A device for purifying and growing quartz sand by shoveling and its crystal growth process
By using plasma heating and single-crystal quartz sheet induction, the problem of hydroxyl contamination in traditional quartz sand agglomeration has been solved, enabling the production of low-hydroxyl single-crystal quartz crystals suitable for high-end applications.
Patent Information
- Application Number
- CN202611542501.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-07
- Publication Date
- 2026-11-17
AI Technical Summary
In the traditional quartz sand agglomeration process, the high-temperature melting of the oxyhydrogen flame results in a high hydroxyl content in the quartz agglomerate, which lowers the softening point and makes it difficult to meet the requirements of high-end applications.
High-temperature molten silica sand is generated by plasma heating, and a bottom monocrystalline silica sheet is used to induce the molten silica sand to form a monocrystalline arrangement, avoiding the introduction of hydroxyl groups by the hydrogen-oxygen flame. At the same time, a ceramic insulation layer is used to reduce heat loss.
To obtain single-crystal quartz crystals with low hydroxyl content, high softening point, and good temperature resistance, which meet the application requirements of high-end industries such as semiconductors.
Smart Images

Figure CN123108720A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of quartz sand purification and crystal growth technology, and specifically relates to a quartz sand purification and crystal growth device and its crystal growth process. Background Technology
[0002] Traditional quartz sand agglomeration process uses an oxyhydrogen flame to melt quartz sand at high temperatures. The hydrogen and water vapor in the flame enter the quartz melt, causing a significant increase in the hydroxyl (-OH) content of the quartz agglomerate, a decrease in the softening point, and a deterioration in temperature resistance, making it difficult to meet the requirements of high-end applications such as semiconductors.
[0003] For example, in the prior art, there is a manufacturing apparatus and method for quartz ingots published under CN114195367A. In this scheme, an oxyhydrogen flame burner forms a high-temperature melting zone in the furnace. Quartz material enters the melting zone from the feed pipe and is sprayed onto a uniformly rotating target to be deposited and formed. The above method uses an oxyhydrogen flame as a heat source. Therefore, the quartz ingot has a high hydroxyl content and is deposited in a glassy state, which is not suitable for high-end industry applications.
[0004] To address the aforementioned issues, the applicant proposed an improved purification and crystal growth process. This process utilizes plasma to generate high-temperature molten quartz sand, and simultaneously uses a bottom monocrystalline quartz sheet to induce the molten quartz sand to form monocrystalline arrangements, thereby obtaining monocrystalline quartz crystals. This solution combines the effects of purification, monocrystalline formation, and low hydroxyl content. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a device for purifying and growing quartz sand by agglomeration. This process uses plasma to generate high-temperature molten quartz sand, and the heat source does not contain hydrogen or oxygen, thus avoiding the formation of hydroxyl groups from the source. At the same time, it uses bottom single-crystal quartz sheets to induce the molten quartz sand to form single crystals, thereby obtaining single-crystal quartz crystals. This solution has the three effects of purification, single crystallization and low hydroxyl groups.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] A device for purifying and growing quartz sand by agglomeration includes a fixed platform, a support plate, and a motor. The fixed platform has legs at its bottom and through holes. The support plate has a ceramic insulation layer for placing seed crystals. A sleeve is provided at the bottom of the support plate, and a key block is provided on the inner wall of the sleeve. The motor is fixed to the bottom of the fixed platform. The motor shaft passes through the through holes and is inserted into the sleeve. The motor shaft has a keyway that fits into the key block inside the sleeve to form a spline structure. A support column is provided at the bottom of the support plate, and a ball head is provided at the bottom of the support column. The ball head abuts against the fixed platform to support the support plate and improve stability during rotation. The motor drives the support plate to rotate.
[0008] Quartz sand is scattered onto the surface of the seed crystal through an externally installed feed end, and then the quartz sand on the seed crystal is heated and melted by an externally installed plasma heater.
[0009] Furthermore, the ceramic insulation layer of the support plate is equipped with an installation ring for limiting and stabilizing the seed crystals.
[0010] Furthermore, a limiting ring is also provided on the fixed platform. The limiting ring is located around the support column to stabilize the rotation of the support column.
[0011] Furthermore, a protective cover is provided on the outside of the motor to protect it.
[0012] A process for purifying and growing crystals from quartz sand by agglomeration, the specific steps of which are as follows:
[0013] S1: Raw Material Preparation
[0014] (1) Material selection: Select quartz sand with a purity of 2N to 6N as raw material, remove obvious impurities and foreign matter, and ensure that the raw material batches are consistent;
[0015] (2) Screening: The quartz sand is classified according to the process requirements to ensure that the raw material has a uniform particle size, which is conducive to uniform melting in the later stage;
[0016] (3) Impurity removal: The quartz sand is subjected to impurity removal treatments such as magnetic separation or acid washing to reduce the content of metal impurities and ensure the purity of the finished product;
[0017] (4) Drying: Dry the treated quartz sand thoroughly to remove surface moisture and prevent moisture from forming bubbles or introducing hydroxyl groups when melting at high temperature;
[0018] (5) Reserve: Store the dried quartz sand in a sealed container to prevent it from getting damp again.
[0019] S2: Seed Placement
[0020] (1) Seed preparation: Select a single crystal quartz sheet with a purity of 6N as the seed crystal and check its surface flatness and integrity;
[0021] (2) Laying and fixing: Lay the single crystal quartz sheet horizontally at the bottom of the melting station as a seed substrate to guide the arrangement of single crystals, ensuring that the crystal face is facing up and the position is centered and stable;
[0022] (3) Setting of heat insulation layer: A ceramic heat insulation layer is set around the seed crystal and melting area to reduce heat loss and maintain a stable melting temperature field.
[0023] S3: Plasma heating melting
[0024] (1) Equipment start-up: Turn on the plasma heater to ionize the working gas and generate plasma at a temperature of 2800-3000℃;
[0025] (2) Temperature control: Raise the temperature of the melting zone to the quartz melting temperature, >1710℃, to ensure that the quartz sand is fully melted;
[0026] (3) Feeding and melting: The dried quartz sand is continuously fed into the high-temperature melting zone at a rate of 5.5-6 kg / min, and the quartz sand melts rapidly under the high temperature of the plasma;
[0027] (4) Spreading and contact: Under the action of gravity and airflow, the molten quartz powder and quartz sand are evenly contacted and spread on the bottom single crystal quartz sheet.
[0028] S4: Seed-guided crystal growth
[0029] (1) Oriented arrangement: After fused quartz powder and quartz sand come into contact on the surface of a single crystal quartz sheet, they generate a single crystal arrangement with the seed lattice as a template, transforming from a polycrystalline state to a single crystal state;
[0030] (2) Crystal orientation control: Combining the principles of physical crystal growth and crystal orientation crystal growth process, the solid-liquid interface is controlled to move along a defined crystal orientation, so that the quartz can grow continuously along the seed crystal orientation; as the crystal growth proceeds slowly, the quartz sand feed end and the plasma heater are raised synchronously, and the whole process is controlled by the PLC program.
[0031] (3) Single crystal formation: As molten quartz is continuously supplied and cooled to crystallize, a complete single crystal quartz structure is formed.
[0032] S5: Rotational forming
[0033] (1) Rotation drive: The motor drives the rotation mechanism to rotate at a speed of 90-120 r / min / min, preferably 110 r / min, so that the molten quartz is evenly distributed under the action of centrifugation and flow;
[0034] (2) Molding control: The diameter of the quartz mass is gradually increased to 400 mm by rotating and continuously supplying molten quartz;
[0035] (3) Growth monitoring: Control the rotation speed, feed rate and temperature to maintain the regular shape and dense internal structure of the quartz block.
[0036] S6: Cooling and Post-treatment
[0037] (1) Slow cooling in the furnace: The quartz block after molding is slowly cooled in the furnace to eliminate internal stress and prevent cracking;
[0038] (2) Cooling control: Control the cooling rate and temperature gradient to avoid rapid cooling that could cause the quartz block to crack or produce internal defects;
[0039] Specifically, the formed quartz blocks are slowly cooled in the furnace: first, the furnace temperature is lowered to 1200-1250℃ at 40-60℃ / h and held for 3-5 hours for annealing; then, the temperature is slowly lowered to 1000℃ at 10-15℃ / h; then lowered to 700℃ at 15-25℃ / h; and finally lowered to 350℃ at 30-40℃ / h before being naturally cooled in the furnace until the furnace temperature is below 200℃ before being removed from the furnace to eliminate internal stress and prevent cracking.
[0040] (3) Inspection: The appearance, size and internal quality of the cooled quartz block are inspected to confirm the single crystal structure and low hydroxyl index;
[0041] (4) Post-processing: Cutting, purification and other post-processing steps are carried out as needed to obtain finished single crystal quartz.
[0042] The advantages of this invention compared to existing technologies are as follows:
[0043] 1) This process utilizes the principle of plasma heating to generate high-temperature melting of quartz sand. Since plasma heating can generate temperatures up to approximately 3000℃, it can fully melt the quartz sand. At the same time, because plasma heating does not contain hydrogen or oxygen, it avoids the introduction of hydroxyl groups during the melting process. Therefore, it eliminates the problem of direct contamination by hydroxyl groups caused by hydrogen-oxygen flame agglomeration, thus reducing the degree of hydroxyl contamination. As a result, the obtained quartz crystals have low hydroxyl content, high softening point, and good temperature resistance, meeting the application requirements of high-end industries such as semiconductors.
[0044] 2) The principle of seed-guided monocrystalline formation can be used to purify quartz sand by growing crystals. Through the seed-guided effect of the bottom monocrystalline quartz sheet, the molten quartz sand is arranged into monocrystalline quartz crystals, which is significantly different from the polycrystalline and glassy quartz agglomerates formed by traditional agglomeration. Taking 2N-6N quartz sand raw material as an example, quartz purification can be achieved during plasma high-temperature melting and seed-guided crystallization to obtain high-purity monocrystalline quartz. For example, if a 6N monocrystalline crystal is used as the seed, it will grow into a 6N quartz agglomerate.
[0045] 3) Using a ceramic insulation layer can reduce heat loss and help maintain a stable melting temperature field; Attached Figure Description
[0046] Appendix Figure 1 This is a schematic diagram of the structure of a quartz sand purification and crystal growth device according to the present invention.
[0047] Appendix Figure 2 This is a schematic diagram of the structure of a quartz sand purification and crystal growth device according to the present invention.
[0048] Appendix Figure 3 This is a simplified view of a quartz sand purification and crystal growth process according to the present invention.
[0049] In the figure: 1. Fixed platform; 101. Through hole; 2. Support leg; 3. Limiting ring; 4. Support plate; 401. Sleeve; 5. Ceramic insulation layer; 51. Mounting ring; 6. Support column; 61. Ball head; 7. Motor; 71. Protective cover; 8. Feed end; 9. Plasma heater; 10. Seed crystal. Detailed Implementation
[0050] To facilitate understanding by those skilled in the art, the following is a detailed explanation in conjunction with the appendix. Figure 1-3 The technical solution of the present invention will be further described in detail below.
[0051] Example 1:
[0052] A device for purifying and growing quartz sand by agglomeration includes a fixed platform 1, a support plate 4, and a motor 7. The fixed platform 1 has legs 2 at its bottom and a through hole 101. The support plate 4 has a ceramic insulation layer 5 for placing seed crystals 10. The bottom of the support plate 4 has a sleeve 401 with a key block on its inner wall. The motor 7 is fixed to the bottom of the fixed platform 1. The motor 7 shaft passes through the through hole 101 and is inserted into the sleeve 401. The motor 7 shaft has a keyway that fits into the key block inside the sleeve 401 to form a spline structure. The bottom of the support plate 4 has a support column 6 with a ball head 61 at its bottom end. The ball head 61 abuts against the fixed platform 1 to support the support plate 4 and improve stability during rotation.
[0053] The motor 7 drives the support plate 4 to rotate; the quartz sand is scattered onto the surface of the seed crystal 10 through the externally set feed end 8, and then the quartz sand on the seed crystal 10 is heated and melted by the externally set plasma heater 9.
[0054] Furthermore, the ceramic insulation layer 5 of the support plate 4 is provided with an installation ring 51 for limiting and stabilizing the seed crystal 10.
[0055] Furthermore, the fixed platform 1 is also provided with a limiting ring 3, which is located around the support column 6 to stabilize the rotation of the support column 6.
[0056] Furthermore, a protective cover 71 is provided on the outside of the motor 7 to protect the motor 7.
[0057] A process for purifying and growing crystals from quartz sand by agglomeration, the specific steps of which are as follows:
[0058] S1: Raw Material Preparation
[0059] (1) Material selection: Select 2N purity quartz sand as raw material, remove obvious impurities and foreign matter, and ensure that the raw material batches are consistent;
[0060] (2) Screening: The quartz sand is classified according to the process requirements to ensure that the raw material has a uniform particle size, which is conducive to uniform melting in the later stage;
[0061] (3) Impurity removal: The quartz sand is subjected to impurity removal treatments such as magnetic separation or acid washing to reduce the content of metal impurities and ensure the purity of the finished product;
[0062] (4) Drying: Dry the treated quartz sand thoroughly to remove surface moisture and prevent moisture from forming bubbles or introducing hydroxyl groups when melting at high temperature;
[0063] (5) Reserve: Store the dried quartz sand in a sealed container to prevent it from getting damp again.
[0064] S2: Seed Placement
[0065] (1) Seed preparation: Select a single crystal quartz sheet with a purity of 6N as the seed crystal and check its surface flatness and integrity;
[0066] (2) Laying and fixing: Lay the single crystal quartz sheet horizontally at the bottom of the melting station as a seed substrate to guide the arrangement of single crystals, ensuring that the crystal face is facing up and the position is centered and stable;
[0067] (3) Setting of heat insulation layer: A ceramic heat insulation layer is set around the seed crystal and melting area to reduce heat loss and maintain a stable melting temperature field.
[0068] S3: Plasma heating melting
[0069] (1) Equipment start-up: Turn on the plasma heater to ionize the working gas and generate plasma at a temperature of 2900℃;
[0070] (2) Temperature control: Raise the temperature of the melting zone to the quartz melting temperature, 1730°C, to ensure that the quartz sand is fully melted;
[0071] (3) Feeding and melting: The dried quartz sand is continuously fed into the high-temperature melting zone at a rate of 6 kg / min, and the quartz sand melts rapidly under the high temperature of the plasma;
[0072] (4) Spreading and contact: Under the action of gravity and airflow, the molten quartz powder and quartz sand are evenly contacted and spread on the bottom single crystal quartz sheet.
[0073] S4: Seed-guided crystal growth
[0074] (1) Oriented arrangement: After fused quartz powder and quartz sand come into contact on the surface of a single crystal quartz sheet, they generate a single crystal arrangement with the seed lattice as a template, transforming from a polycrystalline state to a single crystal state;
[0075] (2) Crystal orientation control: Combining the principles of physical crystal growth and crystal orientation crystal growth process, the solid-liquid interface is controlled to move along a defined crystal orientation, so that the quartz can grow continuously along the seed crystal orientation; as the crystal growth proceeds slowly, the quartz sand feed end and the plasma heater are raised synchronously, and the whole process is controlled by the PLC program.
[0076] (3) Single crystal formation: As molten quartz is continuously supplied and cooled to crystallize, a complete single crystal quartz structure is formed.
[0077] S5: Rotational forming
[0078] (1) Rotation drive: The motor drives the rotation mechanism to rotate at a speed of 110 r / min / minute, so that the molten quartz is evenly distributed under the action of centrifugation and flow;
[0079] (2) Molding control: The diameter of the quartz mass is gradually increased to 400 mm by rotating and continuously supplying molten quartz;
[0080] (3) Growth monitoring: Control the rotation speed, feed rate and temperature to maintain the regular shape and dense internal structure of the quartz block.
[0081] S6: Cooling and Post-treatment
[0082] (1) Slow cooling in the furnace: The quartz block after molding is slowly cooled in the furnace to eliminate internal stress and prevent cracking;
[0083] (2) Cooling control: Control the cooling rate and temperature gradient to avoid rapid cooling that could cause the quartz block to crack or produce internal defects;
[0084] Specifically, the formed quartz blocks are slowly cooled in the furnace: first, the furnace temperature is lowered to 1230℃ at 50℃ / h and held for 4 hours for annealing; then, the temperature is slowly lowered to 1000℃ at 13℃ / h; then lowered to 700℃ at 20℃ / h; and finally lowered to 350℃ at 35℃ / h before being naturally cooled in the furnace until the furnace temperature is below 200℃ before being removed from the furnace to eliminate internal stress and prevent cracking.
[0085] (3) Inspection: The appearance, size and internal quality of the cooled quartz block are inspected to confirm the single crystal structure and low hydroxyl index;
[0086] (4) Post-processing: Cutting, purification and other post-processing steps are carried out as needed to obtain finished single crystal quartz.
[0087] The device is powered by an external power source and achieves coordinated operation between various mechanical components based on the existing PLC controller and the adapted control program and programming logic sequence.
[0088] Example 2: The difference from Example 1 is that...
[0089] Step S6: Cooling and post-processing. The quartz block formed in step (2) is slowly cooled in the furnace: first, the furnace temperature is reduced to 1210℃ at 40℃ / h and held for 3h for annealing; then, the temperature is slowly reduced to 1000℃ at 12℃ / h; then reduced to 700℃ at 15℃ / h; and then reduced to 350℃ at 30℃ / h before being naturally cooled in the furnace until the furnace temperature is below 200℃ before being taken out of the furnace to eliminate internal stress and prevent cracking.
[0090] Example 3: The difference compared to Example 1 is that...
[0091] Step S6: Cooling and post-processing. The quartz block formed in step (2) is slowly cooled in the furnace: first, the furnace temperature is reduced to 1250℃ at 60℃ / h and held for 5h for annealing; then, the temperature is slowly reduced to 1000℃ at 15℃ / h; then reduced to 700℃ at 125℃ / h; and then reduced to 350℃ at 40℃ / h before being naturally cooled in the furnace until the furnace temperature is below 200℃ before being taken out of the furnace to eliminate internal stress and prevent cracking.
[0092] In the description of this invention, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," "outer," "front end," "rear end," "head," "tail," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0093] In the description of this invention, the connection methods are divided into fixed connection and movable connection. Fixed connection methods include, but are not limited to, welding and bolting. Movable connection methods include, but are not limited to, sliding connection, rotating connection, and threaded connection. The connection method to achieve the desired effect should be selected according to the application of the solution. Washers are provided in the connection process of the bolts, fixing bolts, studs and nuts. At the same time, the connection of the bolts, fixing bolts, studs and nuts is fixed by thread locking.
[0094] In summary, the electronic or electrical components, including but not limited to motors and controllers, are existing components that are custom-made or purchased. The electrical connections between these components are conventional circuit or electrical connections in the prior art and are not within the scope of protection of this invention. The coordinated operation between these components is achieved based on existing controllers and adapted control programs and programming logic sequences. The aforementioned control programs are not within the scope of protection of this invention.
[0095] In summary, including but not limited to motors, controllers, and other power systems, as well as the transmission systems output by their respective power systems, protective covers should be provided according to the actual installation location if necessary, and sealing rings should be provided at the relative rotating connections to prevent wear or damage to the power system and transmission system caused by the external environment, and to further ensure the normal operation of the power system and transmission system.
[0096] The "automation" created by this invention does not rely on sensors, but is based on mechanical timing or stroke control. The actions of each mechanism can be automatically executed by the programmable controller and programming logic in a pre-set time sequence. Those skilled in the art know that this control method based on timing and stroke position switches is a mature automation technology, and the automated operation created by this invention can be achieved without sensors.
[0097] The above description is merely an example and illustration of the structure of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the structure of the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
Claims
1. A device for purifying and growing quartz sand by agglomeration, comprising a fixed platform, a support plate, and a motor, characterized in that... The fixed platform has legs at its bottom and through holes on its surface. A ceramic insulation layer is provided on the support plate for placing seed crystals. A sleeve is located at the bottom of the support plate, and a key block is provided on the inner wall of the sleeve. The motor is fixed to the bottom of the fixed platform. The motor shaft passes through the through holes and is inserted into the sleeve. A keyway on the motor shaft fits into the key block inside the sleeve, forming a spline structure. A support column is located at the bottom of the support plate, and a ball head is located at the bottom end of the support column. The ball head abuts against the fixed platform to support the support plate and improve stability during rotation. The motor drives the support plate to rotate. Quartz sand is scattered onto the surface of the seed crystal through an externally installed feed end, and then the quartz sand on the seed crystal is heated and melted by an externally installed plasma heater.
2. The device for purifying and growing quartz sand by agglomeration as described in claim 1, characterized in that... The ceramic insulation layer of the support plate is equipped with mounting rings for limiting and stabilizing the seed crystals; The fixed platform is also provided with a limiting ring, which is located around the support column to stabilize the rotation of the support column; The motor is equipped with a protective cover on its outside to protect it.
3. A process for purifying and growing crystals from quartz sand by agglomeration, characterized in that... The specific steps are as follows: S1: Raw Material Preparation (1) Material selection: Select quartz sand with a purity of 2N to 6N as raw material, remove obvious impurities and foreign matter, and ensure that the raw material batches are consistent; (2) Screening: The quartz sand is classified according to the process requirements to ensure that the raw material has a uniform particle size, which is conducive to uniform melting in the later stage; (3) Impurity removal: The quartz sand is subjected to impurity removal treatments such as magnetic separation or acid washing to reduce the content of metal impurities and ensure the purity of the finished product; (4) Drying: Dry the treated quartz sand thoroughly to remove surface moisture and prevent moisture from forming bubbles or introducing hydroxyl groups when melting at high temperature; (5) Reserve: Store the dried quartz sand in a sealed container to prevent it from getting damp again; S2: Seed Placement (1) Seed preparation: Select a single crystal quartz sheet with a purity of 6N as the seed crystal and check its surface flatness and integrity; (2) Laying and fixing: Lay the single crystal quartz sheet horizontally at the bottom of the melting station as a seed substrate to guide the arrangement of single crystals, ensuring that the crystal face is facing up and the position is centered and stable; (3) Insulation layer setting: A ceramic insulation layer is set around the seed crystal and melting area to reduce heat loss and maintain a stable melting temperature field; S3: Plasma heating melting (1) Equipment start-up: Turn on the plasma heater to ionize the working gas and generate plasma at a temperature of 2800-3000℃; (2) Temperature control: Raise the temperature of the melting zone to the quartz melting temperature, >1710℃, to ensure that the quartz sand is fully melted; (3) Feeding and melting: The dried quartz sand is continuously fed into the high-temperature melting zone at a rate of 5.5-6 kg / min, and the quartz sand melts rapidly under the high temperature of the plasma; (4) Spreading and contact: Under the action of gravity and airflow, the molten quartz powder and quartz sand are evenly contacted and spread on the bottom single crystal quartz sheet; S4: Seed-guided crystal growth (1) Oriented arrangement: After fused quartz powder and quartz sand come into contact on the surface of a single crystal quartz sheet, they generate a single crystal arrangement with the seed lattice as a template, transforming from a polycrystalline state to a single crystal state; (2) Crystal orientation control: Combining the principles of physical crystal growth and crystal orientation crystal growth process, the solid-liquid interface is controlled to move along a defined crystal orientation, so that the quartz can grow continuously along the seed crystal orientation; as the crystal growth proceeds slowly, the quartz sand feed end and the plasma heater are raised synchronously, and the whole process is controlled by the PLC program. (3) Single crystal formation: As molten quartz is continuously supplied and cooled to crystallize, a complete single crystal quartz structure is formed; S5: Rotational forming (1) Rotation drive: The motor drives the rotation mechanism to rotate at a speed of 90-120 r / min / minute, so that the molten quartz is evenly distributed under the action of centrifugation and flow; (2) Molding control: The diameter of the quartz mass is gradually increased to 400 mm by rotating and continuously supplying molten quartz; (3) Growth monitoring: Control the rotation speed, feed rate and temperature to maintain the regular shape and dense internal structure of the quartz mass; S6: Cooling and Post-treatment (1) Slow cooling in the furnace: The quartz block after molding is slowly cooled in the furnace to eliminate internal stress and prevent cracking; (2) Cooling control: Control the cooling rate and temperature gradient to avoid rapid cooling that could cause the quartz block to crack or produce internal defects; (3) Inspection: The appearance, size and internal quality of the cooled quartz block are inspected to confirm the single crystal structure and low hydroxyl index; (4) Post-processing: Cutting, purification and other post-processing steps are carried out as needed to obtain finished single crystal quartz.
4. The process for purifying and growing quartz sand by agglomeration according to claim 3, characterized in that... Step S5: During rotational forming: (1) Rotation drive: The motor drives the rotation mechanism to rotate at a constant speed of 110 r / min.
5. The process for purifying and growing quartz sand by agglomeration according to claim 3, characterized in that... Step S6: Cooling and post-processing (2) Cooling control: Specifically, the quartz block after molding is slowly cooled in the furnace: first, the furnace temperature is reduced to 1200-1250℃ at 40-60℃ / h and held for 3-5h for annealing; then, the temperature is slowly reduced to 1000℃ at 10-15℃ / h; then reduced to 700℃ at 15-25℃ / h; then reduced to 350℃ at 30-40℃ / h and then cooled naturally in the furnace until the furnace temperature is below 200℃ before being taken out of the furnace to eliminate internal stress and prevent cracking.
6. The process for purifying and growing quartz sand by agglomeration according to claim 5, characterized in that... Step S6: Cooling and post-processing (2) Cooling control: Specifically, first reduce the furnace temperature to 1210℃ at 40℃ / h and keep it at that temperature for 3h for annealing; then slowly reduce the temperature to 1000℃ at 12℃ / h; reduce it to 700℃ at 15℃ / h; reduce it to 350℃ at 30℃ / h and then let it cool naturally with the furnace until the furnace temperature is below 200℃ before taking it out of the furnace to eliminate internal stress and prevent cracking.
Citation Information
Patent Citations
Device and method for manufacturing quartz weight
CN114195367A