability and cannot be applied to subsequent device processes. Summary of the Invention

[0009] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a nanowire, a method for preparing nanowires, and an electronic device to solve the problems of poor size monodispersity of nanowires synthesized by existing liquid phase growth methods, making it difficult to achieve directional and localized growth of single-crystal nanowires.

[0010] To achieve the above and other related objectives, the present invention provides a method for preparing nanowires, comprising the following steps:

[0011] A semiconductor substrate is provided, the intermediate is applied to the semiconductor substrate, the intermediate is transformed into metal nanoparticles on the semiconductor substrate, and the metal nanoparticles are fixed to the semiconductor substrate and alloying sites are formed on its surface, wherein the semiconductor substrate has a (111) crystal plane, and the metal nanoparticles comprise a group III, IV or V metal.

[0012] Prepare a precursor solution, wherein the precursor solution contains a coordination compound of a Group IV element and a reducing agent;

[0013] The semiconductor substrate on which the metal nanoparticles are fixed is immersed in the precursor solution. The semiconductor substrate is irradiated with a laser to activate the metal nanoparticles, and a complex redox reaction is initiated in the precursor solution to generate Group IV element atoms. At least a portion of the metal nanoparticles are transformed into a molten state to dissolve the generated Group IV element atoms. Single-crystal nanowires of Group IV elemental semiconductor are induced to grow using alloying sites as growth sites. The resulting single-crystal nanowires grow perpendicular to the surface of the semiconductor substrate.

[0014] Optionally, the preparation step of the intermediate of the metal nanoparticles and the step of applying the intermediate to the semiconductor substrate are performed simultaneously in the following manner:

[0015] An intermediate metal film is formed on the semiconductor substrate by physical vapor deposition, wherein the semiconductor substrate is made of an element composed of group IV main elements, and the metal nanoparticles contain noble metals.

[0016] Optionally, the step of preparing the intermediate of the metal nanoparticles includes: preparing a precursor solution of the group III, IV or V metal, and dispersing the noble metal nanoparticles in the precursor solution of the group III, IV or V metal to prepare a suspension.

[0017] Optionally, the semiconductor substrate on which the intermediate is applied is annealed by laser annealing or rapid thermal annealing to transform the intermediate into metal nanoparticles, while the metal nanoparticles form alloying sites on the surface of the semiconductor substrate.

[0018] Optionally, the step of inducing the growth of single-crystal nanowires using the alloying sites as growth sites includes: using laser irradiation to transform part or all of the group III, IV or V metals into metal droplets, accelerating the reduction reaction near the metal nanoparticles, and after the group IV element atoms dissolved in the metal droplets reach a saturation concentration, inducing the growth of single-crystal nanowires using the alloying sites as growth sites, wherein the resulting single-crystal nanowires are oriented in a direction perpendicular to the surface of the semiconductor substrate; wherein the metal nanoparticles comprise one or an alloy of multiple metals selected from Ga, In, Sn, Al, and Bi.

[0019] Optionally, the step of preparing the precursor solution includes: transferring a reducing agent and a solvent for mixing, followed by introducing an inert gas to obtain a pretreated reaction solution; dissolving the precursor powder in the pretreated reaction solution; wherein the reducing agent is selected from tri-n-octylphosphine (TOP) and oleylamine.

[0020] Optionally, the step of applying the intermediate to the semiconductor substrate includes:

[0021] Remove the intrinsic oxide layer from the semiconductor substrate;

[0022] A patterned template is formed on the semiconductor substrate, and an array of openings is formed in the patterned template to expose the surface of the semiconductor substrate;

[0023] Through laser annealing or rapid thermal annealing, the opening defines the contact area between the intermediate and the semiconductor substrate, and the intermediate is transformed into metal nanoparticles in the contact area. The metal nanoparticles form an array of alloying sites on the surface of the semiconductor substrate.

[0024] Optionally, the step of preparing the precursor solution of the group III, IV or V metal includes:

[0025] A precursor, reducing agent, and surface ligand containing the group III, IV, or V metals are added to the oil phase solvent to react and obtain a suspension containing dispersed metal nanoparticles; the suspension containing dispersed metal nanoparticles is diluted and centrifuged to classify, and the supernatant is taken as an intermediate solution, wherein the metal nanoparticles contain Bi and an alloy selected from Ga, In, and Sn.

[0026] The present invention also provides a method for preparing nanowires, comprising the following steps:

[0027] Intermediates for preparing metal nanoparticles;

[0028] A semiconductor substrate is provided, the intermediate is applied to the semiconductor substrate, the intermediate is transformed into metal nanoparticles on the semiconductor substrate, and the metal nanoparticles are fixed to the semiconductor substrate and alloying sites are formed on its surface, wherein the semiconductor substrate has a (111) crystal plane, and the metal nanoparticles comprise a group III, IV or V metal.

[0029] Prepare a precursor solution, wherein the precursor solution comprises a Group III precursor, a Group V precursor, and a reducing agent;

[0030] The semiconductor substrate on which the metal nanoparticles are fixed is immersed in the precursor solution. The semiconductor substrate is irradiated with a laser to activate the metal nanoparticles, and a complex redox reaction is initiated in the precursor solution to generate III and V group element atoms. At least a portion of the metal nanoparticles and the generated III and V group element atoms form a fused state. Single-crystal nanowires of III-V group compound semiconductors are induced to grow using alloying sites as growth sites. The resulting single-crystal nanowires grow perpendicular to the surface of the semiconductor substrate.

[0031] Optionally, the preparation step of the intermediate of the metal nanoparticles and the step of applying the intermediate to the semiconductor substrate are performed simultaneously in the following manner:

[0032] An intermediate metal film is formed on the semiconductor substrate by physical vapor deposition, wherein the semiconductor substrate is a compound semiconductor substrate composed of III-V group elements.

[0033] Optionally, the step of preparing the intermediate of the metal nanoparticles includes: preparing a precursor solution of the group III, IV or V metal.

[0034] Optionally, the semiconductor substrate on which the intermediate is applied is annealed by laser annealing or rapid thermal annealing to transform the intermediate into metal nanoparticles, while the metal nanoparticles form alloying sites on the surface of the semiconductor substrate.

[0035] Optionally, the step of applying the intermediate to the semiconductor substrate includes:

[0036] The semiconductor substrate is pre-cleaned;

[0037] A patterned template is formed on the semiconductor substrate, and an array of openings is formed in the patterned template to expose the surface of the semiconductor substrate;

[0038] Through laser annealing or rapid thermal annealing, the opening defines the contact area between the intermediate and the semiconductor substrate, and the intermediate is transformed into metal nanoparticles in the contact area. The metal nanoparticles form an array of alloying sites on the surface of the semiconductor substrate.

[0039] This invention provides a nanowire, which is prepared using the aforementioned nanowire preparation method:

[0040] The nanowires grow from the alloying sites of the metal nanoparticles fixed on the semiconductor substrate in a direction perpendicular to the surface of the semiconductor substrate, and the nanowires are arranged at intervals on the semiconductor substrate.

[0041] Optionally, the diameter of the nanowire is from 20 nm to 400 nm, and the length of the nanowire along the growth direction is from 0.3 μm to 7 μm.

[0042] The present invention provides a nanowire array comprising the aforementioned nanowires arranged in an array on the semiconductor substrate.

[0043] The present invention also provides an electronic device comprising the aforementioned nanowires, the electronic device including a solar cell, a sensor, a light-emitting diode, a laser diode, an electroluminescent (EL) device, a photoluminescent (PL) device, a cathodic emission (CL) device, and a field-effect transistor (FET).

[0044] As described above, the nanowires, nanowire preparation method, and electronic device provided by the present invention have the following beneficial technical effects:

[0045] The nanowire preparation method of this invention involves forming alloying sites on the surface of a semiconductor substrate using metal nanoparticles, followed by nanowire growth. A laser irradiation of the semiconductor substrate initiates a redox reaction of a complex, and the resulting atoms dissolve in molten metal droplets. The alloying sites are used as growth sites to induce the growth of single-crystal nanowires. This method lowers the reaction temperature of the system and avoids the subsequent arrangement and assembly processes required for conventional liquid-phase nanowire growth. It enables the production of single-crystal nanowires with high crystallinity and high collimation on semiconductor substrates. The resulting nanowires exhibit good monodispersity and tunable geometric dimensions, and the reaction conditions are mild, suggesting broad application prospects.

[0046] The nanowire preparation method of the present invention provides a method for obtaining spaced or arrayed nanowires on a semiconductor substrate. The nanowires have high crystallinity, collimation, and perpendicularity, which can meet the application requirements of sensors, field emission devices, field effect devices, etc. Attached Figure Description

[0047] Figure 1 The flowchart shown is a process for preparing nanowires in this invention.

[0048] Figure 2 This is a schematic diagram of the nanowire growth apparatus based on solution phase growth according to the present invention.

[0049] Figure 3 and Figure 4 The diagram shows the application of different types of lasers during the confined growth process of nanowires in an embodiment of the present invention.

[0050] Figure 5 Figures 9 to 9 are schematic diagrams of the structures obtained at each stage of the fabrication method of the nanowire array according to the present invention; wherein, Figures 6A to 9A This is a schematic diagram of the structure obtained at different stages of the photolithography process used to form a patterned template during the fabrication of nanowire arrays. Figures 6B to 9B The diagram shows the structures obtained at different stages of the fabrication process of nanowire arrays, which uses a combination of photolithography and etching processes to form a patterned template.

[0051] Figures 10A to 10D The diagram illustrates the principle of nanowires grown from solution phase in this invention example.

[0052] Component designation explanation

[0053] 1. Closed chamber

[0054] 2 Support base

[0055] 3. Laser source

[0056] 4. Focusing lens

[0057] 5. Vacuum pumping equipment

[0058] 6. Gas Piping

[0059] 7. Reaction Vessel

[0060] 301 laser beam

[0061] 10 Semiconductor substrate

[0062] 20a, 20b Graphical templates

[0063] 310 Intermediate Metal Film

[0064] 31a and 31b metal nanoparticles

[0065] 32 nanowires

[0066] Steps S11~S14, S21~S25 Detailed Implementation

[0067] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0068] In the detailed description of embodiments of the present invention, for ease of explanation, the cross-sectional views illustrating the device structure may be partially enlarged and not to scale. Furthermore, the schematic diagrams are merely examples and should not limit the scope of protection of the present invention. In actual fabrication, the three-dimensional spatial dimensions of length, width, and depth should be included.

[0069] For ease of description, spatial relation terms such as “below,” “under,” “lower than,” “below,” “above,” and “upper” may be used herein to describe the relationship between one element or feature shown in the accompanying drawings and other elements or features. It will be understood that these spatial relation terms are intended to include directions other than those depicted in the drawings for devices in use or operation. Furthermore, when a layer is referred to as being “between” two layers, it may be the only layer between the two layers, or there may be one or more layers in between.

[0070] In the context of this application, the structure described above the first feature may include embodiments in which the first and second features are formed in direct contact, or embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.

[0071] It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the illustrations only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.

[0072] Compared to VLS (Vacuum-Layered Synthesis), solution-phase-based SLS (Synthetic-Layered Synthesis) can also achieve high-quality semiconductor nanowire growth. Traditional SLS systems are mild, based on an aliphatic alkane chemical environment. By introducing small or large molecular ligands, the growth of nanowire crystal faces is suppressed, thus achieving a one-dimensional linear structure. Simultaneously, high temperatures can be used to ensure reactivity and nanowire crystallinity. Recent studies have shown that combining electrochemistry (electrolysis of the reaction solution) with SLS, using low-melting-point metal catalysts, can achieve rapid growth of semiconductor nanowires at room temperature.

[0073] Although the SLS method described above can obtain nanowire solutions, it cannot achieve confined growth of nanowires on a substrate, that is, it does not fix the catalyst on the substrate, thereby failing to induce directional growth of nanowires on the substrate.

[0074] Preparation methods of nanowires

[0075] like Figure 1 As shown, the present invention provides a method for preparing nanowires.

[0076] The preparation method of the nanowires of the present invention will be described in detail below with reference to the accompanying drawings. It should be noted that the above order does not strictly represent the preparation order of the nanowires of the present invention, and those skilled in the art can modify it according to the actual process steps. Figure 1 The fabrication steps of the nanowires are shown in only one example.

[0077] like Figure 1 In step S11, an intermediate for preparing metal nanoparticles is prepared.

[0078] In step S11, the intermediate can be an intermediate solution for synthesizing metal nanoparticles or an intermediate metal film formed directly on a semiconductor substrate. The metal nanoparticles contain group III, IV or V metals, including but not limited to, for example, Ga, In, Sn, Al, Bi. Preferably, the metal nanoparticles are bismuth nanoparticles, which have a photothermal effect to accelerate the reaction rate in the SLS reaction system.

[0079] Furthermore, the metal nanoparticles also contain noble metals, which can be selected based on a multi-element alloy phase diagram of the noble metal element, the group III, IV, or V metal element, and the semiconductor substrate. This ensures that the subsequent annealing process can achieve effective fusion of the metal nanoparticles and the semiconductor substrate, thereby fixing the catalyst. The noble metal is selected from or includes one or a combination of Ag, Au, Pt, and Pd. In an exemplary embodiment, preparing an intermediate solution of the noble metal includes: uniformly dispersing the noble metal nanoparticles in an oil-phase solvent to prepare a colloidal solution; wherein the noble metal nanoparticles are prepared by a chemical reduction method.

[0080] like Figure 1 In step S12, a semiconductor substrate is provided, the intermediate is applied to the semiconductor substrate, the intermediate is transformed into metal nanoparticles on the semiconductor substrate, and the metal nanoparticles are fixed to the semiconductor substrate and alloying sites are formed on its surface.

[0081] Specifically, the semiconductor substrate may include a silicon substrate, a germanium (Ge) substrate, a silicon germanide (SiGe) substrate, or a III-V compound semiconductor substrate, such as indium phosphide, gallium phosphide, or gallium arsenide. The semiconductor substrate may also be a multilayer structure, such as a silicon / germanium-silicon multilayer. In this embodiment, the semiconductor substrates are selected as germanium substrates with (111) crystal planes and indium phosphide substrates, respectively. The term "semiconductor substrate" as used herein refers to a substrate that is itself a semiconductor material or has a semiconductor layer formed on it.

[0082] In step S12, before applying the intermediate to the semiconductor substrate, the semiconductor substrate is pretreated to remove its intrinsic oxide layer. In one example, the specific steps for pretreating the semiconductor substrate are as follows: a germanium substrate of appropriate size is taken, and the germanium substrate is pretreated with hydrofluoric acid to remove its intrinsic oxide layer.

[0083] After step S11, step S12 is performed, in which the intermediate solution is transferred to the semiconductor substrate by suspension coating or drop coating. For example, the intermediate solution is a suspension of dispersed metal nanoparticles.

[0084] Alternatively, step S12 can be performed concurrently with step S11 by forming an intermediate metal film on the semiconductor substrate using physical vapor deposition, wherein the semiconductor substrate is composed of elemental materials of group IV main elements, and the metal nanoparticles contain noble metals.

[0085] In one exemplary embodiment, an intermediate metal film is formed on the semiconductor substrate by vapor deposition, sputtering, or molecular beam epitaxy (MBE); subsequently, the intermediate metal film is transformed into metal nanoparticles by annealing, and the metal nanoparticles form alloying sites in situ with the semiconductor substrate, which serve as growth sites for subsequent nanowires. The alloying sites serve to fix the metal nanoparticles, and the metal nanoparticles act as catalysts in the solution-phase reaction system.

[0086] Furthermore, after the intermediate is applied to the semiconductor substrate, the semiconductor substrate is annealed using a laser annealing process or a rapid thermal annealing (RTP) process. Since there is no solvent interference during the annealing process, the intermediate undergoes atomic-level annealing crystallization, transforming into nanocrystals, thus obtaining metal nanoparticles. By including noble metal nanoparticles in the metal nanoparticles, the metal nanoparticles and the surface of the semiconductor substrate form a multi-component alloy phase after the annealing process. This allows for the regulation of nanowire growth behavior in the actual reaction system. For example, alloy phases of materials such as silicon and germanium with gold and / or bismuth have significantly lower eutectic points and are easy to alloy. At the same time, by selecting the alloy ratio of the metal nanoparticles, the growth and doping results of the nanowires in subsequent steps can be controlled.

[0087] Regardless of specific theories, nanoparticles of group III, IV, or V metals can be prepared by thermal reduction, thermal decomposition, or liquid-phase chemical reduction methods. These group III, IV, or V metals have low melting points, for example, below 270°C. In this embodiment, bismuth nanoparticles are generated from a bismuth source in the intermediate solution via thermal reduction.

[0088] In some embodiments, the intermediate solution contains noble metal nanoparticles. The intermediate solution can be applied to the semiconductor substrate via suspension coating or drop coating, followed by annealing of the semiconductor substrate to fix the nanoparticles containing the noble metal and the III, IV, or V group metals onto the surface of the semiconductor substrate. In some cases, noble metal nanoparticles are prepared by chemical reduction, and can be dispersed in an oil phase solution to form a solution of nanoscale noble metal colloids. Further, a dispersant is added to the oil phase solvent, and the dispersant coats the surface of the noble metal nanoparticles to prevent metal agglomeration.

[0089] Depending on the circumstances, the metal nanoparticles may also contain transition metals, such as Cu or Pb. For example, after forming an intermediate metal film on the surface of the semiconductor substrate by sputtering, Cu metal nanoparticles are formed in an oil-phase solvent using laser reduction.

[0090] like Figure 1 In step S13, the precursor solution is prepared.

[0091] In some embodiments, the precursor solution contains coordination compounds of Group IV elements for growing Group IV nanowires. The steps for preparing the precursor solution include: ① weighing an appropriate amount of precursor powder under a protective atmosphere and placing it in a transition chamber for later use; ② mixing a reducing agent and a solvent, followed by introducing an inert gas to obtain a pretreated reaction solution; ③ dissolving the pre-weighed precursor powder in the pretreated reaction solution; wherein the coordination compound of the Group IV element includes a dissolved inorganic salt of the Group IV element and a ligand, the inorganic salt of the Group IV element includes a halide of the Group IV element, and the reducing agent is selected from one or a combination of tri-n-octylphosphine (TOP) and oleylamine. Tri-n-octylphosphine (TOP) can act as a reducing agent, ligand, and surfactant in the reaction system. Furthermore, in the SLS reaction, by adding a surfactant to adjust the effective surface energy of the nanocrystals, the selective end-capping effect is beneficial for promoting the growth of nanowires along a specific direction.

[0092] In another embodiment, the precursor solution includes a Group III precursor and its ligand, a Group V precursor and its ligand, for growing Group III-V nanowires. The step of preparing the precursor solution includes: sequentially removing the Group III precursor and its ligand, the Group V precursor and its ligand, and a solvent under anhydrous and oxygen-free conditions. In some examples, the Group III-V compounds include, but are not limited to, indium phosphide (InP), gallium phosphide (GaP), and gallium arsenide (GaAs).

[0093] In a specific example, a precursor solution for growing indium phosphide nanowires is prepared. The precursor solution comprises an indium precursor and its ligands, a phosphorus precursor and its ligands, and a solvent. The indium precursor is, for example, one of indium chloride, indium iodide, indium bromide, indium acetylacetone, and indium acetate. The indium ligands include, for example, one of hexadecanoic acid, myristic acid, and oleic acid, which can act as a reducing agent and surfactant in the reaction system. The phosphorus precursor is, for example, one of tris(trimethylsilyl)phosphine and tris(triethylsilyl)phosphine. The phosphorus ligands include, for example, one of trioctylphosphine and tributylphosphine, which can also act as a reducing agent and surfactant in the reaction system.

[0094] like Figure 1In step S14, the semiconductor substrate on which the metal nanoparticles are fixed is immersed in the precursor solution. The semiconductor substrate is irradiated with a laser to activate the metal nanoparticles, and a complex redox reaction is initiated in the precursor solution, causing at least a portion of the metal nanoparticles to transform into a molten state to dissolve the atoms obtained from the reaction. Single-crystal nanowires are induced to grow using alloying sites as growth sites. The resulting single-crystal nanowires grow in a direction perpendicular to the surface of the semiconductor substrate.

[0095] Figure 2 The diagram shows a growth apparatus for growing nanowires based on a solution phase. The specific structure and usage of the growth apparatus will be described in detail below. In this embodiment, step S14 involves transferring the metal nanoparticles to a sealed chamber. The sealed chamber is configured to perform confined growth of nanowires based on a solution phase. The semiconductor substrate is immersed in the precursor solution with its top surface 1-3 cm below the liquid surface of the semiconductor substrate.

[0096] In some embodiments, step S14 includes: immersing a semiconductor substrate with the immobilized metal nanoparticles in a precursor solution containing dissolved inorganic salts and ligands of group IV elements; irradiating the semiconductor substrate with a laser to activate the metal nanoparticles; initiating a redox reaction of the complex in the precursor solution to generate group IV element atoms; causing at least a portion of the metal nanoparticles to melt to dissolve the generated group IV element atoms; and inducing the growth of single-crystal nanowires of the group IV semiconductor using alloying sites as growth sites. In the SLS reaction system, irradiating the semiconductor substrate with a laser allows for precise and uniform energy distribution / focusing on a limited area. Through heat exchange, the precursor solution is heated to generate group IV element atoms. The alloying sites obtained in step S13 provide growth sites, and under the induction of the semiconductor substrate, the generated group IV element atoms grow into a single-crystal nanowire structure. Due to the high energy of the laser, the reactivity and crystallinity of the nanowires can be guaranteed. Without annealing the metal nanoparticles, only parallel nanowires can be induced to grow on the semiconductor substrate. At the same time, some catalysts will be released into the solution phase during the growth process, inducing the formation of nanowires in the solution. Based on the above scheme, by annealing the metal nanoparticles to form alloying sites on the surface of the semiconductor substrate, the collimated growth of nanowires can be induced. The resulting nanowire structure has high crystallinity and good monodispersity. In particular, when the semiconductor substrate is a semiconductor substrate with a crystal plane (111), the resulting nanowire structure has a growth direction perpendicular to the surface of the semiconductor substrate.

[0097] In another embodiment, step S14 includes: immersing a semiconductor substrate on which the metal nanoparticles are fixed in a precursor solution, the precursor solution containing a Group III precursor, a Group V precursor and a reducing agent; irradiating the semiconductor substrate with a laser to activate the metal nanoparticles; initiating a complex redox reaction in the precursor solution to generate Group III and V element atoms; causing at least a portion of the metal nanoparticles to form a fused state with the generated Group III and V element atoms; and inducing the growth of single-crystal nanowires of a Group III-V compound semiconductor using alloying sites as growth sites.

[0098] In one exemplary embodiment, step S14 includes: irradiating the semiconductor substrate with a laser, and converting part or all of the group III, IV, or V metals into metal droplets, accelerating the reduction reaction near the metal nanoparticles, continuously dissolving group IV element atoms in the metal droplets, precipitating them after reaching a saturation concentration, and inducing the growth of single-crystal nanowires using the alloying sites as growth sites. The resulting single-crystal nanowires are oriented in a direction perpendicular to the surface of the semiconductor substrate. The metal nanoparticles contain one or an alloy of multiple metals, namely Ga, In, Sn, Al, and Bi. In some examples, the oriented growth of nanowires is induced using the alloying sites as growth sites, and the metal droplets obtained from the melting of the metal nanoparticles may contain noble metals and group III, IV, or V metals, whose atoms are embedded in the nanowires. Since noble metals introduce deep-level traps in semiconductors such as silicon and germanium, resulting in low efficiency of deep donor / acceptor in generating mobile charge carriers and acting as non-radiative recombination centers for electron-hole pairs, the introduction of group III, IV, and V metals can improve these effects. In a preferred example, the metal nanoparticles and the precursor solution contain the same Group III metal element, thereby avoiding the introduction of additional impurity atoms, such as indium-containing metal nanoparticles immobilized on the semiconductor substrate, and the precursor solution containing an indium precursor.

[0099] Compared to conventional methods that use only noble metal nanoparticles as catalysts to grow nanowires, the above-mentioned technical solution can obtain single-crystal nanowires in an inert gas environment at room temperature and pressure, or even in an atmospheric environment. The maximum power of the laser required is less than 300W, which significantly reduces the process temperature and greatly saves reaction energy consumption, providing a reliable basis for large-scale production and greatly saving costs and pretreatment time. By introducing a substrate, vertically grown nanowires are directly obtained in one step. Compared with the CVD method, the nanowires obtained by the laser SLS method have a stronger bonding with the substrate. Moreover, the nanowires grown in the solution phase in this invention have a growth rate several times that of conventional solid-phase, gas-phase, or liquid-phase nanowires. The reaction time for growing nanowires can be controlled within 2-3 minutes. For example, the growth rate of nanowires induced by existing methods such as PECVD, VLS, and SLS is basically between 0.03μm / min and 0.3μm / min, which is increased to between 0.33μm / min and 1.8μm / min.

[0100] Preferably, the process is performed by introducing a reducing or inert gas into the sealed chamber under normal temperature and pressure conditions, wherein the inert gas includes one of argon (Ar) and nitrogen (N2).

[0101] It should be noted that the above order does not strictly represent the execution order of the nanowire preparation method protected by this invention, and those skilled in the art can change the order of steps according to the actual process.

[0102] Nanowire growth device

[0103] This invention provides a nanowire growth apparatus for preparing nanowires according to the preparation method described above. The nanowire growth apparatus includes: a laser source 3, a sealed chamber 1, a support base 2, a vacuum pumping device 5, and a gas pipeline 6. The laser source 3 is disposed outside the sealed chamber 1 and irradiates the surface of the substrate to be processed. The support base 2 is located inside the sealed chamber 1 to support the reaction vessel 7, which contains a solution phase for nanowire growth. The support base 2 is operable to move the reaction vessel, thereby achieving optical path alignment of the laser beam 301 emitted by the laser source 3 irradiating the substrate to be processed. The vacuum pumping device 5 is connected to the interior of the sealed chamber 1 and is used to evacuate the interior of the sealed chamber. The gas pipeline 6 is connected to the interior of the sealed chamber 1 and is used to supply at least one of an inert gas, a reducing gas, or the atmosphere to the interior of the sealed chamber 1.

[0104] like Figure 2As shown, the sealed chamber 1 has an internal volume defined by a shell. A transmission window 8 is provided on the shell. A focusing lens 4 or a beam expander can be provided between the laser source 3 and the sealed chamber 1. The laser beam 301 emitted by the laser source 3 is focused by the focusing lens (or expanded by the beam expander) and then penetrates the reaction solution in the reaction container 7 to irradiate the substrate to be processed immersed in it.

[0105] In this embodiment, the reaction container 7 is detachably mounted on the support base 2. The reaction container 7 has sufficient light transmittance to allow laser light to penetrate the precursor solution and irradiate the semiconductor substrate on which the metal nanoparticles are fixed. The reaction container includes, but is not limited to, disposable glass reaction bottles, beakers, spouted circular dishes, crystallizing dishes, or similar glass containers.

[0106] Figure 3 and Figure 4 Schematic diagram of applying different types of lasers during the confined growth of nanowires. (Example) Figure 3 and Figure 4 As shown, the laser source 3 is configured to apply one or a combination of pulsed laser, continuous laser, for example, an Nd:YAG laser.

[0107] Methods for fabricating nanowire arrays

[0108] The present invention also provides a method for using nanowire arrays, comprising the following steps:

[0109] S21; an intermediate for the preparation of metal nanoparticles;

[0110] S22; Provide a semiconductor substrate, and form a patterned template on the semiconductor substrate;

[0111] S23; The intermediate is applied to the surface of the semiconductor substrate on which the patterned template is formed, so that the intermediate is transformed into metal nanoparticles on the semiconductor substrate, and the metal nanoparticles are fixed to the semiconductor substrate and alloying sites are formed on its surface.

[0112] S24; Prepare the precursor solution;

[0113] S25; Immerse the semiconductor substrate with the metal nanoparticles fixed thereon in the precursor solution, irradiate the semiconductor substrate with a laser to activate the metal nanoparticles, and initiate a complex redox reaction in the precursor solution, causing at least a portion of the metal nanoparticles to transform into a molten state to dissolve the atoms obtained from the reaction, and induce the growth of single-crystal nanowires with alloying sites as growth sites. The obtained single-crystal nanowires are arranged in an array on the semiconductor substrate and grow perpendicular to the surface of the semiconductor substrate.

[0114] In step S21, the step of preparing the intermediate solution includes: adding a precursor, a reducing agent, and a surface ligand containing the group III, IV, or V metals to the oil phase solvent to react and obtain a suspension containing group III, IV, or V metal nanoparticles; diluting and centrifuging the suspension, and taking the supernatant as the intermediate solution, wherein the group III metal element includes one or a combination of Ga, In, and Al, the group IV metal element includes Sn, and the group V metal element includes Bi.

[0115] Specifically, in step S22, the semiconductor substrate is preferably a substrate of the same composition as the nanowires to be grown. Utilizing the crystal structure of the semiconductor substrate to induce the growth of nanowires is beneficial for obtaining nanostructures with high crystallinity. In this embodiment, the semiconductor substrate is a germanium substrate with a (111) crystal plane. For example, in solution-phase growth of germanium nanowires on a germanium substrate, before applying the intermediate to the semiconductor substrate in step S22, the semiconductor substrate is pretreated; a patterned template is formed on the semiconductor substrate. As another example, in solution-phase growth of germanium nanowires on a germanium substrate, before applying the intermediate to the semiconductor substrate in step S22, the semiconductor substrate is pre-cleaned; a patterned template is formed on the semiconductor substrate. Figure 5 Figure 9 shows a schematic diagram of the structures obtained at each stage of the fabrication method of the nanowire array according to the present invention.

[0116] In some embodiments, a patterned template is formed on the semiconductor substrate, the patterned template having openings that expose the surface of the semiconductor substrate, wherein the patterned template may be a soft template made by nanoimprinting, such as polydimethylsiloxane (PDMS). Figures 6A to 9A This diagram illustrates the structures obtained at different stages of the photolithography process used to form patterned templates during the fabrication of nanowire arrays. (Example:) Figure 6A As shown, a patterned template 20a is formed by the following steps: a photoresist layer is spin-coated on a germanium substrate; a nanometer / micrometer-scale through-hole array is defined on the germanium substrate through a series of processes such as photolithography, exposure, soft baking, development, and hard baking.

[0117] Alternatively, in other embodiments, a hard template with a transfer pattern layer is formed by photolithography and etching processes, such as a hard template deposited on a semiconductor substrate by atomic layer deposition (ALD) or chemical vapor deposition (CVD), wherein the material of the hard template includes aluminum oxide or silicon dioxide. Figures 6B to 9B The diagram illustrates the structures obtained at different stages of the fabrication process of nanowire arrays, which utilizes a combination of photolithography and etching processes to form a patterned template. (Example:...) Figure 6BAs shown, a patterned template 20b is formed by the following steps: an aluminum oxide or silicon dioxide thin film is prepared on a semiconductor substrate by, for example, PECVD; a patterned area of ​​photoresist is defined on the silicon dioxide thin film by photolithography by coating photoresist; subsequently, the aluminum oxide or silicon dioxide dielectric in the area outside the photoresist coverage is etched away by an anisotropic etching method; residual photoresist on the semiconductor substrate is removed and dried for later use.

[0118] Further, in step S23, the intermediate solution obtained in step S21 is applied to the semiconductor substrate. After the solution dries, the metal nanoparticles, such as bismuth nanoparticles, on the surface of the patterned template are directly removed. The patterned template has an array of openings exposing the surface of the semiconductor substrate. Due to the presence of the photoresist layer / hard template, the metal nanoparticles on its upper surface do not easily contact the semiconductor substrate. Instead, the openings define the contact area between the metal nanoparticles and the semiconductor substrate, where they transform into metal nanoparticles. These metal nanoparticles then form an array of alloying sites on the surface of the semiconductor substrate. Alternatively, in other examples, such as... Figures 8B to 9B As shown, after the metal nanoparticles 31b on the surface of the photoresist layer / hard template are ground and removed by chemical mechanical polishing (CMP), the semiconductor substrate 10 is annealed. Simultaneously, the metal nanoparticles 31b are alloyed in situ with the bulk material of the semiconductor substrate, fixing the metal nanoparticles onto the semiconductor substrate. The metal nanoparticles and the semiconductor substrate form alloying sites in situ, serving as growth sites for subsequent nanowires. These alloying sites fix the metal nanoparticles, which act as catalysts for nanowire growth in the SLS reaction system. The annealing process includes laser annealing or rapid thermal annealing. In other embodiments, the intermediate can also be an intermediate metal film 310 formed on the semiconductor substrate by physical vapor deposition; subsequently, the intermediate metal film 310 covering the patterned template is removed.

[0119] Step S24 in this embodiment can be performed in a similar manner to step S13 of the previous embodiment. In some embodiments, at step S24, the semiconductor substrate on which the metal nanoparticles are immobilized is immersed in the precursor solution, the precursor solution containing dissolved inorganic salts of Group IV elements for growing Group IV nanowires. In another embodiment, at step S24, the semiconductor substrate on which the metal nanoparticles are immobilized is immersed in the precursor solution, the precursor solution containing precursors from Group III and Group V for growing Group III-V nanowires.

[0120] In this embodiment, at step S25, before or after the operation of growing single-crystal nanowires at the alloying sites of the semiconductor substrate, the patterned template is removed; subsequently, the confined growth of single-crystal nanowires at the alloying sites is performed; nanowires are induced to grow at the alloying sites of the semiconductor substrate, while a metal catalyst comprising group III, IV, and V metals is embedded in the nanowires. When the metal nanoparticles contain metals with melting points lower than bismuth, such as In, Ga, or Sn, uniform doping of nanowires such as silicon and germanium can be achieved.

[0121] Based on the above scheme, metal nanoparticles are arrayed and distributed onto a semiconductor substrate and alloyed with the bulk material of the semiconductor substrate. Low-melting-point metals such as Bi, In, and Ga are alloyed with the germanium substrate. The metal nanoparticles are activated by laser, so that at least a portion of the metal nanoparticles are transformed into a molten state. The alloying sites on the surface of the semiconductor substrate provide growth sites for nanowires, realizing collimated growth of nanowires and arraying of nanowires with micrometer or nanometer spacing, thereby realizing a nanowire array with adjustable spacing.

[0122] The following specific embodiments and implementation effect data will be used to further explain and verify the above technical solutions and effects.

[0123] (1) Intermediate for preparing metal nanoparticles

[0124] The intermediate solution for preparing bismuth nanoparticles includes: weighing 0.4-0.8 g of bismuth neodecanoate as a raw material in a reaction vessel, adding 4-4.3 mL of 1-octadecene as a reducing agent, and introducing Ar / N2 at 115℃-130℃ to remove water and oxygen for 60-120 minutes; then transferring the reaction vessel to a glove box, adding 0.5-1.5 mL of trioctylphosphine as a surface ligand, and maintaining the resulting solution at 60℃-730℃ for a complex redox reaction for 20-40 minutes, followed by standing for 2 hours to synthesize a suspension containing bismuth metal micelles; diluting the bismuth metal micelle suspension to 1.5-2.5 times its volume, taking 0.8-1.2 mL of the diluted solution containing bismuth nanoparticles, centrifuging and separating, and collecting the brownish-yellow supernatant for later use.

[0125] The intermediate solution for preparing gold nanoparticles includes: weighing approximately 0.2 mmol-0.35 mmol of triphenylphosphine chloride as a raw material in a reaction vessel, mixing it with 20 mL-40 mL of toluene and 0.8 mmol-1.2 mmol of dodecyl mercaptan to prepare a gold precursor solution, wherein dodecyl mercaptan is used as a surface ligand; weighing 2.0 mmol-3.0 mmol of a methylborane-tert-butylamine complex and dissolving it in 10 mL-20 mL of toluene to prepare a reducing agent solution; preheating the above gold precursor solution and reducing agent solution to 100℃-120℃ respectively, and stirring until completely dissolved; then, rapidly injecting the reducing agent solution into the gold precursor solution, and reacting at a constant temperature of 100℃-120℃ for 4-8 minutes, stopping the reaction and cooling to room temperature, the resulting colloidal solution is finally purple-red; centrifuging the above-reacted micelle solution in a glove box, taking the supernatant and dispersing it in toluene to obtain a diluted solution of nanoscale gold colloids for later use.

[0126] The preparation of an intermediate metal film for bismuth nanoparticles includes: growing a 2nm-10nm bismuth metal film on a pretreated germanium substrate by molecular beam epitaxy (MBE).

[0127] (2) Pretreatment of semiconductor substrate and fixation of metal nanoparticles

[0128] The laser source is an Nd:YAG laser; the parameters are set as follows: laser wavelengths are 1064nm and 532nm; laser power is 10W-60W.

[0129] Germanium and indium phosphide substrates, each having a (111) crystal plane, were pretreated separately. The germanium substrate was pretreated by sequentially cleaning it with acetone and deionized water, followed by removing the intrinsic oxide layer from its surface using hydrofluoric acid or hydrochloric acid; then purging with N2 and drying for later use. The indium phosphide substrate was pretreated by sequentially ultrasonically cleaning it with acetone, isopropanol, and deionized water; then purging with N2 and drying for later use.

[0130] The diluted solutions of bismuth and gold nanoparticles were suspended onto the surface of a germanium substrate. Subsequently, the germanium substrate with the diluted solution was annealed using a laser by performing the following steps to obtain the growth substrate for confined growth of nanowires in Experimental Example 1: First, the guide light of the laser was turned on, the collimation of the optical path was checked, and after confirming that there were no objects obstructing the optical path, the stage was moved to transmit the laser spot to a preset position. Then, the laser was turned on to provide a low-frequency, high-pulse-width laser beam. The laser beam irradiated the diluted solution with bismuth and gold nanoparticles, and annealing and crystallization were performed on the germanium substrate to form bismuth and gold nanoparticles. The laser beam emitted by the laser source can be expanded by a beam expander. The expanded laser beam has a sufficiently large spot size to ensure that the germanium substrate forms an alloy with the metal nanoparticles under irradiation for a few seconds (<10s). The germanium substrate with fixed bismuth and gold nanoparticles was used as the growth substrate for confined growth of germanium nanowires in Experimental Example 1.

[0131] After the indium phosphide substrate pretreatment step, the growth substrate for confined growth of nanowires in Experiment 2 was obtained by performing the following steps: an indium metal film with a thickness of about 2 nm was deposited on the indium phosphide substrate by electron beam evaporation; the indium metal film was annealed at 150°C for 5 minutes using rapid thermal annealing (RTP) process, and indium nanoparticles were crystallized by annealing. The indium phosphide substrate with indium nanoparticles fixed was used as the growth substrate for confined growth of indium phosphide nanowires in Experiment 2.

[0132] After the pretreatment of the germanium substrate, the growth substrate for confined growth of germanium nanowires in Experiment 3 is obtained by performing the following steps: a patterned template is formed on the germanium substrate, specifically by: spin-coating a photoresist layer on the germanium substrate; defining a nanometer / micrometer-scale via array on the germanium substrate through a series of processes including photolithography, exposure, soft baking, development, and hard baking; removing the photoresist and drying it for later use; subsequently, depositing a bismuth metal film with a thickness of approximately 2 nm on the germanium substrate with the via array formed by molecular beam epitaxy (MBE); and removing the bismuth metal film covering the photoresist layer by chemical mechanical polishing (CMP).

[0133] Furthermore, the bismuth metal film was heat-treated at 400°C to 900°C using a rapid thermal annealing (RTP) process to anneal and crystallize into bismuth nanoparticles. The germanium substrate with the bismuth nanoparticles fixed was then used as the growth substrate for the confined growth of the germanium nanowire array in Experimental Example 2.

[0134] (3) Preparation of precursor solution for germanium nanowires

[0135] Raw material: Germanium diiodide (GeI2), yellow powder. After opening, it must be stored in an inert gas environment and protected from light.

[0136] ① Weigh 0.1g-1.0g of GeI2 in a glove box with exhaust treatment and place it in a transition chamber for later use; ② Remove the reaction vessel from the 110℃-130℃ oven, and sequentially transfer about 18mL-22mL of trioctylphosphine (TOP) or oleylamine into the reaction vessel to prepare a ligand solution. Introduce argon gas into the small white bottle at 110℃-130℃ for 1.2-1.8 hours; ③ After the ligand solution cools to room temperature, transfer GeI2 into the cooled ligand solution, seal the container and protect it from light. Use an ultrasonic oscillator to mix GeI2 and the ligand solution for 15-20 minutes until the yellow powder of GeI2 is completely dissolved, obtaining a clear, pale yellow precursor solution for later use. This precursor solution should be prepared immediately before use and should not be stored for a long time.

[0137] (4) Preparation of precursor solution for indium phosphide nanowires

[0138] Under anhydrous and oxygen-free conditions, appropriate amounts of 1-octadecene, approximately 8.0 mmol of myristic acid, and approximately 4.0 mmol of trioctylphosphine were sequentially transferred to prepare a ligand solution. The ligand solution, approximately 8.0 mmol of indium acetylacetone, and approximately 16.0 mmol of tris(trimethylsilyl)phosphine were mixed and placed in a reaction vessel to obtain a precursor solution for later use. This precursor solution should be prepared immediately before use and should not be stored for a long period of time.

[0139] (5) Confined growth of solution-phase nanowires

[0140] Experimental Example 1

[0141] The laser source is an Nd:YAG laser; the parameters are set as follows: laser wavelength is 1064nm; laser power is 10W-60W; the spot size is about 3mm to 7mm; the duration of laser irradiation is 1-30 minutes.

[0142] At room temperature, the precursor solution for growing germanium nanowires is transferred to a reaction vessel, and the pretreated germanium substrate is immersed in the precursor solution with its top surface 1-3 cm below the liquid surface of the precursor solution. The following phenomena can be observed when performing solution-phase growth of germanium nanowires: After the laser is turned on, the precursor solution gradually begins to change color; under continuous laser irradiation, the reaction rate accelerates, and the generated germanium atoms dissolve into the metal droplets until a saturation concentration is reached, agglomerating to form metal clusters; by reducing the laser power, nanocrystals grow at the alloying sites under the induction of the germanium substrate crystal structure, and finally, single-crystal nanowires are directionally grown at these alloying sites. Figures 10A to 10D This diagram illustrates the principle of epitaxial growth of germanium nanowires induced by alloying sites on the surface of a germanium substrate.

[0143] Combination Figures 10A to 10DThe growth behavior of nanowires based on the solution phase can be analyzed as follows:

[0144] In the initial stage of the reaction, the germanium substrate is heated to an extremely high temperature under laser irradiation, which in turn heats the precursor solution through heat exchange. When the surface temperature of the nanoparticle catalyst or the solution rises to the temperature required for the reaction, the redox reaction begins, as shown in Equation 1 below. Therefore, a color change in the precursor solution can be observed. Bismuth metal exhibits a photothermal conversion effect after absorbing a specific wavelength of laser light, and its heating effect is much faster than the thermal conversion effect of the laser-heated substrate on the solution, further rapidly increasing the alloy temperature until it melts. Figure 10A As shown, metal droplets obtained by melting metal nanoparticles (partially or completely) are distributed at intervals on a germanium substrate. Due to the alloying of the metal nanoparticles on the surface of the germanium substrate in the previous steps, they have a certain orientation with the surface of the germanium substrate. Therefore, the molten metal nanoparticles wet the germanium substrate to a certain extent. On the other hand, bismuth metal in the molten state also has enhanced catalytic performance, especially the catalytic performance of activating noble metals such as gold, accelerating the process of redox reaction in the precursor solution. Moreover, the temperature near the alloying site of the germanium substrate will rise rapidly, the reduction reaction rate will be faster, and germanium atoms will be generated more efficiently.

[0145]

[0146] Meanwhile, liquid bismuth metal provides dissolution sites for germanium atoms / nanocrystals. Germanium atoms continuously dissolve in the liquid bismuth metal and enter the metal droplets formed by partial or complete melting (depending on the composition of the metal nanoparticles). This results in a much higher concentration of germanium atoms in the metal droplets compared to the solution phase. Figure 10B As shown; with continuous laser irradiation, the reaction rate accelerates until the germanium atoms in the metal droplets reach a saturation concentration, agglomerate to form metal clusters, and then precipitate, as... Figure 10C The structure shown is formed on a germanium substrate, and island-shaped nanoparticles are formed thereon.

[0147] Next, the laser power is reduced, and the epitaxial growth is driven by the metal droplet. Under the induction of the substrate crystal structure, the nanocrystals are oriented and stably grown. As the reaction continues, metal atoms, such as bismuth atoms, in the metal droplet are continuously consumed until the concentration of dissolved germanium atoms becomes too low to precipitate, thus terminating the growth. Finally, nanowires are grown at this growth site. Figure 10D The structure shown indicates that the resulting nanowires grow stably along a direction perpendicular to the germanium substrate without easily undergoing interparticle fusion or slippage, and the lateral size of the nanowires does not change much along the growth direction.

[0148] In the above reaction process, laser irradiation activates the metal catalyst on the one hand, and at the same time acts as a heat source to rapidly bring the precursor solution to the reaction temperature. The laser induces the epitaxial growth of the solution phase. In the initial stage, a high-frequency, high-pulse-width, and high-peak-energy pulsed laser can be used to accelerate the nucleation process of germanium. In the subsequent reaction stage and the stable growth stage, the laser power can be appropriately reduced to stabilize the growth of nanowires and avoid the high-temperature effect of the laser causing the generated nanowires to melt under the high-temperature laser.

[0149] Experimental Example 2

[0150] The laser source is an Nd:YAG laser; the parameters are set as follows: laser wavelength is 532nm; power density is set to approximately 300W / cm². -2 The duration of laser irradiation is 2 minutes.

[0151] At room temperature, the precursor solution for growing indium phosphide nanowires is transferred to a reaction vessel, and the indium phosphide substrate with indium nanoparticles fixed is immersed in the precursor solution with its top surface 1-3 cm above the liquid surface of the precursor solution. The step of growing indium phosphide nanowires based on solution phase is performed, and the phenomenon of spaced nanowires can be observed, similar to that described in Experimental Example 1. The difference is that, since the precursor solution in Experimental Example 2 contains indium and phosphorus precursors, a complex redox reaction is initiated in the precursor solution to generate indium and phosphorus atoms, causing at least a portion of the indium nanoparticles to form a mutually fused state with the generated indium and phosphorus atoms until the indium and phosphorus atoms in the metal droplet reach a saturation concentration, and then precipitate. Under the induction of the substrate crystal structure, nanocrystalline indium phosphide is directionally and stably grown using alloying sites as growth sites, and finally indium phosphide nanowires are formed.

[0152] Experiment Example 3

[0153] The laser source is an Nd:YAG laser; the parameters are set as follows: laser wavelength is 1064nm; laser power is 10W-60W; the spot size is about 3mm to 7mm; the duration of laser irradiation is 1-30 minutes.

[0154] At room temperature, the precursor solution of germanium nanowires is transferred to a reaction vessel, and the germanium substrate with bismuth nanoparticles is immersed in the precursor solution with its top surface 1-3 cm from the liquid surface of the precursor solution. The step of growing germanium nanowire array based on solution phase is performed, and the phenomenon of arrayed nanowires can be observed, similar to that described in Experimental Example 1. The difference is that, because the surface of the germanium substrate in Experimental Example 2 is fixed with arrayed alloying sites, nanocrystals are grown in a directional and stable manner at the alloying sites, and finally a nanowire array is formed.

[0155] application

[0156] The present invention also provides a nanowire, which is preferably prepared by the aforementioned nanowire preparation method.

[0157] The nanowires are fixed to the semiconductor substrate at alloying sites of metal nanoparticles and grow in a direction perpendicular to the surface of the semiconductor substrate.

[0158] The nanowires are arranged at intervals or in an array on the semiconductor substrate, particularly in an array with micrometer or nanometer-level spacing. In an exemplary embodiment, the diameter of the nanowires is 20 nm to 400 nm, and the length of the nanowires along the growth direction is 0.3 μm to 7 μm; preferably, the nanowires have a lateral dimension that does not change significantly along the growth direction.

[0159] The present invention also provides an electronic device comprising the aforementioned nanowires.

[0160] In some implementations, the electronic device includes a solar cell, a sensor, a light-emitting diode, a laser diode, an electroluminescent (EL) device, a photoluminescent (PL) device, a cathodic light-emitting (CL) device, and a field-effect transistor (FET).

[0161] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for producing a nanowire, characterized by, Includes the following steps: Intermediates for preparing metal nanoparticles; A semiconductor substrate is provided, the intermediate is applied to the semiconductor substrate, the intermediate is transformed into metal nanoparticles on the semiconductor substrate, and the metal nanoparticles are fixed to the semiconductor substrate and alloying sites are formed on its surface, wherein the semiconductor substrate has a (111) crystal plane, and the metal nanoparticles comprise a group III, IV or V metal. Prepare a precursor solution, wherein the precursor solution contains a coordination compound of a Group IV element and a reducing agent; The semiconductor substrate on which the metal nanoparticles are fixed is immersed in the precursor solution. The semiconductor substrate is irradiated with a laser to activate the metal nanoparticles, and a complex redox reaction is initiated in the precursor solution to generate Group IV element atoms. At least a portion of the metal nanoparticles are transformed into a molten state to dissolve the generated Group IV element atoms. Single-crystal nanowires of Group IV elemental semiconductor are induced to grow using alloying sites as growth sites. The resulting single-crystal nanowires grow perpendicular to the surface of the semiconductor substrate.

2. The method of claim 1, wherein: The preparation steps of the intermediate for the metal nanoparticles and the application of the intermediate to the semiconductor substrate are performed simultaneously in the following manner: An intermediate metal film is formed on the semiconductor substrate by physical vapor deposition, wherein the semiconductor substrate is made of an element composed of group IV main elements, and the metal nanoparticles contain noble metals.

3. The preparation method according to claim 1, characterized in that, The step of preparing the intermediate of the metal nanoparticles includes: preparing a precursor solution of the group III, IV or V metal, and dispersing the noble metal nanoparticles in the precursor solution of the group III, IV or V metal to prepare a suspension.

4. The preparation method according to claim 2 or 3, characterized in that, The semiconductor substrate on which the intermediate is applied is annealed using a laser annealing process or a rapid thermal annealing process, which transforms the intermediate into metal nanoparticles and simultaneously forms alloying sites on the surface of the semiconductor substrate using the metal nanoparticles.

5. The preparation method according to any one of claims 1-4, characterized in that; The step of inducing the growth of single-crystal nanowires using the alloying sites as growth sites includes: using laser irradiation to transform part or all of the group III, IV or V metals into metal droplets, accelerating the reduction reaction near the metal nanoparticles, and after the group IV element atoms dissolved in the metal droplets reach a saturation concentration, inducing the growth of single-crystal nanowires using the alloying sites as growth sites, wherein the resulting single-crystal nanowires are oriented in a direction perpendicular to the surface of the semiconductor substrate; wherein the metal nanoparticles comprise one or an alloy of multiple metals selected from Ga, In, Sn, Al, and Bi.

6. The preparation method according to claim 1, characterized in that, Also includes: The step of preparing the precursor solution includes: transferring a reducing agent and a solvent and mixing them, then passing an inert gas through them to obtain a pretreated reaction solution; dissolving the precursor powder in the pretreated reaction solution; wherein the reducing agent is selected from tri-n-octylphosphine and oleylamine.

7. The preparation method according to claim 1, characterized in that, The step of applying the intermediate to the semiconductor substrate includes: Remove the intrinsic oxide layer from the semiconductor substrate; A patterned template is formed on the semiconductor substrate, and an array of openings is formed in the patterned template to expose the surface of the semiconductor substrate; Through laser annealing or rapid thermal annealing, the opening defines the contact area between the intermediate and the semiconductor substrate, and the intermediate is transformed into metal nanoparticles in the contact area. The metal nanoparticles form an array of alloying sites on the surface of the semiconductor substrate.

8. The preparation method according to claim 1, characterized in that, The steps for preparing the precursor solution of the group III, IV or V metal include: A precursor, reducing agent, and surface ligand containing the group III, IV, or V metals are added to the oil phase solvent to react and obtain a suspension containing dispersed metal nanoparticles; the suspension containing dispersed metal nanoparticles is diluted and centrifuged to classify, and the supernatant is taken as an intermediate solution, wherein the metal nanoparticles contain Bi and an alloy selected from Ga, In, and Sn.

9. A method for preparing nanowires, characterized in that, Includes the following steps: Intermediates for preparing metal nanoparticles; A semiconductor substrate is provided, the intermediate is applied to the semiconductor substrate, the intermediate is transformed into metal nanoparticles on the semiconductor substrate, and the metal nanoparticles are fixed to the semiconductor substrate and alloying sites are formed on its surface, wherein the semiconductor substrate has a (111) crystal plane, and the metal nanoparticles comprise a group III, IV or V metal. Prepare a precursor solution, wherein the precursor solution comprises a Group III precursor, a Group V precursor, and a reducing agent; The semiconductor substrate on which the metal nanoparticles are fixed is immersed in the precursor solution. The semiconductor substrate is irradiated with a laser to activate the metal nanoparticles, and a complex redox reaction is initiated in the precursor solution to generate III and V group element atoms. At least a portion of the metal nanoparticles and the generated III and V group element atoms form a fused state. Single-crystal nanowires of III-V group compound semiconductors are induced to grow using alloying sites as growth sites. The resulting single-crystal nanowires grow perpendicular to the surface of the semiconductor substrate.

10. The preparation method according to claim 9, characterized in that: The preparation steps of the intermediate for the metal nanoparticles and the application of the intermediate to the semiconductor substrate are performed simultaneously in the following manner: An intermediate metal film is formed on the semiconductor substrate by physical vapor deposition, wherein the semiconductor substrate is a compound semiconductor substrate composed of III-V group elements.

11. The preparation method according to claim 9, characterized in that, The step of preparing the intermediate of the metal nanoparticles includes: preparing a precursor solution of the group III, IV or V metal.

12. The preparation method according to claim 10 or 11, characterized in that: The semiconductor substrate on which the intermediate is applied is annealed using a laser annealing process or a rapid thermal annealing process, which transforms the intermediate into metal nanoparticles and simultaneously forms alloying sites on the surface of the semiconductor substrate using the metal nanoparticles.

13. The preparation method according to claim 9, characterized in that, The step of applying the intermediate to the semiconductor substrate includes: The semiconductor substrate is pre-cleaned; A patterned template is formed on the semiconductor substrate, and an array of openings is formed in the patterned template to expose the surface of the semiconductor substrate; Through laser annealing or rapid thermal annealing, the opening defines the contact area between the intermediate and the semiconductor substrate, and the intermediate is transformed into metal nanoparticles in the contact area. The metal nanoparticles form an array of alloying sites on the surface of the semiconductor substrate.

14. A nanowire, characterized in that, The nanowires were prepared using the method for preparing nanowires according to any one of claims 1 to 13: The nanowires grow from the alloying sites of the metal nanoparticles fixed on the semiconductor substrate in a direction perpendicular to the surface of the semiconductor substrate, and the nanowires are arranged at intervals on the semiconductor substrate.

15. The nanowire according to claim 14, characterized in that: The nanowires have a diameter of 20 nm to 400 nm and a length of 0.3 μm to 7 μm along the growth direction.

16. A nanowire array, characterized in that, Includes nanowires according to claim 14 arranged in an array on the semiconductor substrate.

17. An electronic device, characterized in that, The electronic device, including the nanowires according to claim 14 or 15, comprises a solar cell, a sensor, a light-emitting diode, a laser diode, an electroluminescent device, a photoluminescent device, a cathode ray emitting device, and a field-effect transistor.