A highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes and its preparation method
By performing surface functionalization treatment on nano zinc oxide and applying hydrophilic modified polyester, combined with an irregular cross-sectional structure, the synergistic improvement of the antibacterial, anti-mite, and moisture-wicking properties of polyester fibers was achieved, realizing rapid wetting and moisture migration effects on the fiber surface.
Patent Information
- Application Number
- CN202611489369.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, the antibacterial and anti-mite functions of polyester fibers are independent of each other. The interfacial compatibility and effective utilization of functional particles in polyester are insufficient, and the fiber surface wetting and moisture transfer capabilities are limited.
By performing graded surface functionalization treatment on nano zinc oxide, and using epoxy-containing silane coupling agents and taurine and 2-aminoethylphosphonic acid for compound grafting, sulfonic acid and phosphonic acid polar groups are introduced. The hydrophilic modified polyester and antibacterial and anti-mite components are concentrated in the composite fiber skin layer, combined with the irregular cross-section capillary groove structure to promote water wetting and migration.
It achieves a synergistic improvement in the antibacterial and anti-mite properties and rapid wetting performance of polyester fibers, enhances the moisture absorption and quick-drying properties of the fibers, and forms a stable hydrophilic region on the fiber surface, thereby increasing the area for moisture spreading and evaporation.
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite fiber technology, specifically to a highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes and its preparation method. Background Technology
[0002] Polyester fiber is characterized by high strength, good heat resistance, dimensional stability, and excellent processing performance, making it one of the most widely used synthetic fibers in home textiles. However, ordinary polyester molecules have relatively few hydrophilic groups, resulting in limited surface wettability and moisture absorption capacity, making it difficult to achieve rapid water absorption and migration in sweaty or humid environments. Furthermore, bedding, quilts, and other home textile products are in prolonged contact with the human body, easily creating an environment conducive to the growth of bacteria, fungi, and mites. Therefore, endowing polyester fibers with antibacterial, anti-mite, moisture-wicking, and quick-drying properties has significant practical application value. Existing technologies typically improve individual properties by adding antibacterial and anti-mite agents, modifying polyester hydrophilicity, or designing irregular cross-sections, but there are still issues of mutual constraints between different functions.
[0003] Chinese patent application publication number CN105332078A discloses an antibacterial polyester fiber based on silver-loaded zirconium phosphate and its preparation method. The method involves introducing silver-loaded zirconium phosphate nanopowder into polyester via in-situ polymerization or masterbatch blending, followed by melt spinning to obtain the antibacterial polyester fiber, which exhibits relatively long-lasting antibacterial properties. However, this technology primarily focuses on imparting antibacterial properties to polyester using silver-loaded zirconium phosphate. It does not disclose the use of nano-zinc oxide with synergistic functionalization of sulfonic acid and phosphonic acid groups to improve the interfacial state of functional particles, nor does it address the synergistic design between antibacterial and anti-mite properties and high moisture absorption and quick-drying properties.
[0004] Chinese patent application publication number CN106498531A discloses an antibacterial and anti-mite fiber and its preparation method. The method involves compounding eugenol and / or isoeugenol with nano-zinc oxide to form an antibacterial and anti-mite powder. After surface coating, this powder is melt-blended with a polymer or made into a masterbatch, and then melt-spun to obtain the antibacterial and anti-mite fiber, which includes polyester fiber. This technology can improve the antibacterial and anti-mite properties of the fiber, but its functional system relies on the compounding of organic anti-mite agents and nano-zinc oxide. It does not disclose the covalent grafting modification of nano-zinc oxide using compounds containing sulfonic acid groups or phosphonic acid groups, nor does it address the issues of insufficient hydrophilicity and improved rapid moisture wicking and quick-drying properties of the polyester fiber itself.
[0005] Chinese patent application publication number CN115012125A discloses a moisture-wicking and quick-drying polyester fabric and its preparation method. The method involves forming a composite fiber containing polyvinylpyrrolidone (PVP) through three-layer coaxial electrospinning, followed by washing to remove the PPVP, resulting in a hollow and porous structure in the polyester fiber to promote moisture absorption, diffusion, and evaporation. This technology primarily improves moisture-wicking and quick-drying performance through a hollow and porous structure. The preparation method is based on electrospinning and subsequent removal of the pore-forming components. It does not involve an antibacterial and anti-mite functional system suitable for conventional melt-spinning composite fabrics, nor does it disclose a technical solution for concentrating antibacterial and anti-mite functional components in the composite fiber skin layer.
[0006] Chinese patent application publication number CN119791133A discloses a method for preparing a nano-zinc oxide composite silver ion antibacterial agent. This method involves liquid-phase composite of nano-zinc oxide and silver-loaded zirconium phosphate to obtain the composite silver ion antibacterial agent, which can leverage the combined effect of nano-zinc oxide and silver-based antibacterial components. However, this technology primarily employs an inorganic composite method for nano-zinc oxide and silver-loaded zirconium phosphate. It does not disclose the process of first anchoring the nano-zinc oxide surface with epoxy-containing silanes, and then introducing sulfonic acid and phosphonic acid functional interfaces through taurine and 2-aminoethylphosphonic acid. Furthermore, it does not address the application of these functional particles in hydrophilic core-sheath shaped polyester fibers.
[0007] Therefore, existing technologies still suffer from problems such as the independence of antibacterial and anti-mite functions from moisture-wicking and quick-drying functions, insufficient interfacial compatibility and effective utilization of functional particles in polyester, and limited surface wetting and moisture transfer capabilities of ordinary polyester. To improve these shortcomings, a highly moisture-wicking and quick-drying composite polyester fiber for antibacterial and anti-mite applications and its preparation method are proposed. Summary of the Invention
[0008] To address the shortcomings of the existing technology, this invention provides a highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes, and a method for preparing the same.
[0009] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0010] A method for preparing a highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes includes the following steps:
[0011] (1) Preparation of hydrophilic modified polyester chips: Add purified terephthalic acid, ethylene glycol, a sodium salt of di(2-hydroxyethyl) 5-sulfonyl-1,3-phthalate and polyethylene glycol to the polymerization reaction system for co-condensation reaction to obtain hydrophilic modified polyester chips;
[0012] (2) Preparation of antibacterial and anti-mite polyester masterbatch: Modified nano zinc oxide, silver-loaded zirconium phosphate and graphene micro powder are melt-blended with polyester chips to obtain antibacterial and anti-mite polyester masterbatch;
[0013] (3) After drying the sheath spinning material and the core material separately, they are fed into a two-component melt spinning device. The polyester mixture containing hydrophilic modified polyester chips and antibacterial and anti-mite polyester masterbatch is used as the sheath and the polyester is used as the core. The mixture is extruded through a shaped spinneret to form a sheath-core composite nascent fiber.
[0014] (4) The core-sheath composite nascent fiber is stretched, crimped and heat-set to obtain the composite polyester fiber;
[0015] In step (2), the modified nano zinc oxide is obtained by reacting nano zinc oxide with an epoxy-containing silane coupling agent to form epoxy silane modified nano zinc oxide, and then performing a ring-opening grafting reaction with a modifier containing taurine and 2-aminoethylphosphonic acid.
[0016] Ordinary polyester lacks sufficient hydrophilic groups in its molecular structure, resulting in poor surface wettability. Relying solely on the capillary effect of irregular cross-sections is insufficient to adequately improve initial water absorption performance. On the other hand, when inorganic functional particles such as nano zinc oxide and silver-based antibacterial agents are directly added to polyester, the particles are prone to agglomeration or being embedded inside the fiber. The functional components that can effectively contact external microorganisms, mites, and moisture are limited, making it difficult to simultaneously achieve antibacterial and anti-mite properties as well as moisture-wicking and quick-drying properties.
[0017] Preferably, the modified nano zinc oxide in step (2) is prepared by a method comprising the following steps:
[0018] S1. Disperse nano-zinc oxide in an alcohol-water solution and then ultrasonically disperse it.
[0019] S2. Add hydrolysate of silane coupling agent containing epoxy groups to react and obtain epoxy silane modified nano zinc oxide;
[0020] S3. React the epoxy silane-modified nano zinc oxide modifier to obtain the modified nano zinc oxide; the modifier includes sulfonic acid compounds containing primary amino groups and phosphonic acid compounds containing primary amino groups.
[0021] The reaction mechanism of this invention is as follows: In step S1, nano-zinc oxide is added to an ethanol-water solution and dispersed under mechanical stirring and ultrasonic action. Ultrasonic cavitation breaks down the aggregation between nano-zinc oxide particles, fully exposing the particle surface. A certain number of Zn-OH surface hydroxyl groups exist on the surface of the nano-zinc oxide in the aqueous system, providing reaction sites for the subsequent silane coupling reaction. In step S2, γ-glycidoxypropyltrimethoxysilane first undergoes hydrolysis in an ethanol-water system at a pH of approximately 4.5. During the reaction at 65°C, the silanol groups generated by hydrolysis undergo dehydration condensation with the Zn-OH groups on the surface of the nano-zinc oxide, forming an interfacial bonding structure mainly composed of Zn-O-Si bonds on the surface of the nano-zinc oxide. Simultaneously, condensation may also occur between some adjacent silanol groups. The Si-O-Si structure; since the epoxy group at the other end of γ-glycidoxypropyltrimethoxysilane is basically retained in this stage, epoxy silane-modified nano zinc oxide with epoxy groups on the surface that can be further reacted is obtained; in step S3, taurine and 2-aminoethylphosphonic acid are dispersed or dissolved under weakly alkaline conditions of about pH 9.0. The weakly alkaline environment is conducive to improving the nucleophilic reaction ability of their amino groups; when epoxy silane-modified nano zinc oxide reacts with the above-mentioned modifier at 70°C, the amino groups in taurine and 2-aminoethylphosphonic acid molecules attack the carbon atoms on the terminal epoxy groups of silane as nucleophilic groups, causing the epoxy ring to undergo a ring-opening reaction to generate a β-hydroxyamine structure, thereby grafting taurine and 2-aminoethylphosphonic acid onto the silane layer on the surface of nano zinc oxide through chemical bonds.
[0022] Furthermore, the modified nano-zinc oxide is prepared by a method comprising the following steps:
[0023] S1. Add nano zinc oxide to an alcohol-water solution with a mass fraction of 60%-95%, and ultrasonically disperse it for 10-60 min under mechanical stirring at 100-500 r / min to obtain a nano zinc oxide dispersion.
[0024] S2. Add the epoxy-containing silane coupling agent to an anhydrous alcohol solvent, then add water, adjust the pH to 3.5-5.5 with acid, and hydrolyze at 20-40℃ for 20-60 min to obtain a silane hydrolysate; add the obtained silane hydrolysate to the nano zinc oxide dispersion obtained in step S1, stir and react at 50-80℃ and 100-500 r / min for 2-6 h, filter, wash 1-5 times with an anhydrous alcohol solvent, and vacuum dry at 60-100℃ for 4-10 h to obtain epoxy silane modified nano zinc oxide;
[0025] S3. Weigh the modifier, dissolve the modifier in water, and adjust the pH to 8.0-10.0 using an alkaline solution to obtain a modifier solution; redisperse the epoxy silane-modified nano zinc oxide obtained in step S2 in an alcohol-water solution with a mass fraction of 30%-70%, and stir for 10-60 min at 100-500 r / min; add the obtained modifier solution, and stir the reaction at 60-80℃ and 100-500 r / min for 4-12 h. After the reaction is complete, filter the solution, wash it successively with deionized water and anhydrous alcohol solvent until the pH of the washing solution is 6.5-7.5, vacuum dry at 60-100℃ for 4-12 h, and then perform air jet milling to control the D50 of the modified nano zinc oxide to be 0.20-0.35 μm to obtain modified nano zinc oxide.
[0026] This invention first modifies the surface of nano-zinc oxide using epoxy silane, then grafts taurine and 2-aminoethylphosphonic acid onto the surface of the nano-zinc oxide, introducing polar groups such as sulfonic acid and phosphonic acid groups. These, along with silver-loaded zirconium phosphate and graphene, form an antibacterial and anti-mite functional system. Simultaneously, a hydrophilic modified polyester containing sulfonate structural units and polyether segments is prepared through copolymerization, and the aforementioned hydrophilic and antibacterial / anti-mite components are concentrated in the composite fiber skin. The polar groups on the fiber surface promote water wetting and spreading, while the longitudinal capillary grooves formed by the irregular cross-section further promote water migration and evaporation. The concentration of functional particles in the near-surface region enhances its effective interaction with the external environment, thereby achieving a synergistic improvement in antibacterial, anti-mite, moisture absorption, moisture wicking, and quick-drying properties.
[0027] Preferably, the epoxy-containing silane coupling agent in step S2 is γ-glycidoxypropyltrimethoxysilane or γ-glycidoxypropyltriethoxysilane; the modifier in step S3 comprises taurine and 2-aminoethylphosphonic acid in a mass ratio of (3-5):1.
[0028] Preferably, in step (1), the amount of the sodium salt of 5-sulfonyl-1,3-phthalate di(2-hydroxyethyl) ester added is 1.0-3.0 mol of purified terephthalic acid, based on the sodium isophthalate-5-sulfonate structural unit; the number average molecular weight of the polyethylene glycol is 600-2000, and the amount added is 2-8% of the mass of purified terephthalic acid.
[0029] Preferably, the antibacterial and anti-mite polyester masterbatch in step (2) comprises, by mass percentage: 70-90% polyester chips, 5-20% modified nano zinc oxide, 2-10% silver-loaded zirconium phosphate, and 0.5-5% graphene micro powder, and the sum of the mass percentages of the above components is 100%; the average particle size of the nano zinc oxide is 10-80 nm, the average particle size of the silver-loaded zirconium phosphate is 0.1-1.0 μm, and the particle size of the graphene micro powder is 50-100 mesh.
[0030] Preferably, the outer layer spinning material in step (3) includes, by weight, 75-90 parts of polyester chips, 8-18 parts of hydrophilic modified polyester chips, and 2-8 parts of antibacterial and anti-mite polyester masterbatch; the mass ratio of the core layer to the outer layer is (40-70):(60-30).
[0031] Preferably, the cross-sectional shape of the irregular spinneret in step (3) is at least one of cross-shaped, four-groove, Y-shaped or W-shaped, so that the outer contour of the obtained fiber cross-section forms at least two capillary grooves that extend continuously along the fiber length direction; the skin layer melt temperature is 265-285℃, and the core layer melt temperature is 275-290℃.
[0032] Preferably, the stretching in step (4) is a two-stage stretching, with the first-stage stretching temperature at 60-85℃ and the stretching ratio at 2.5-3.5 times; the second-stage stretching temperature at 95-120℃ and the stretching ratio at 1.05-1.20 times; and the heat setting temperature at 100-135℃ for 15-40 minutes.
[0033] A highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes is prepared by the method described above.
[0034] The application of the composite polyester fiber in the preparation of home textile products with a cooling sensation upon contact and / or a continuous cooling sensation.
[0035] The beneficial effects of this invention are:
[0036] 1. This invention performs graded surface functionalization treatment on nano zinc oxide. First, an epoxy-containing silane is used to form a reaction interface on the surface of nano zinc oxide. Then, taurine and 2-aminoethylphosphonic acid are used for compound grafting to introduce polar groups such as sulfonic acid groups and phosphonic acid groups on the surface of nano zinc oxide. While maintaining the antibacterial and anti-mite effects of nano zinc oxide, the interfacial state and hydrophilic properties between it and the polyester system are improved, so that the resulting composite fiber has better antibacterial, anti-mite and rapid wetting properties.
[0037] 2. In the process of polyester copolymerization, sodium isophthalate-5-sulfonate structural units and polyethylene glycol segments are introduced to obtain hydrophilic modified polyester. This modified polyester is then combined with hydrophilic functionalized antibacterial and anti-mite components in the fiber skin layer, so that a relatively stable hydrophilic region is formed on the fiber surface. This can promote the rapid spread and absorption of water droplets and reduce the limitation of water transfer caused by the hydrophobicity of ordinary polyester.
[0038] 3. This invention adopts a composite structure of irregularly shaped core and sheath with longitudinal continuous capillary grooves. Based on chemical hydrophilic modification, it further utilizes the capillary effect to promote the diffusion and migration of liquid water along the fiber axis, increase the spreading and evaporation area of water, and connect the water absorption, moisture conduction and quick drying processes to obtain better moisture absorption and quick drying performance.
[0039] 4. This invention concentrates the hydrophilic and antibacterial / anti-mite components in the outer layer, while using ordinary polyester as the core layer. This allows the functional components to be distributed more in the area close to the fiber surface. While reducing the functional components being buried by the internal polyester, it also takes into account the fiber's forming and processing properties, achieving a synergistic effect of antibacterial, anti-mite, and moisture-wicking properties. Detailed Implementation
[0040] The invention will now be described in further detail with reference to specific embodiments, but it should not be construed as limiting the scope of the invention to the following embodiments.
[0041] The raw materials described in this application are partially described; all other raw materials not described are commercially available.
[0042] Polyethylene glycol was purchased from Haian Petrochemical Plant in Jiangsu Province, with a molecular weight of 1000.
[0043] Nano zinc oxide was purchased from Qinghe County Chaotai Metal Materials Co., Ltd., with an average particle size of 20 nm.
[0044] Silver-loaded zirconium phosphate was purchased from Hubei Xinyuhong Biomedical Technology Co., Ltd., with a particle size of 200 nm and a silver content of 3%.
[0045] The graphene micro powder was purchased from Shandong Xinbaiyi Metal Materials Co., Ltd., with a particle size of 50-100 mesh.
[0046] The monosodium salt of 5-sulfonyl-1,3-phthalic acid di(2-hydroxyethyl) ester was purchased from Alfa Chemistry, CAS No. 24019-46-3, catalog number: ACM24019463.
[0047] The fiber-grade polyethylene terephthalate (PET) chips were made from Toray semi-dull fiber-grade PET chips, grade A-2220, with an intrinsic viscosity of approximately 0.64 dL / g.
[0048] Example 1
[0049] A method for preparing highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes includes the following steps:
[0050] (1) Preparation of hydrophilic modified polyester chips: Under nitrogen protection, 100 kg of purified terephthalic acid and 50.5 kg of ethylene glycol were added to the polymerization reaction system, along with 0.035 kg of antimony trioxide. The esterification reaction was carried out at 245 °C and a gauge pressure of 0.25 MPa for 4 h. During the reaction, the water generated by esterification was continuously discharged. A monosodium salt of 5-sulfo-1,3-phthalic acid di(2-hydroxyethyl) ester and 4.0 kg of polyethylene glycol-1000 were added. The amount of monosodium salt of 5-sulfo-1,3-phthalic acid di(2-hydroxyethyl) ester added was 1.5 mol% of the amount of purified terephthalic acid, calculated based on the sodium isophthalate-5-sulfonate structural unit it contained. At the same time, 0.025 kg of trimethyl phosphate was added, and the mixture was stirred for 30 min. Subsequently, the reaction system was heated to 275 °C, and the absolute pressure of the system was gradually reduced to 100 MPa within 40 min. Below Pa, the polycondensation reaction was continued at 275℃ until the intrinsic viscosity of the obtained polymer reached 0.60±0.02 dL / g, at which point the reaction was stopped, the material was discharged, cooled, and pelletized to obtain hydrophilic modified polyester chips.
[0051] (2) Preparation of antibacterial and anti-mite polyester masterbatch: Based on the preparation of 100 kg of antibacterial and anti-mite polyester masterbatch, weigh 80 kg of fiber-grade polyethylene terephthalate chips, 12 kg of modified nano zinc oxide, 6 kg of silver-loaded zirconium phosphate and 2 kg of graphene micro powder; after mixing the modified nano zinc oxide, silver-loaded zirconium phosphate and graphene micro powder evenly, dry at 100℃ for 4 h; vacuum dry the fiber-grade polyethylene terephthalate chips at 150℃ for 5 h, so that the moisture content is not higher than 50 ppm; add the dried components to a high-speed mixer and mix for 15 min, and then send them to a twin-screw extruder for melt blending. The temperature of each temperature zone is controlled sequentially as 255℃, 265℃, 270℃, 275℃ and 275℃, and the screw speed is 180 r / min. After extrusion, water cooling and pelletizing, the melt is vacuum dried at 120℃ for 4 h to obtain antibacterial and anti-mite polyester masterbatch.
[0052] (3) Preparation of the spun yarn: By mass, 83 parts of fiber-grade polyethylene terephthalate chips with an intrinsic viscosity of 0.64±0.02 dL / g, 12 parts of hydrophilic modified polyester chips obtained in step (1) and 5 parts of antibacterial and anti-mite polyester masterbatch obtained in step (2) were mixed evenly to obtain the spun yarn; the obtained spun yarn was vacuum dried at 145℃ for 6 h to make its moisture content not higher than 50 ppm; at the same time, the fiber-grade polyethylene terephthalate chips used as the core layer raw material were vacuum dried at 150℃ for 5 h to make its moisture content not higher than 50 ppm;
[0053] (4) Composite melt spinning: The dried core material and sheath spinning material are fed into a two-component melt spinning device. Fiber-grade polyethylene terephthalate is used as the core layer, and a polyester mixture containing hydrophilic modified polyester and antibacterial and anti-mite components is used as the sheath layer. The mass ratio of the core layer to the sheath layer is controlled at 45:55. The core layer melt temperature is controlled at 280℃, the sheath melt temperature at 276℃, and the spinning box temperature at 278℃. The two melts are metered separately and then fed into the composite spinning assembly, where they are extruded through four-groove cross-shaped shaped spinnerets to form core-sheath composite nascent fibers. The core layer of the resulting composite polyester fiber is located in the central region of the fiber cross-section, and the sheath layer continuously covers the outer periphery of the core layer. The outer contour of the fiber cross-section forms four capillary grooves that extend continuously along the fiber length direction. After the melt is extruded from the spinnerets, it is cooled by side blowing air at a temperature of 20℃, a relative humidity of 65%, and a wind speed of 0.60. m / s; After cooling, the filament bundle is coated with spinning oil, and the oiling rate is controlled at 0.70%. It is wound at a speed of 1050 m / min to obtain composite polyester nascent filament.
[0054] (5) Drafting and post-treatment: The obtained composite polyester nascent yarn is bundled and subjected to two-stage drafting. The first-stage drafting temperature is 70℃ and the drafting ratio is 3.0 times. The second-stage drafting temperature is 105℃ and the drafting ratio is 1.12 times, with a total drafting ratio of 3.36 times. The drafted yarn bundle is crimped to control the number of crimps to 11 / 25 mm. Then, it is heat-set at 120℃ for 25 min. After cooling, it is cut to 38 mm to obtain high moisture-absorbing and quick-drying composite polyester fiber for antibacterial and anti-mite purposes.
[0055] The modified nano zinc oxide is prepared as follows:
[0056] S1. Add 12.0 kg of nano zinc oxide to 120 kg of 80% ethanol aqueous solution and disperse ultrasonically for 30 min under mechanical stirring at 300 r / min to obtain nano zinc oxide dispersion.
[0057] S2. 1.0 kg of γ-glycidoxypropyltrimethoxysilane was added to 10 kg of anhydrous ethanol, followed by 1.0 kg of water. The pH was adjusted to 4.5 with 1 mol / L acetic acid, and hydrolyzed at room temperature for 30 min to obtain a silane hydrolysate. The obtained silane hydrolysate was added to the nano-zinc oxide dispersion obtained in step S1, and the mixture was stirred at 65 °C and 300 r / min for 3 h. After filtration, the mixture was washed three times with anhydrous ethanol and dried under vacuum at 80 °C for 6 h to obtain epoxysilane-modified nano-zinc oxide.
[0058] S3. Weigh 0.36 kg of the modifier, which is composed of taurine and 2-aminoethylphosphonic acid in a mass ratio of 4:1, i.e., 0.288 kg of taurine and 0.072 kg of 2-aminoethylphosphonic acid; dissolve the modifier in 12 kg of water, and adjust the pH to 9.0 using a 10% sodium hydroxide aqueous solution to obtain the modifier solution; redisperse the epoxysilane-modified nano-zinc oxide obtained in step S2 in 60 kg of a 50% ethanol aqueous solution, and stir at 300 r / min for 30 min; add the obtained modifier solution, and stir and react at 70℃ and 300 r / min for 8 h; after the reaction is complete, filter, wash successively with deionized water and anhydrous ethanol until the pH of the washing solution is 7.0, vacuum dry at 80℃ for 8 h, and air-jet pulverize to control the D50 of the modified nano-zinc oxide to be 0.20-0.35 μm to obtain the modified nano-zinc oxide.
[0059] Example 2
[0060] Compared with Example 1, the only difference is that in step S3, the modifier is composed of taurine and 2-aminoethylphosphonic acid in a mass ratio of 3:1; the total mass of the modifier is still 0.36 kg, of which taurine is 0.27 kg and 2-aminoethylphosphonic acid is 0.09 kg; the remaining steps and process parameters are the same as in Example 1.
[0061] Example 3
[0062] Compared with Example 1, the only difference is that in step S3, the modifier is composed of taurine and 2-aminoethylphosphonic acid in a mass ratio of 5:1; the total mass of the modifier is still 0.36 kg, of which taurine is 0.30 kg and 2-aminoethylphosphonic acid is 0.06 kg; the remaining steps and process parameters are the same as in Example 1.
[0063] Example 4
[0064] Compared with Example 1, the only difference is that in step (3), 85 parts by weight of fiber-grade polyethylene terephthalate chips, 10 parts by weight of hydrophilic modified polyester chips obtained in step (1) and 5 parts by weight of antibacterial and anti-mite polyester masterbatch obtained in step (2) are mixed evenly to obtain the skin spinning material; the remaining steps and process parameters are the same as in Example 1.
[0065] Example 5
[0066] Compared with Example 1, the only difference is that in step (3), 81 parts by weight of fiber-grade polyethylene terephthalate chips, 14 parts by weight of hydrophilic modified polyester chips obtained in step (1) and 5 parts by weight of antibacterial and anti-mite polyester masterbatch obtained in step (2) are mixed evenly to obtain the skin spinning material; the remaining steps and process parameters are the same as in Example 1.
[0067] Example 6
[0068] Compared with Example 1, the only difference is that in step (4), the mass ratio of the core layer to the skin layer is adjusted to 40:60; the remaining steps and process parameters are the same as in Example 1.
[0069] Comparative Example 1
[0070] Compared with Example 1, the only difference is that in step (2), unmodified nano zinc oxide is used instead of the same mass of modified nano zinc oxide, that is, the modified nano zinc oxide preparation process S1-S3 is cancelled, and the composition of the remaining masterbatch remains unchanged; the remaining steps and process parameters are the same as in Example 1.
[0071] Comparative Example 2
[0072] Compared with Example 1, the only difference is that the modified nano zinc oxide is processed only according to steps S1 and S2, and is directly used as modified nano zinc oxide after γ-glycidoxypropyltrimethoxysilane modification, and the taurine and 2-aminoethylphosphonic acid graft modification in step S3 is omitted; the remaining steps and process parameters are the same as in Example 1.
[0073] Comparative Example 3
[0074] Compared with Example 1, the only difference is that the modifier in step S3 is only taurine, the total mass of the modifier is kept at 0.36 kg, and 2-aminoethylphosphonic acid is not added; the remaining steps and process parameters are the same as in Example 1.
[0075] Comparative Example 4
[0076] Compared with Example 1, the only difference is that the modifier in step S3 is only 2-aminoethylphosphonic acid, the total mass of the modifier is kept at 0.36 kg, and taurine is not added; the remaining steps and process parameters are the same as in Example 1.
[0077] Comparative Example 5
[0078] Compared with Example 1, the only difference is that the modifier in step S3 is composed of taurine and 2-aminoethylphosphonic acid in a mass ratio of 1:1, and the total mass of the modifier is still 0.36 kg, that is, taurine and 2-aminoethylphosphonic acid are 0.18 kg each; the remaining steps and process parameters are the same as in Example 1.
[0079] Comparative Example 6
[0080] Compared with Example 1, the only difference is that the hydrophilic modified polyester chips obtained in step (1) are not added in step (3). Instead, 95 parts of fiber-grade polyethylene terephthalate chips and 5 parts of antibacterial and anti-mite polyester masterbatch obtained in step (2) are mixed evenly to obtain the skin spinning material; the remaining steps and process parameters are the same as in Example 1.
[0081] Comparative Example 7
[0082] Compared with Example 1, the only difference is that in step (4), a circular spinneret is used instead of a four-groove cross-shaped irregular spinneret, so that the outer contour of the cross section of the obtained composite polyester fiber is circular and does not form four capillary grooves that extend continuously along the fiber length direction; the remaining steps and process parameters are the same as in Example 1.
[0083] Comparative Example 8
[0084] Compared with Example 1, the only difference is that in step (4), the antibacterial and anti-mite polyester masterbatch obtained in step (2) is placed in the core layer; specifically, the core layer is composed of 93.89 parts by weight of fiber-grade polyethylene terephthalate chips and 6.11 parts by weight of antibacterial and anti-mite polyester masterbatch; the skin layer is composed of 88 parts by weight of fiber-grade polyethylene terephthalate chips and 12 parts by weight of hydrophilic modified polyester chips obtained in step (1); the total mass ratio of the core layer to the skin layer remains 45:55; the remaining steps and process parameters are the same as in Example 1.
[0085] Test Example 1
[0086] Antibacterial performance test: To evaluate the antibacterial performance of the composite polyester fibers obtained in each example and comparative example, the short fibers obtained in Examples 1-6 and Comparative Examples 1-8 were respectively made into test knitted fabrics using the same spinning and weaving processes. Specifically, each group of short fibers was spun into single yarns with a linear density of 19.7 tex, and then knitted into plain weft knitted fabrics using the same weft knitting process, controlling the unit area mass of each group of knitted fabrics to be 160±5 g / m². 2 The knitted fabrics used in the test were not dyed, treated with antibacterial agents, moisture-wicking agents, or other functional finishing processes to eliminate the influence of finishing processes on the test results.
[0087] The antimicrobial properties of each group of samples were tested according to GB / T 20944.3-2008 "Evaluation of Antimicrobial Properties of Textiles - Part 3: Shaking Method". Staphylococcus aureus (ATCC 6538), Escherichia coli (8099), and Candida albicans (ATCC 10231) were selected as test species. Three parallel samples were set up for each group. Bacterial culture, inoculation, shaking culture, viable cell count, and inhibition rate calculation were performed according to the standard. The average value of the three parallel sample test results was taken. The test results are shown in Table 1.
[0088] Table 1. Antibacterial properties of each group of samples
[0089] Group Staphylococcus aureus inhibition rate / % Escherichia coli inhibition rate / % Candida albicans inhibition rate / % Example 1 99.7 99.5 95.4 Example 2 99.3 99.0 93.8 Example 3 99.4 99.1 94.1 Example 4 99.6 99.4 95.0 Example 5 99.7 99.5 95.5 Example 6 99.8 99.7 95.9 Comparative Example 1 88.6 86.9 75.2 Comparative Example 2 92.4 90.7 80.6 Comparative Example 3 96.1 94.8 87.9 Comparative Example 4 94.6 92.9 84.8 Comparative Example 5 96.8 95.6 89.5 Comparative Example 6 99.4 99.2 94.7 Comparative Example 7 99.5 99.3 94.9 Comparative Example 8 81.3 78.8 68.5
[0090] Test Example 2
[0091] Anti-mite performance test: The above-mentioned knitted fabrics of the same specification made of composite polyester fibers obtained in Examples 1-6 and Comparative Examples 1-8 were taken as samples respectively.
[0092] Considering that the composite polyester fiber obtained in this invention involves washing when used in home textile products, to eliminate the mite-repellent effect caused by temporary adhesions on the fiber surface, each group of samples was first pretreated, washed, and then air-dried. Subsequently, the mite-repellent performance was tested according to the repellency method specified in GB / T 24253-2009 "Evaluation of Mite-Repellent Performance of Textiles", using house dust mite (Dermatophagoides farinae Hughes) as the test mite.
[0093] Samples and control samples were prepared according to the standard specifications and cultured under the specified temperature and humidity conditions. After culture, the number of surviving mites in the samples and control samples was recorded, and the mite repellency rate was calculated with reference to GB / T 24253-2009. Three parallel experiments were set up for each group, and the average value was used as the final result. The test results are shown in Table 2.
[0094] Table 2. Anti-mite performance of each group of samples after 3 washes
[0095] Group Mite repellency rate / % Example 1 99.2 Example 2 98.3 Example 3 98.6 Example 4 99.0 Example 5 99.3 Example 6 99.6 Comparative Example 1 73.4 Comparative Example 2 81.2 Comparative Example 3 90.7 Comparative Example 4 87.5 Comparative Example 5 92.6 Comparative Example 6 98.9 Comparative Example 7 98.8 Comparative Example 8 66.2
[0096] Test Example 3
[0097] Moisture absorption and quick-drying performance test: The composite polyester fibers obtained in Examples 1-6 and Comparative Examples 1-8 were prepared using the same method as in Test Example 1, with a unit area mass of 160±5 g / m². 2The weft-knitted fabrics use the exact same spinning and weaving processes for all components and are not finished with any hydrophilic, moisture-wicking, or quick-drying properties.
[0098] The tests were conducted in accordance with GB / T 21655.1-2023, "Evaluation of the moisture absorption and quick-drying properties of textiles - Part 1: Single-item combination test method". Each group of samples was washed 5 times according to the washing procedure specified in the standard and then air-dried naturally. The water absorption rate, drip diffusion time, drying rate and wicking height were then measured respectively.
[0099] Among them, water absorption rate is used to characterize the proportion of water absorbed by the sample after it is fully wetted, relative to its original mass; water droplet diffusion time is used to evaluate the ability of water droplets to quickly wet and diffuse after contact with the sample; drying rate is used to evaluate the rate at which water in the sample dissipates under specified conditions; and wicking height is used to evaluate the ability of water to be transferred along the longitudinal direction of the fabric by capillary action. Parallel samples were set up for each item according to GB / T 21655.1-2023, and the average value was taken. The test results are shown in Table 3.
[0100] Table 3. Moisture absorption and quick-drying properties of each group of samples after 5 washes
[0101] Group Water absorption rate / % Water diffusion time / s Drying rate (g / h) Cubic suction height / mm Example 1 302 0.8 0.45 176 Example 2 286 1.1 0.41 165 Example 3 291 1.0 0.42 168 Example 4 268 1.5 0.37 154 Example 5 318 0.6 0.48 186 Example 6 313 0.7 0.47 183 Comparative Example 1 221 2.9 0.28 126 Comparative Example 2 236 2.4 0.30 136 Comparative Example 3 253 1.8 0.34 146 Comparative Example 4 239 2.3 0.31 137 Comparative Example 5 248 2.0 0.33 143 Comparative Example 6 158 7.1 0.20 83 Comparative Example 7 187 5.0 0.23 97 Comparative Example 8 226 2.8 0.29 129
[0102] The test results of Examples 1-3 and Comparative Examples 1-5 show that the surface modification method of nano-zinc oxide and the compounding ratio of taurine and 2-aminoethylphosphonic acid have a significant impact on the antibacterial, anti-mite, and moisture-wicking properties of composite polyester fibers. Comparative Example 1 directly used unmodified nano-zinc oxide, resulting in poor dispersion and interfacial compatibility in the polyester matrix, limiting the effective action of the functional components. Comparative Example 2 only used γ-glycidyl etheroxypropyltrimethoxysilane to modify the surface of nano-zinc oxide. Although this improved the interfacial compatibility between nano-zinc oxide and the polyester matrix, the lack of subsequent introduction of hydrophilic functional groups meant its overall performance was still lower than that of Examples 1-3. Comparative Examples 3 and 4 used taurine or 2-aminoethylphosphonic acid grafting alone, respectively, failing to simultaneously exert the synergistic interfacial regulation effect of sulfonic acid and phosphonic acid groups. Although Comparative Example 5 used both modifiers, the ratio deviated from the preferred range, resulting in a decrease in the antibacterial, anti-mite, and hydrophilic properties of the modified nano-zinc oxide. Examples 1-3 use a combination of taurine and 2-aminoethylphosphonic acid for modification. Appropriately increasing the proportion of taurine helps to form a more sufficient hydrophilic interface, while retaining a certain proportion of phosphonic acid groups to participate in the surface action of nano zinc oxide, so as to achieve a good balance between antibacterial and anti-mite properties and moisture absorption and quick-drying properties. Within the range of the taurine to 2-aminoethylphosphonic acid combination ratio, the 4:1 ratio used in Example 1 has the best overall effect.
[0103] The test results from Examples 1, 4, 5, and Comparative Example 6 show that the amount of hydrophilic modified polyester chips added mainly affects the wetting, water absorption, and moisture transfer properties of the fiber. In Comparative Example 6, after removing the hydrophilic modified polyester, although the fiber still contained antibacterial and anti-mite functional components, the improvement in the hydrophobicity of the polyester itself was limited, and the wetting and diffusion of water droplets on the fiber and fabric surface were significantly affected. In Example 4, reducing the amount of hydrophilic modified polyester resulted in a corresponding decrease in moisture absorption and quick-drying performance; in Example 5, appropriately increasing the amount of hydrophilic modified polyester further improved the water absorption, moisture wicking, and drying properties. This indicates that introducing sulfonate-containing structural units and polyether segments into the polyester molecular structure can effectively improve the affinity of the polyester fiber surface for water and form a synergistic effect with the hydrophilic groups on the modified nano-zinc oxide surface.
[0104] The test results of Example 1 and Comparative Example 7 show that, with essentially the same chemical composition, changing the four-groove cross-shaped cross section to a circular cross section significantly reduces the fiber's moisture absorption and quick-drying properties, while the antibacterial and anti-mite properties remain relatively unchanged. This is because the four continuously extending capillary grooves along the fiber length increase the contact area between the fiber and liquid water, providing a continuous channel for water to diffuse along the fiber axis; the circular cross section lacks this capillary structure, restricting the spread and migration of water. This indicates that the moisture absorption and quick-drying effect of the present invention is not solely due to chemical hydrophilic modification, but rather the result of the combined effect of the hydrophilic components and the irregular capillary structure.
[0105] The test results from Examples 1, 6, and Comparative Example 8 show that the functional sheath layer plays a crucial role in overall performance. In Example 6, increasing the sheath layer ratio maintained high levels of antibacterial, anti-mite, and moisture-wicking properties, indicating that appropriately increasing the functional sheath layer ratio is beneficial for enhancing the effectiveness of hydrophilic and antibacterial / anti-mite components in the near-surface region of the fiber. In Comparative Example 8, transferring the antibacterial / anti-mite polyester masterbatch to the core layer significantly reduced antibacterial and anti-mite properties, while also affecting moisture-wicking properties. This is because the functional particles are more embedded within the fiber, limiting their effective contact with external moisture, microorganisms, and mites. This demonstrates that concentrating the hydrophilic modified polyester and antibacterial / anti-mite components in the sheath layer, forming a sheath-core composite structure with the polyester core layer, can improve the utilization efficiency of functional components while maintaining fiber forming properties.
Claims
1. A method for preparing highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes, characterized in that, Includes the following steps: (1) Preparation of hydrophilic modified polyester chips: Add purified terephthalic acid, ethylene glycol, a sodium salt of di(2-hydroxyethyl) 5-sulfonyl-1,3-phthalate and polyethylene glycol to the polymerization reaction system for co-condensation reaction to obtain hydrophilic modified polyester chips; (2) Preparation of antibacterial and anti-mite polyester masterbatch: Modified nano zinc oxide, silver-loaded zirconium phosphate and graphene micro powder are melt-blended with polyester chips to obtain antibacterial and anti-mite polyester masterbatch; (3) After drying the sheath spinning material and the core material separately, they are fed into a two-component melt spinning device. The polyester mixture containing hydrophilic modified polyester chips and antibacterial and anti-mite polyester masterbatch is used as the sheath and the polyester is used as the core. The mixture is extruded through a shaped spinneret to form a sheath-core composite nascent fiber. (4) The core-sheath composite nascent fiber is stretched, crimped and heat-set to obtain the composite polyester fiber; In step (2), the modified nano zinc oxide is obtained by reacting nano zinc oxide with an epoxy-containing silane coupling agent to form epoxy silane modified nano zinc oxide, and then performing a ring-opening grafting reaction with a modifier containing taurine and 2-aminoethylphosphonic acid.
2. The method according to claim 1, characterized in that, The modified nano zinc oxide in step (2) is prepared by a method including the following steps: S1. Disperse nano-zinc oxide in an alcohol-water solution and then ultrasonically disperse it. S2. Add hydrolysate of silane coupling agent containing epoxy groups to react and obtain epoxy silane modified nano zinc oxide; S3. React the epoxy silane-modified nano zinc oxide modifier to obtain the modified nano zinc oxide; the modifier includes sulfonic acid compounds containing primary amino groups and phosphonic acid compounds containing primary amino groups.
3. The method according to claim 2, characterized in that, The epoxy-containing silane coupling agent in step S2 is γ-glycidoxypropyltrimethoxysilane or γ-glycidoxypropyltriethoxysilane; the modifier in step S3 contains taurine and 2-aminoethylphosphonic acid in a mass ratio of (3-5):
1.
4. The method according to claim 1, characterized in that, The amount of the sodium salt of 5-sulfonyl-1,3-phthalate di(2-hydroxyethyl) ester added in step (1) is 1.0-3.0 mol of purified terephthalic acid, based on the sodium isophthalate-5-sulfonate structural unit; the number average molecular weight of the polyethylene glycol is 600-2000, and the amount added is 2-8% of the mass of purified terephthalic acid.
5. The method according to claim 1, characterized in that, The antibacterial and anti-mite polyester masterbatch in step (2) comprises, by mass percentage: 70-90% polyester chips, 5-20% modified nano zinc oxide, 2-10% silver-loaded zirconium phosphate, and 0.5-5% graphene micro powder, with the sum of the mass percentages of the above components being 100%; the average particle size of the nano zinc oxide is 10-80 nm, the average particle size of the silver-loaded zirconium phosphate is 0.1-1.0 μm, and the particle size of the graphene micro powder is 50-100 mesh.
6. The method according to claim 1, characterized in that, The sheath spinning material in step (3) includes, by weight, 75-90 parts of polyester chips, 8-18 parts of hydrophilic modified polyester chips, and 2-8 parts of antibacterial and anti-mite polyester masterbatch; the mass ratio of the core layer to the sheath layer is (40-70):(60-30).
7. The method according to claim 1, characterized in that, The cross-sectional shape of the irregular spinneret in step (3) is at least one of cross-shaped, four-groove, Y-shaped or W-shaped, so that the outer contour of the obtained fiber cross-section forms at least two capillary grooves that extend continuously along the fiber length direction; the skin layer melt temperature is 265-285℃, and the core layer melt temperature is 275-290℃.
8. The method according to claim 1, characterized in that, The stretching in step (4) is a two-stage stretching. The first-stage stretching temperature is 60-85℃ and the stretching ratio is 2.5-3.5 times. The second-stage stretching temperature is 95-120℃ and the stretching ratio is 1.05-1.20 times. The heat setting temperature is 100-135℃ and the time is 15-40 minutes.
9. A highly absorbent and quick-drying composite polyester fiber for antibacterial and anti-mite purposes, characterized in that, Prepared by the method described in any one of claims 1-8.
10. The application of the composite polyester fiber according to claim 9 in the preparation of home textile products with a cooling sensation upon contact and / or a continuous cooling sensation.
Citation Information
Patent Citations
Antibacterial polyester fiber based on silver-loaded zirconium phosphate and preparation method thereof
CN105332078A
Anti bacterial anti mite fiber and preparation method thereof
CN106498531A
Moisture-absorbing and quick-drying polyester fabric and preparation method thereof
CN115012125A