A high-temperature resistant simulated silk fabric and its finishing process
By modifying PET substrate with nano starch and nano ZrO2 powder, and combining it with a low-temperature alkali reduction-dyeing one-bath process, the problems of insufficient heat resistance of polyester imitation silk and high energy consumption and pollution in the production process have been solved, realizing high-performance, green and low-carbon short-process production.
Patent Information
- Application Number
- CN202611489421.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional polyester imitation silk lacks heat resistance and stability, is prone to deformation during high-temperature processing, and has a poor hand feel. Moreover, the production process is energy-intensive, water-intensive, and causes serious pollution, making it difficult to meet the heat resistance and quality requirements of high-end fabrics.
A short-process 110℃ low-temperature alkali reduction-dyeing process was constructed by modifying PET substrate with nano starch and nano ZrO2 powder. The uniform dispersion of nano starch and nano ZrO2 powder in PET substrate improves fiber thermal stability and simultaneously completes alkali reduction and dyeing at low temperature, eliminating the need for reduction and cleaning steps.
It achieves dimensional stability and biodegradability of fibers at high temperatures, reduces energy consumption and pollution, shortens the production process, and improves the drape and color fastness of fabrics, making it suitable for heat-resistant and green production of high-end fabrics.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a simulated silk fabric and finishing process, particularly a high-temperature resistant simulated silk fabric and finishing process. Background Technology
[0002] Polyester imitation silk, with its soft luster, excellent drape, and high cost-effectiveness, has long occupied a core market share in high-end women's wear, home textiles, and decorative fabrics. However, traditional polyester imitation silk suffers from insufficient heat resistance, easily deforming and deteriorating in hand feel during high-temperature processing and use. Furthermore, the small surface area of conventional round fibers limits its imitation effect, making it difficult to meet the heat resistance and quality requirements of high-end fabrics. Simultaneously, traditional imitation silk dyeing and finishing processes employ a long process involving high-temperature strong alkali reduction, high-temperature dyeing, and multiple washing stages, resulting in high energy consumption, large water consumption, low production efficiency, and severe fiber damage. Traditional 130℃ high-temperature processing easily damages the fiber structure, leading to a decrease in fabric heat resistance, and the cumbersome and polluting process is inconsistent with the trend of green printing and dyeing development. Summary of the Invention
[0003] The purpose of this invention is to provide a high-temperature resistant simulated silk fabric and its finishing process. This invention modifies a PET substrate by combining nano-starch and nano-ZrO2 powder, improving the thermal stability of polyester fibers and endowing the fabric with good high-temperature dimensional stability and biodegradability. Furthermore, it constructs a 110℃ low-temperature alkali reduction-dyeing one-bath short-process technology, achieving simultaneous alkali reduction etching and dyeing under the action of benzyl alcohol as a carrier, eliminating the reduction cleaning process. While ensuring the fabric's simulated drape, high color depth, and excellent color fastness, this shortens the production process, reduces energy consumption, water consumption, and pollutant emissions, enabling efficient and low-carbon large-scale production of high-temperature resistant biodegradable simulated silk fabric.
[0004] The technical solution of the present invention is a high-temperature resistant simulated silk fabric, which is woven from polyester fibers modified by nano ZrO2 powder and nano starch.
[0005] In the aforementioned high-temperature resistant simulated silk fabric, the polyester fiber is prepared from nano ZrO2 powder, nano starch and PET substrate, comprising 25-35 parts nano starch, 2-5 parts nano ZrO2 powder and 145-160 parts PET substrate by weight.
[0006] In the aforementioned high-temperature resistant simulated silk fabric, the polyester fiber modified with nano-ZrO2 powder and nano-starch is obtained through the following steps:
[0007] S1. Raw material drying pretreatment: Drying nano ZrO2 powder, nano starch and PET substrate;
[0008] S2. Raw material proportioning and premixing: 30 parts by weight of nano starch, 3 parts by weight of nano ZrO2 powder and 65 parts by weight of PET substrate are put into a high-speed mixer, and compatibilizer and heat stabilizer are added to achieve raw material mixing.
[0009] S3. Melt blending to prepare modified masterbatch: Melt blending is carried out using a co-rotating twin-screw extruder, and the nano starch and nano ZrO2 powder are uniformly dispersed in the PET substrate by gradient heating and melt plasticization. The extruded melt is water-cooled, pelletized, and dried to obtain nano starch / ZrO2 high-temperature resistant composite modified masterbatch.
[0010] S4. Irregular melt spinning: Nano starch / ZrO2 high-temperature resistant composite modified masterbatch is mixed with PET substrate in a 3:7 ratio, dried thoroughly at 120℃, and then fed into a spinning machine. The spinning temperature is 265-275℃. The mixture is melt-extruded using an irregular spinneret, cooled by side blowing, and then hot-stretched at 85℃ and heat-set and wound at 160℃ to obtain polyester fibers modified by both nano ZrO2 powder and nano starch.
[0011] In the aforementioned high-temperature resistant simulated silk fabric, the specific steps of the raw material drying pretreatment in S1 are as follows: nano starch is dried at 105℃ for 6 hours; PET substrate is placed in a vacuum oven at 120℃ for 12 hours to dry, and the moisture content is controlled to be <30 ppm; nano ZrO2 powder is ultrasonically dispersed for 30 minutes and vacuum dried at 80℃ for 4 hours.
[0012] In the aforementioned high-temperature resistant simulated silk fabric, the raw material mixing conditions in S2 are stirring at 80°C for 15 minutes.
[0013] In the aforementioned high-temperature resistant simulated silk fabric, the screw speed of the co-rotating twin-screw extruder is 300 r / min, and the processing temperature is gradually increased within the range of 160 to 270°C.
[0014] A finishing process for a high-temperature resistant simulated silk fabric includes the following steps:
[0015] P1. Pretreatment of high temperature resistant simulated silk fabric: Soap wash 3 times in hot water at 50℃, 30min each time, air dry at room temperature, and dry in oven at 50℃ for 30min.
[0016] P2. Preparation of working solution: Add alkali-resistant disperse dye, benzyl alcohol carrier and weak alkali regulator, stir until the auxiliary agent is completely dissolved, and prepare a uniform and stable alkali reduction dyeing integrated bath solution.
[0017] P3. Low-temperature one-bath processing: The fabric is immersed in the prepared alkali reduction dyeing integrated bath solution, heated to 110℃ at 2℃ / min, kept at 110℃ for 40-50min, and then cooled to 80℃ at 3℃ / min. After washing, drying, and weighing, the surface of the polyester fiber is moderately swollen by utilizing the swelling and penetration effect of benzyl alcohol carrier. The alkali reduction etching and disperse dyeing and fixing are completed simultaneously in a low-temperature alkaline environment.
[0018] In the aforementioned finishing process for a high-temperature resistant simulated silk fabric, the amount of alkali-resistant disperse dye in P2 is 2% owf; the amount of benzyl alcohol carrier is 15 g / L; and the amount of sodium hydroxide is 20 g / L.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] 1. The nano starch compounded with nano zirconium oxide modified system of the present invention improves the heat resistance of the fiber by 20% compared with ordinary polyester. It can stably maintain the crystalline structure at high temperature and inhibit melt deformation. The fabric has both biodegradability and high temperature dimensional stability, which broadens the application scenarios in high temperature fields.
[0021] 2. This invention replaces the traditional 130℃ high-temperature processing with a low temperature of 110℃, saving more than 30% of energy; alkali reduction and dyeing are completed simultaneously in one bath, eliminating the need for reduction cleaning and multiple neutralization washing processes, shortening the overall process by 30%, and significantly reducing water consumption and alkaline wastewater discharge, which is in line with the dual carbon and energy conservation and emission reduction policies of the printing and dyeing industry.
[0022] 3. This invention can precisely control the alkali reduction rate of 20% to 30%, resulting in a soft and draping fabric (drape coefficient ≤35%) that is breathable, cool, and comfortable. The finished product has a high K / S value, full and uniform color, and stable color fastness of all grades reaching level 4 or above, with no dyeing defects such as color spots or color shift.
[0023] 4. The complete set of modified spinning and low-temperature dyeing and finishing process parameters in this application are controllable and can be directly adapted to the company's existing spinning machines and high-temperature dyeing equipment. No large-scale equipment modification is required, making it easy to scale up and improve production and processing efficiency. Detailed Implementation
[0024] The present invention will be further described below with reference to embodiments, but these embodiments are not intended to limit the scope of the invention.
[0025] Example 1. A high-temperature resistant simulated silk fabric, wherein the high-temperature resistant simulated silk fabric is woven from polyester fibers modified by nano-ZrO2 powder and nano-starch.
[0026] The polyester fiber is prepared from nano ZrO2 powder, nano starch and PET substrate, and by mass, it includes 25 parts nano starch, 2 parts nano ZrO2 powder and 152 parts PET substrate.
[0027] The polyester fiber modified by the nano-ZrO2 powder and nano-starch is prepared by the following steps:
[0028] S1. Raw material drying pretreatment: Nano starch is dried at 105℃ for 6 hours; PET substrate is dried in a vacuum oven at 120℃ for 12 hours, with the moisture content controlled to be <30 ppm; Nano ZrO2 powder is ultrasonically dispersed for 30 minutes and vacuum dried at 80℃ for 4 hours.
[0029] S2. Raw material ratio and premixing: 25 parts by weight of nano starch, 2 parts by weight of nano ZrO2 powder and 65 parts by weight of PET substrate are put into a high-speed mixer, and two parts by weight of compatibilizer and heat stabilizer are added. The mixture is stirred at 80°C for 15 minutes to achieve raw material mixing.
[0030] S3. Melt blending to prepare modified masterbatch: Melt blending is carried out using a co-rotating twin-screw extruder with a screw speed of 300 r / min and a gradient temperature increase in the range of 160-270℃ to uniformly disperse nano-starch and nano-ZrO2 powder in PET substrate. The extruded melt is then water-cooled, pelletized, and dried to obtain nano-starch / ZrO2 high-temperature resistant composite modified masterbatch.
[0031] S4. Irregular melt spinning: Nano starch / ZrO2 high-temperature resistant composite modified masterbatch is mixed with PET substrate in a 3:7 ratio, dried thoroughly at 120℃, and then fed into a spinning machine. The spinning temperature is 265-275℃. The mixture is melt-extruded using an irregular spinneret, cooled by side blowing, and then hot-stretched at 85℃ and heat-set and wound at 160℃ to obtain polyester fibers modified by both nano ZrO2 powder and nano starch.
[0032] A finishing process for a high-temperature resistant simulated silk fabric includes the following steps:
[0033] P1. Pretreatment of high temperature resistant simulated silk fabric: Soap wash 3 times in hot water at 50℃, 30min each time, air dry at room temperature, and dry in oven at 50℃ for 30min.
[0034] P2. Preparation of working solution: Add alkali-resistant disperse dye, benzyl alcohol carrier, and weak alkali regulator, and stir until the auxiliaries are completely dissolved to prepare a uniform and stable alkali-reducing dyeing integrated bath solution. The amount of alkali-resistant disperse dye in the alkali-reducing dyeing integrated bath solution is 2% owf; the amount of benzyl alcohol carrier is 15 g / L; and the amount of sodium hydroxide is 20 g / L.
[0035] P3. Low-temperature one-bath processing: The fabric is immersed in the prepared alkali reduction dyeing integrated bath solution, heated to 110℃ at 2℃ / min, kept at 110℃ for 40-50min, and then cooled to 80℃ at 3℃ / min. After washing, drying, and weighing, the surface of the polyester fiber is moderately swollen by utilizing the swelling and penetration effect of benzyl alcohol carrier. The alkali reduction etching and disperse dyeing and fixing are completed simultaneously in a low-temperature alkaline environment.
[0036] Example 2. Based on Example 1, the proportion of nano ZrO2 powder was changed to 4 parts, while the rest remained unchanged.
[0037] Example 3. Based on Example 1, the proportion of nano ZrO2 powder was changed to 3 parts, the proportion of nano starch was changed to 30 parts, and the rest remained unchanged.
[0038] Example 4. Based on Example 1, the proportions of nano ZrO2 powder were changed to 5 parts, the proportions of nano starch were changed to 30 parts, and the rest remained unchanged.
[0039] Example 5. Based on Example 1, the proportion of nano ZrO2 powder was changed to 3 parts, the proportion of nano starch was changed to 35 parts, and the rest remained unchanged.
[0040] Comparative Example 1. Based on Example 1, unmodified PET chips were used for spinning, and the fabric was treated using a conventional 130°C stepwise alkali reduction + dyeing process.
[0041] Spinning raw materials: Only pure PET chips are used, without adding nano starch or nano ZrO2 powder composite masterbatch. The other spinning equipment, temperature, stretching and setting parameters remain unchanged, and pure polyester imitation silk fabric is woven.
[0042] Prepare a concentrated alkali reduction working solution (sodium hydroxide 20g / L), with a liquor ratio of 1:50. Put the greige fabric into the dyeing vat, heat it to 130℃ at a uniform rate, and keep it at a constant temperature for 45 minutes. After the heat preservation is completed, wash it twice with hot water at 80℃ and twice with cold water to remove residual alkali, and then dry it.
[0043] Prepare a dye bath without benzyl alcohol carrier (disperse dye + weak alkali agent only), with a liquor ratio of 1:50. Heat to 130℃ and keep warm for 45 min. After dyeing, add a reducing cleaning agent, wash at 85℃ for 20 min, then wash with water 3 times, dry, and soften and set at 120℃ to obtain the finished product.
[0044] Comparative Example 2. Based on Example 1, the proportion of nano ZrO2 powder was changed to 3 parts, the proportion of nano starch was changed to 0 parts, and the rest remained unchanged.
[0045] Comparative Example 3. Based on Example 1, the proportion of nano ZrO2 powder was changed to 0 parts, the proportion of nano starch was changed to 30 parts, and the rest remained unchanged.
[0046] Comparative Example 4. Based on Example 1, the proportions of nano-ZrO2 powder were changed to 3 parts and nano-starch to 30 parts. The fabric was treated using a traditional 130℃ stepwise alkali reduction + dyeing process. During the treatment, a concentrated alkali reduction working solution (20g / L sodium hydroxide) was prepared at a liquor ratio of 1:50. The fabric was placed in the dye bath, and the temperature was uniformly raised to 130℃ and held at that temperature for 45 minutes. After the holding period, multiple hot water neutralization washes were performed, followed by drying. No benzyl alcohol carrier was added to the dye bath; all other steps were the same as the previous process. The fabric was then placed in the dye bath and held at 130℃ for 45 minutes. After dyeing, reduction washing, multiple water washes, drying, and setting at 120℃ were performed to obtain the finished product.
[0047] Comparative Example 5. Based on Example 1, the proportions of nano-ZrO2 powder were changed to 3 parts, and the proportions of nano-starch were changed to 30 parts. Furthermore, benzyl alcohol carrier was not added in the low-temperature one-bath process. In the low-temperature one-bath process, a carrier-free dye bath was first prepared: only 2% owf alkali-resistant disperse dye and 20 g / L sodium hydroxide were added, without benzyl alcohol carrier, at a bath ratio of 1:50. The fabric was then immersed in the dye bath, heated to 110°C and held at that temperature for 45 min, with simultaneous alkali reduction and dyeing. After dyeing, the fabric was washed twice with warm water, without reduction washing, and then softened and shaped at 120°C to obtain the finished product.
[0048] Performance tests were conducted on Examples 1-5 and Comparative Examples 1-5:
[0049] The surface color characteristic values L, a, b, and K / S values of the dyed fabric were tested using a Datacolor colorimeter under a D65 light source and a 10° viewing angle.
[0050] Color fastness to rubbing was determined in accordance with GB / T 3920-2008 "Textiles - Tests for color fastness - Color fastness to rubbing".
[0051] Color fastness to washing was determined in accordance with GB / T 3921-2008 "Textiles - Tests for color fastness to washing: Test 1".
[0052] The fabric drape coefficient was tested according to GB / T 23319 "Determination of drape performance of textiles".
[0053] The air permeability of the fabric was tested in accordance with the standard GB / T 5453 "Textiles - Determination of Air Permeability of Fabrics".
[0054] Table 1. Performance test results of Examples 1-5 and Comparative Examples 1-5
[0055]
[0056] As can be seen from the experimental results in the table above, the present invention uses a combination of nano-starch and nano-ZrO2 powder as a modifying additive, and the two produce a significant synergistic effect. The heat resistance and mechanical strength of the sample with only nano-starch added are significantly reduced, while the biodegradability of the fabric with only nano-ZrO2 powder added is extremely poor. When the nano-starch addition is 30wt%, the nano-ZrO2 powder addition is 3wt%, combined with a 110℃ low-temperature alkali reduction-dyeing one-bath simultaneous process and 15g / L benzyl alcohol carrier (Experimental Example 3), the resulting high-temperature resistant biodegradable simulated silk fabric exhibits the best overall performance. The fabric's heat resistance can reach 185℃, its breaking strength is 3.08 cN / dtex, its alkali reduction rate is 25%, its K / S value is 24.2, and its color fastness to soaping and rubbing reaches grade 4-5. It also possesses excellent air permeability and a simulated silk drape and feel, and its weight loss rate after soil burial degradation can reach 32.6%.
[0057] In terms of dyeing and finishing processes, the 110℃ low-temperature one-bath simultaneous process combined with a 15g / L benzyl alcohol carrier can effectively promote dye uptake and uniform alkali reduction in fibers, resulting in fabrics with higher color depth, better color fastness, and good drape and breathability. Comparative experiments show that the traditional 130℃ high-temperature stepwise process severely damages the starch components and inorganic stable structure inside the fibers, causing a decrease in the fabric's heat resistance and a significant reduction in biodegradability. Furthermore, the process is cumbersome, energy-intensive, and highly polluting. The carrier-free low-temperature process, on the other hand, suffers from defects such as insufficient dye uptake, shallow color depth, poor color fastness, and uneven weight reduction.
[0058] Considering all indicators, the optimal process scheme of this invention is 30wt% nano starch + 3wt% nano ZrO2 powder, 110℃ low temperature one-bath process, and 15g / L benzyl alcohol carrier (Example 3). Under this condition, the heat resistance, mechanical strength, dyeing performance, hand feel comfort and biodegradability of the fabric are all in the best balance, realizing the integrated processing effect of high performance, green low carbon and short process.
Claims
1. A high-temperature resistant simulated silk fabric, characterized in that, The high-temperature resistant simulated silk fabric is woven from polyester fibers modified with nano ZrO2 powder and nano starch.
2. A high-temperature resistant simulated silk fabric, characterized in that, The polyester fiber is prepared from nano ZrO2 powder, nano starch and PET substrate, and by mass, it includes 25-35 parts nano starch, 2-5 parts nano ZrO2 powder and 145-160 parts PET substrate.
3. The high-temperature resistant simulated silk fabric according to claim 2, characterized in that, The polyester fiber modified by the nano-ZrO2 powder and nano-starch is prepared by the following steps: S1. Raw material drying pretreatment: Drying nano ZrO2 powder, nano starch and PET substrate; S2. Raw material proportioning and premixing: 30 parts by weight of nano starch, 3 parts by weight of nano ZrO2 powder and 65 parts by weight of PET substrate are put into a high-speed mixer, and compatibilizer and heat stabilizer are added to achieve raw material mixing. S3. Melt blending to prepare modified masterbatch: Melt blending is carried out using a co-rotating twin-screw extruder, and the nano starch and nano ZrO2 powder are uniformly dispersed in the PET substrate by gradient heating and melt plasticization. The extruded melt is water-cooled, pelletized, and dried to obtain nano starch / ZrO2 high-temperature resistant composite modified masterbatch. S4. Irregular melt spinning: Nano starch / ZrO2 high-temperature resistant composite modified masterbatch is mixed with PET substrate in a 3:7 ratio, dried thoroughly at 120℃, and then fed into a spinning machine. The spinning temperature is 265-275℃. The mixture is melt-extruded using an irregular spinneret, cooled by side blowing, and then hot-stretched at 85℃ and heat-set and wound at 160℃ to obtain polyester fibers modified by both nano ZrO2 powder and nano starch.
4. The high-temperature resistant simulated silk fabric according to claim 3, characterized in that, The specific steps of the raw material drying pretreatment in S1 are as follows: nano starch is dried at 105℃ for 6 hours; PET substrate is dried in a vacuum oven at 120℃ for 12 hours, and the moisture content is controlled to be <30 ppm; nano ZrO2 powder is ultrasonically dispersed for 30 minutes and vacuum dried at 80℃ for 4 hours.
5. The high-temperature resistant simulated silk fabric according to claim 3, characterized in that, The raw material mixing conditions in S2 are stirring at 80°C for 15 minutes.
6. The high-temperature resistant simulated silk fabric according to claim 3, characterized in that, The co-rotating twin-screw extruder has a screw speed of 300 r / min and a processing temperature that is gradually increased within the range of 160 to 270°C.
7. The finishing process for a high-temperature resistant simulated silk fabric according to any one of claims 1-6, characterized in that, Includes the following steps: P1. Pretreatment of high temperature resistant simulated silk fabric: Soap wash 3 times in hot water at 50℃, 30min each time, air dry at room temperature, and dry in oven at 50℃ for 30min. P2. Preparation of working solution: Add alkali-resistant disperse dye, benzyl alcohol carrier and weak alkali regulator, stir until the auxiliary agent is completely dissolved, and prepare a uniform and stable alkali reduction dyeing integrated bath solution. P3. Low-temperature one-bath processing: The fabric is immersed in the prepared alkali reduction dyeing integrated bath solution, heated to 110℃ at 2℃ / min, kept at 110℃ for 40-50min, and then cooled to 80℃ at 3℃ / min. After washing, drying, and weighing, the surface of the polyester fiber is moderately swollen by utilizing the swelling and penetration effect of benzyl alcohol carrier. The alkali reduction etching and disperse dyeing and fixing are completed simultaneously in a low-temperature alkaline environment.
8. The finishing process for a high-temperature resistant simulated silk fabric according to claim 7, characterized in that, The amount of alkali-resistant disperse dye in P2 is 2% owf; the amount of benzyl alcohol carrier is 15 g / L; and the amount of sodium hydroxide is 20 g / L.