A method for controllable growth of perovskite single crystals based on crown ether host-guest coordination
By regulating the growth process of perovskite single crystals through the host-guest coordination of crown ethers, the problems of disordered multi-nucleation and crystal instability in solution preparation are solved, enabling the controllable growth and reproducible preparation of high-quality, large-size single crystals, which are suitable for photodetectors and X-ray imaging devices.
Patent Information
- Application Number
- CN202611423096.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing solution-based methods for preparing perovskite single crystals suffer from problems such as disordered multinucleation, unstable crystal growth, numerous defects, difficulty in achieving large-size single crystal preparation, and difficulty in standardizing the process.
By employing crown ether host-guest coordination, and by controlling the ionic coordination structure and solvation environment of the precursor solution, combined with seed crystal-induced growth and a low-speed temperature gradient, effective separation of crystal nucleation and growth is achieved, reducing the influence of random nucleation and improving the controllability of the crystallization process and the quality of single crystals.
High-quality, large-size perovskite single crystals with low defect density and high structural uniformity were obtained. The process conditions were mild and the parameter window was controllable, making them suitable for devices such as photodetectors and X-ray imaging.
Smart Images

Figure CN123108716A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of perovskite single crystal preparation technology, specifically relating to a controllable growth method for perovskite single crystals based on crown ether host-guest coordination. Background Technology
[0002] Perovskite single crystals have become a promising semiconductor material in the field of optoelectronic detection due to their excellent carrier migration and transport characteristics, defect tolerance, and low-cost fabrication process. Currently, the solution method can achieve ion-level controllable assembly under low temperature and low supersaturation conditions, and can enable perovskite single crystals to obtain high crystal quality and low defect density with low energy consumption and high chemical designability, making it an ideal method for preparing perovskite single crystals.
[0003] However, although solution processing provides a feasible route for high-quality perovskite single crystal growth at low temperatures, the quality of perovskite single crystals prepared by solution processing is often affected by uncontrolled supersaturation and rapid nucleation kinetics, leading to disordered multinucleation, unstable crystal growth, and V... Cs V Pb The formation of intrinsic defects and undercoordinated surface sites can affect crystal properties. Furthermore, solution methods face significant limitations in crystal size scaling. As crystal growth time increases, the probability of spontaneous nucleation rises significantly, leading to competitive growth between single crystals and hindering the stable fabrication of high-quality, large-size single crystals. Simultaneously, solvent molecules may form stable coordination structures with the precursor during crystallization, resulting in incomplete or uneven desorption processes that can introduce residual stress or localized defect states within the crystal, affecting carrier transport properties and device stability. On the other hand, solution methods typically require long growth times. During these extended periods, impurity accumulation, container wall adsorption effects, and external environmental disturbances gradually amplify, significantly impacting the final crystal quality. Finally, solution methods are highly sensitive to environmental conditions, requiring strict control over temperature, humidity, and solvent purity. The relatively narrow process window makes high standardization and large-scale production difficult. Therefore, while solution methods are well-suited for the preparation and mechanism study of high-quality single crystals, they still face limitations in reproducibility control, size scaling, and engineering applications.
[0004] Problems such as size scaling and reproducible growth control severely restrict the application of perovskite single crystals in fields such as photoelectric sensors. Therefore, it is essential to develop a controllable growth method for perovskite single crystals in order to improve the size and reproducibility of solution-grown perovskite single crystals, reduce crystal preparation costs, improve crystal growth uniformity, and reduce defect concentration in the crystal. Summary of the Invention
[0005] To address the aforementioned problems in the existing technology, this invention provides a method for the controllable growth of perovskite single crystals based on crown ether host-guest coordination. The technical problem to be solved by this invention is achieved through the following technical solution: This invention provides a method for the controllable growth of perovskite single crystals based on crown ether host-guest coordination, comprising: Step 1: Add the perovskite raw material to an organic solvent and stir for the first time. After it is fully dissolved, add an antisolvent and stir for the second time to obtain a saturated precursor solution. Filter the saturated precursor solution and heat the filtrate to precipitate crystals to obtain perovskite seed crystals. Step 2: Fix the perovskite seed crystal onto the substrate; Step 3: Add the same perovskite raw material as used in the preparation of the perovskite seed crystal to the organic solvent, and simultaneously add crown ether. After the first stirring, and after complete dissolution, add the antisolvent and stir and filter to obtain a saturated precursor solution containing crown ether. Keep the saturated precursor solution containing crown ether at a certain temperature and then filter. Immerse the substrate with the perovskite seed crystal fixed in it into the filtrate of the saturated precursor solution containing crown ether, and grow the crystal under a temperature gradient to obtain a perovskite single crystal.
[0006] In one embodiment of the present invention, the perovskite raw material includes lead halide and halide salt; the lead halide includes at least one of PbCl2, PbBr2 and PbI2; the halide salt includes at least one of MACl, MABr, MAI, FACl, FABr, FAI, CsCl, CsBr and CsI; the molar ratio of lead halide to halide salt in the perovskite raw material is 1~2:1.
[0007] In one embodiment of the present invention, the organic solvent is at least one of dimethyl sulfoxide, N,N dimethylformamide and γ-valerolactone.
[0008] In one embodiment of the present invention, the antisolvent is at least one of methanol and cyclohexanol, and the volume ratio of the antisolvent to the organic solvent is 0 to 1:1.
[0009] In one embodiment of the present invention, the temperature of the first stirring is 50°C and the stirring time is 3-5 hours; the stirring time of the second stirring is 3-6 hours.
[0010] In one embodiment of the present invention, in step 1, the heating temperature for heating the filtrate to precipitate crystals is 50-100°C, and the heating time is 6-12 hours.
[0011] In one embodiment of the present invention, the substrate is a quartz glass sheet or a double-polished sapphire substrate with a size of 30×30×1mm.
[0012] In one embodiment of the present invention, the crown ether is any one of 15-crown ether-5, benzo-15-crown ether-5, dibenzo-15-crown ether-5, aza-15-crown ether-5, diaza-15-crown ether-5, 18-crown ether-6, benzo-18-crown ether-6, dibenzo-18-crown ether-6, aza-18-crown ether-6, diaza-18-crown ether-6, 21-crown ether-7, benzo-21-crown ether-7, dibenzo-21-crown ether-7, aza-21-crown ether-7, diaza-21-crown ether-7, 24-crown ether-8, benzo-24-crown ether-8, dibenzo-24-crown ether-8, aza-24-crown ether-8, and diaza-24-crown ether-8.
[0013] In one embodiment of the present invention, the amount of crown ether added is 8-20 mg / ml.
[0014] In one embodiment of the present invention, in step 3, the temperature of the crown ether-containing saturated precursor solution is 50°C and the holding time is 6-12h; the temperature of crystal growth is 50-80°C, the temperature gradient is 0.05-0.25°C / h, and the growth time is 14-26 days.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The controllable growth method for perovskite single crystals based on crown ether host-guest coordination of the present invention effectively reconstructs the local chemical structure of the precursor in solution through the host-guest coordination synergy of crown ether and perovskite cation, thereby improving the controllability of the crystallization process; at the same time, the combination of antisolvent-assisted strategy and seed crystal induced growth achieves effective separation of nucleation and crystal growth stages, significantly reducing the impact of random nucleation on crystal quality; in addition, the slow transport and ordered deposition of ions in solution are achieved by introducing a low-speed temperature gradient, thereby obtaining high-quality single crystal materials with low defect density and high structural uniformity.
[0016] 2. The controllable growth method for perovskite single crystals of the present invention has mild overall process conditions, good controllability of parameter windows, high repeatability, and is suitable for the controllable preparation of large-size perovskite single crystals. The obtained single crystals can be further applied to related devices such as photodetectors and X-ray imaging.
[0017] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of the present invention more apparent and understandable, preferred embodiments are described in detail below with reference to the accompanying drawings. Attached Figure Description
[0018] Figure 1This is a flowchart of a method for controllable growth of perovskite single crystals based on crown ether host-guest coordination provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of a self-designed solution crystal growth furnace; Figure 3 These are single-crystal photographs of Example 1 and Comparative Example 1; Figure 4 These are the single-crystal SEM images of Example 1 and Comparative Example 1; Figure 5 These are the single-crystal XRD patterns of Example 1 and Comparative Example 1; Figure 6 This is a single-crystal photograph of Example 2; Figure 7 These are single-crystal photographs of Example 3 and Comparative Example 2; Figure 8 This is the single-crystal XRD pattern of Example 3; Figure 9 This is a single-crystal photograph of Example 4. Detailed Implementation
[0019] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following describes in detail, with reference to the accompanying drawings and specific embodiments, a method for controllable growth of perovskite single crystals based on crown ether host-guest coordination proposed in accordance with the present invention.
[0020] The foregoing and other technical contents, features, and effects of the present invention will be clearly presented in the following detailed description of specific embodiments in conjunction with the accompanying drawings. Through the description of the specific embodiments, a more in-depth and concrete understanding can be gained of the technical means and effects adopted by the present invention to achieve its intended purpose. However, the accompanying drawings are for reference and illustration only and are not intended to limit the technical solutions of the present invention.
[0021] This invention provides a method for the controllable growth of perovskite single crystals based on the host-guest coordination of crown ethers. The core of this method lies in the introduction of crown ethers to regulate the ion coordination structure and solvation environment in the precursor solution, thereby achieving effective control over the crystal nucleation and growth process, and thus improving the quality of single crystals and the reproducibility of growth.
[0022] Please see Figure 1 , Figure 1 This is a flowchart of a method for controllable growth of perovskite single crystals based on the host-guest coordination of crown ethers, provided in an embodiment of the present invention.
[0023] like Figure 1 As shown, the controllable growth method for perovskite single crystals based on crown ether host-guest coordination in this embodiment includes the following steps: Step 1: Add the perovskite raw material to an organic solvent and stir for the first time. After it is fully dissolved, add an antisolvent and stir for the second time to obtain a saturated precursor solution. Filter the saturated precursor solution and heat the filtrate to precipitate crystals, thus obtaining perovskite seed crystals.
[0024] In this embodiment, the perovskite raw material includes lead halide and halide salt; the lead halide includes at least one of PbCl2, PbBr2 and PbI2; the halide salt includes at least one of MACl, MABr, MAI, FACl, FABr, FAI, CsCl, CsBr and CsI; the molar ratio of lead halide to halide salt in the perovskite raw material is 1~2:1.
[0025] Specifically, lead halide and halide salt are added to an organic solvent at a molar ratio of 1-2:1 and stirred for 3-5 hours at a reaction temperature of 50°C. After complete dissolution, an antisolvent is added and stirring continues for another 3-6 hours. The solution is then filtered using an organic hydrophobic filter head with a pore diameter of 0.45-0.22 μm, where the volume ratio of antisolvent to organic solvent is 0-1:1. The filtrate is then heated on a hot plate at 50-100°C for 6-12 hours to rapidly precipitate crystals. After crystal precipitation, the solution is cooled to room temperature, and 1-2 mm crystals are carefully removed with tweezers and dried with a nitrogen gun to obtain perovskite seed crystals.
[0026] Optionally, the organic solvent is at least one selected from dimethyl sulfoxide, N,N dimethylformamide, and γ-valerol. The antisolvent is at least one selected from methanol and cyclohexanol.
[0027] It is understandable that when the volume ratio of antisolvent to organic solvent is 0:1, i.e., antisolvent is not needed, such as perovskite single crystals with MA as a cation.
[0028] Step 2: Fix the perovskite seed crystal onto the substrate.
[0029] Specifically, select a square seed crystal and place it on a clean paper for later use. Then, select a square quartz glass or double-polished sapphire substrate with dimensions of 30×30×1mm. Use silicone to attach the perovskite seed crystal to the center of the substrate and wait for the silicone to dry completely to complete the preparation of the perovskite seed crystal.
[0030] Step 3: Add the same perovskite raw material as used for preparing the perovskite seed crystal to an organic solvent, add crown ether, and stir for the first time. After fully dissolving, add antisolvent and stir for the second time. Filter to obtain a saturated precursor solution containing crown ether. Keep the saturated precursor solution containing crown ether at a certain temperature and then filter. Immerse the substrate with the perovskite seed crystal fixed in it into the filtrate of the saturated precursor solution containing crown ether. Under temperature gradient conditions, crystal growth is carried out to obtain a perovskite single crystal.
[0031] Specifically, perovskite raw materials with the same composition as those used in the perovskite seed crystal preparation and a certain amount of crown ether are added to the same organic solvent used in the perovskite seed crystal preparation and stirred for 3-5 hours. The amount of crown ether added is 8-20 mg / mL, and the reaction temperature is 50°C. After thorough stirring and dissolution, an antisolvent with the same proportion as that used in the perovskite seed crystal preparation is added, and stirring is continued for another 3-6 hours. After filtration, a saturated precursor solution containing crown ether is prepared. The saturated precursor solution containing crown ether is then placed in a 50°C water bath and kept at that temperature for 6-12 hours before filtration. The substrate with the perovskite seed crystal fixed is then added to the filtrate of the saturated precursor solution containing crown ether and placed in a self-designed solution crystal growth furnace. Crystal growth is carried out at 50-80°C with a temperature gradient of 0.05-0.15°C / h. Perovskite single crystals can be obtained after 14-26 days of growth.
[0032] Please see Figure 2 , Figure 2 This is a schematic diagram of a self-designed solution crystal growth furnace. The equipment mainly consists of a temperature control system, a water tank, and a stirring system. The temperature control system uses a temperature controller; the water tank is made of high-temperature quartz, cylindrical with a wall thickness of 1.5cm and a volume of 25L; the stirring system is equipped with an electric motor to maintain a constant temperature. The temperature gradient of the self-built aqueous solution crystal growth equipment can be accurate to 0.1℃ / h, which is beneficial for single crystal growth.
[0033] In this embodiment, the crown ether is 15-crown ether-5 (15C5), benzo-15-crown ether-5 (B15C5), dibenzo-15-crown ether-5 (DB15C5), aza-15-crown ether-5 (N15C5), diaza-15-crown ether-5 (DN15C5), 18-crown ether-6 (18C6), benzo-18-crown ether-6 (B18C6), dibenzo-18-crown ether-6 (DB18C6), aza-18-crown ether-6 (N18C6), or diaza-18-crown ether-6 (DN18C5). 6) Any one of 21-crown ether-7 (21C7), benzo-21-crown ether-7 (B21C7), dibenzo-21-crown ether-7 (DB21C7), aza-21-crown ether-7 (N21C7), diaza-21-crown ether-7 (DN21C7), 24-crown ether-8 (24C8), benzo-24-crown ether-8 (B24C8), dibenzo-24-crown ether-8 (DB24C8), aza-24-crown ether-8 (N24C8), and diaza-24-crown ether-8 (DN24C8).
[0034] The controllable growth method for perovskite single crystals based on crown ether host-guest coordination in this invention can effectively control the crystal nucleation and growth process, improve single crystal quality, and enhance growth repeatability.
[0035] Specifically, firstly, crown ether molecules possess a unique negatively charged cavity structure, enabling them to interact with perovskite A-site cations (such as Cs) through their negatively charged cavities. + MA + (etc.) can selectively perform host-guest complexation, while its ether oxygen site can also interact with Pb. 2+ The precursor undergoes weak coordination. This host-guest complexation and coordination synergy can simultaneously regulate the cation activity and metal halide coordination environment in the solution phase, achieving dual regulation of the precursor's chemical state. Through this dual regulation, the effective concentration of free cations in the precursor solution is reduced, requiring precursor molecules to overcome higher energy barriers to aggregate and form critical nuclei. This effectively inhibits the rapid occurrence of disordered homogeneous nucleation in the solution, fundamentally reducing polycrystalline competitive growth and making the crystal growth process more inclined towards seed-dominated directional epitaxial growth.
[0036] Secondly, the host-guest complexation between crown ethers and A-site cations is dynamic and reversible. As solute is consumed during crystal growth, the complexation equilibrium shifts and cations are gradually released. This strategy can finely control the release rate of supersaturation in the solution, transforming the crystal growth kinetics from rapid growth with explosive nucleation to a slow and controllable diffusion growth mode, thereby significantly improving crystal size uniformity and structural integrity.
[0037] Furthermore, the regulation of the precursor coordination environment by crown ether molecules in solution can effectively reduce the probability of intrinsic defects forming during crystal growth. Simultaneously, heteroatoms (such as N and O) in crown ether molecules or their derivatives can interact with undercoordinated Pb at the crystal growth interface. 2+ Interactions at the sites enable in-situ passivation of deep-level trap states, which is beneficial for improving the carrier transport and photoelectric detection performance of the crystal.
[0038] Furthermore, the method of this invention does not rely on strong chemical reactions or complex external field conditions, and has the characteristics of being mild, scalable and universal. The growth process can be highly controllable through simple temperature gradient control, and it can be applied to a variety of halide perovskite systems. It provides a general strategy with clear mechanism and engineering operability for the controllable synthesis of high-quality large-size single crystals.
[0039] Furthermore, specific embodiments and comparative examples are provided to illustrate the performance of the method of the present invention and the perovskite single crystals prepared therefrom.
[0040] Example 1 A controllable growth method for perovskite single crystals based on crown ether host-guest coordination was proposed to prepare CsPbBr3 single crystals with a growth cycle of 21 days. The specific steps are as follows: (1) Weigh PbBr2 and CsBr in a molar ratio of 2:1 into clean glass bottles, where PbBr2 is 1.4M and CsBr is 0.7M (M is the concentration unit, mol / L). Use a pipette to add 20 mL of dimethyl sulfoxide (DMSO) into the bottle, add a magnet, and seal the bottle. Place the bottle on a 50°C water bath and stir for 3 hours. After the raw materials are fully dissolved, add 5 mL of methanol (MeOH) and stir for another 3 hours. Then filter the solution using a 0.22 μm diameter PTFE (polytetrafluoroethylene) filter head. Finally, place the filtered solution on a hot plate and heat it from 50°C to 80°C for 12 hours.
[0041] (2) After 12 hours, remove the bottle and allow it to cool to room temperature. Use tweezers to remove the square seed crystal and dry it with a nitrogen gun for later use. Select a double-polished sapphire substrate with a size of 30×30×1mm, ultrasonically clean it with deionized water for 30 minutes, and then dry it with a nitrogen gun for later use. Then, use silicone to attach the seed crystal to the center of the sapphire substrate and wait for the silicone to dry completely to complete the seed crystal preparation.
[0042] (3) Weigh out PbBr2 and CsBr in a molar ratio of 2:1 and place them in a clean glass bottle, where PbBr2 is 1.4M and CsBr is 0.7M. Use a pipette to add 20mL of DMSO to the bottle, add 18C6 solution with a concentration of 12mg / mL, add a magnet, and seal the bottle. Place the bottle on a 50°C water bath and stir for 5h. After the raw materials are fully dissolved, add 5mL of MeOH and stir for another 6h. Filter the solution using a 0.22μm diameter PTFE filter. Finally, keep the filtered solution at 50°C for 6h and then filter again. After filtration, add seed crystals and place the solution in a crystal growth furnace. Use a reverse temperature crystallization method with a growth gradient of 0.083°C / h. After 21 days of growth, 18C6-assisted CsPbBr3 single crystals can be obtained.
[0043] Example 2 A controllable growth method for perovskite single crystals based on crown ether host-guest coordination was proposed to prepare CsPbBr3 single crystals with a growth cycle of 18 days. The specific steps are as follows: (1) The seed crystal preparation method is the same as steps (1)-(2) in Example 1, and will not be repeated here.
[0044] (2) Weigh PbBr2 and CsBr in a molar ratio of 2:1 into clean glass bottles, where PbBr2 is 1.4M and CsBr is 0.7M. Add 20mL of DMSO to the bottle using a pipette, add B18C6 (benzo-18-crown ether-6) with a concentration of 8mg / mL, add a magnet, and seal the bottle. Place the bottle on a 50°C water bath and stir for 5h. After the raw materials are fully dissolved, add 5mL of MeOH and stir for another 6h. Filter the solution using a 0.22μm diameter PTFE filter. Finally, keep the filtered solution at 50°C for 6h and then filter again. After filtration, add seed crystals and place the solution in a crystal growth furnace. Use a reverse temperature crystallization method with a growth gradient of 0.01°C / h. After 18 days of growth, CsPbBr3 single crystals assisted by B18C6 can be obtained.
[0045] Example 3 A controllable growth method for perovskite single crystals based on crown ether host-guest coordination was proposed to prepare MAPbBr3 single crystals with a growth cycle of 18 days. The specific steps are as follows: (1) Weigh out PbBr2 and MABr in a 1:1 molar ratio and place them in a clean glass bottle. Both PbBr2 and MABr are 1.8M. Use a pipette to add 20mL of N,N-dimethylformamide (DMF) to the bottle, add a magnet, and seal the bottle. Place the bottle on a 50°C water bath and stir for 5 hours. After the raw materials are fully dissolved, filter the solution using a 0.22μm diameter PTFE filter. Finally, place the filtered solution on a hot plate and heat it from 50°C to 80°C for 6 hours.
[0046] (2) After 6 hours, remove the bottle and allow it to cool to room temperature. Use tweezers to remove the square seed crystal and dry it with a nitrogen gun for later use. Select a double-polished sapphire substrate with a size of 30×30×1mm, ultrasonically clean it with deionized water for 30 minutes, and then dry it with a nitrogen gun for later use. Then, use silicone to attach the seed crystal to the center of the sapphire substrate and wait for the silicone to dry completely to complete the seed crystal preparation.
[0047] (3) Weigh out PbBr2 and MABr in a 1:1 molar ratio and place them in a clean glass bottle. Both PbBr2 and MABr are 1.85M. Use a pipette to add 20mL of DMF to the bottle, add 16mg / mL of 18C6, add a magnet, and seal the bottle. Place the bottle on a 50°C water bath and stir for 6 hours. Then filter using a 0.22μm diameter PTFE filter. Finally, place the filtered solution on a 50°C hot plate for 10 hours and filter again. After filtration, add seed crystals and place the solution in a crystal growth furnace. Use the reverse temperature crystallization method with a growth gradient of 0.0125°C / h. After 18 days of growth, MAPbBr3 single crystals with 18C6 assistance can be obtained.
[0048] Example 4 A controllable growth method for perovskite single crystals based on crown ether host-guest coordination was proposed to prepare MAPbCl3 single crystals with a growth cycle of 25 days. The specific steps are as follows: (1) Weigh out PbCl2 and MACl in a 1:1 molar ratio and place them in a clean glass bottle, with each PbCl2 and MACl being 1.5M. Use a pipette to add 10 mL of LDMF and 10 mL of DMSO to the bottle, add a magnet, and seal the bottle. Place the bottle on a 50°C water bath and stir for 3 hours. After the raw materials are fully dissolved, filter the solution using a 0.22 μm diameter PTFE filter. Finally, place the filtered solution on a hot plate and heat it from 50°C to 70°C for 4 hours.
[0049] (2) After 4 hours, remove the bottle and allow it to cool to room temperature. Use tweezers to remove the square seed crystal and dry it with a nitrogen gun for later use. Select a double-polished sapphire substrate with a size of 30×30×1mm, ultrasonically clean it with deionized water for 30 minutes, and then dry it with a nitrogen gun for later use. Then use silicone to attach the seed crystal to the center of the sapphire substrate and wait for the silicone to dry completely to complete the seed crystal preparation.
[0050] (3) Weigh out PbCl2 and MACl in a 1:1 molar ratio and place them in a clean glass bottle. Both PbCl2 and MACl are 1.5M. Use a pipette to add 10mL of LDMF and 10mL of DMSO to the bottle, respectively. Add 18C6 solution with a concentration of 10mg / mL, add a magnet, and seal the bottle. Place the bottle on a 50°C water bath and stir for 3 hours. Then filter the solution using a 0.22μm diameter PTFE filter. Finally, place the filtered solution on a 50°C hot plate for 12 hours and filter again. After filtration, add seed crystals and place the solution in a crystal growth furnace. Use a reverse temperature crystallization method with a growth gradient of 0.083°C / h. After 25 days of growth, MAPbCl3 single crystals with 18C6-assisted growth can be obtained.
[0051] Comparative Example 1 The difference from Example 1 is that 18C6 is not added in step (3), and the other conditions are exactly the same as in Example 1, resulting in CsPbBr3 single crystal without 18C6 addition.
[0052] Comparative Example 2 The difference from Example 3 is that 18C6 is not added in step (3), and the other conditions are exactly the same as in Example 3, resulting in MAPbBr3 single crystal without 18C6 addition.
[0053] The CsPbBr3 single crystals obtained in Example 1 and Comparative Example 1 were compared. The comparison results are shown in [link to comparison]. Figures 3-5 . Figure 3These are single-crystal photographs of Example 1 (Figure (b)) and Comparative Example 1 (Figure (a)). Figure 4 These are the single-crystal SEM images of Example 1 (Figure (b)) and Comparative Example 1 (Figure (a)). Figure 5 These are the single-crystal XRD patterns of Example 1 and Comparative Example 1. From... Figure 3 It can be seen that the addition of 18C6 additive suppressed disordered impurities in the perovskite solution, resulting in larger and brighter single crystals. Figure 4 It can be seen that the surface of the single crystal grown with 18C6 assistance is smoother and without grooves. From Figure 5 It can be seen that diffraction peaks appeared in the spectra of all samples, but no diffraction peaks of other substances were present in the diffraction pattern of the 18C6-assisted growth single crystal, indicating that CsPbBr3 has good crystallization performance and high purity. This further indicates that crown ethers can achieve controllable growth of perovskite single crystals through host-guest coordination.
[0054] Please see Figure 6 , Figure 6 This is a single-crystal photograph from Example 2. From Figure 6 It can be seen that high-quality, large-size CsPbBr3 single crystals can also be prepared using B18C6.
[0055] Please see Figure 7 and Figure 8 , Figure 7 These are single-crystal photographs of Example 3 (Figure (b)) and Comparative Example 2 (Figure (a)); Figure 8 This is the single-crystal XRD pattern of Example 3. From... Figure 7 As can be seen, MAPbBr3 single crystals grown from 18C6 have a bright, defect-free surface, resulting in crystals of superior quality and larger size. Figure 8 This further demonstrates that crown ethers can enable the controllable growth of perovskite single crystals.
[0056] Please see Figure 9 , Figure 9 This is a single-crystal photograph of Example 4. Figure 9 This indicates that the method of the present invention is also applicable to the controlled growth of chloride-based perovskite single crystals.
[0057] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations are intended to cover non-exclusive inclusion, such that an article or device comprising a list of elements includes not only those elements but also other elements not expressly listed. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the article or device comprising said element. Terms such as "connected" or "linked" are not limited to physical or mechanical connections but can include electrical connections, whether direct or indirect. The orientations or positional relationships indicated by terms such as "upper," "lower," "left," and "right" are based on the orientations or positional relationships shown in the accompanying drawings and are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be construed as limiting the invention.
[0058] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features or characteristics described may be combined in any suitable manner in one or more embodiments or examples. In addition, those skilled in the art can combine and integrate the different embodiments or examples described in this specification.
[0059] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention.
Claims
1. A method for controllable growth of perovskite single crystals based on crown ether host-guest coordination, characterized in that, include: Step 1: Add the perovskite raw material to an organic solvent and stir for the first time. After it is fully dissolved, add an antisolvent and stir for the second time to obtain a saturated precursor solution. Filter the saturated precursor solution and heat the filtrate to precipitate crystals to obtain perovskite seed crystals. Step 2: Fix the perovskite seed crystal onto the substrate; Step 3: Add the same perovskite raw material as used in the preparation of the perovskite seed crystal to the organic solvent, and simultaneously add crown ether. After the first stirring, and after complete dissolution, add the antisolvent and stir and filter to obtain a saturated precursor solution containing crown ether. Keep the saturated precursor solution containing crown ether at a certain temperature and then filter. Immerse the substrate with the perovskite seed crystal fixed in it into the filtrate of the saturated precursor solution containing crown ether, and grow the crystal under a temperature gradient to obtain a perovskite single crystal.
2. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, The perovskite raw material includes lead halides and halide salts; the lead halides include at least one of PbCl2, PbBr2, and PbI2; the halide salts include at least one of MACl, MABr, MAI, FACl, FABr, FAI, CsCl, CsBr, and CsI; the molar ratio of lead halides to halide salts in the perovskite raw material is 1~2:
1.
3. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, The organic solvent is at least one of dimethyl sulfoxide, N,N dimethylformamide, and γ-valerolactone.
4. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, The antisolvent is at least one of methanol and cyclohexanol, and the volume ratio of the antisolvent to the organic solvent is 0 to 1:
1.
5. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, The temperature for the first stirring is 50°C, and the stirring time is 3-5 hours; the stirring time for the second stirring is 3-6 hours.
6. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, In step 1, the heating temperature for precipitating crystals by heating the filtrate is 50-100°C, and the heating time is 6-12 hours.
7. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, The substrate is a quartz glass sheet or a double-polished sapphire substrate with dimensions of 30×30×1mm.
8. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, The crown ether is any one of 15-crown ether-5, benzo-15-crown ether-5, dibenzo-15-crown ether-5, aza-15-crown ether-5, diaza-15-crown ether-5, 18-crown ether-6, benzo-18-crown ether-6, dibenzo-18-crown ether-6, aza-18-crown ether-6, diaza-18-crown ether-6, 21-crown ether-7, benzo-21-crown ether-7, dibenzo-21-crown ether-7, aza-21-crown ether-7, diaza-21-crown ether-7, 24-crown ether-8, benzo-24-crown ether-8, dibenzo-24-crown ether-8, aza-24-crown ether-8, and diaza-24-crown ether-8.
9. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, The amount of crown ether added is 8-20 mg / ml.
10. The method for controllable growth of perovskite single crystals based on crown ether host-guest coordination according to claim 1, characterized in that, In step 3, the temperature of the crown ether-containing saturated precursor solution is 50°C and the holding time is 6-12h; the crystal growth temperature is 50-80°C, the temperature gradient is 0.05-0.25°C / h, and the growth time is 14-26 days.