A micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase

By preparing a micro-nano activated hydroxyl negative ion composite powder coating on the pillowcase, the problem of insufficient purification ability of existing pillowcases in dark environments and pollution caused by long-term use is solved. It achieves antibacterial, anti-mite and deodorizing effects within 7 days and provides a clear standard for hygienic replacement.

CN123108926APending Publication Date: 2026-11-17XIANGXING BIOTECHNOLOGY (WUXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611418175.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing functional pillowcases cannot continuously release hydroxyl negative ions with oxidative decomposition capabilities in dim light and normal temperature environments, making it difficult to maintain their antibacterial, anti-mite, and odor-decomposing effects. Furthermore, the lack of a clear hygiene replacement cycle leads to the continuous accumulation of microorganisms and sebum pollutants on the pillow surface.

Method used

Using micro-nano activated hydroxyl negative ion composite powder as a functional coating, combined with water-based flexible film-forming aids, nano dispersants and plant antibacterial stabilizers, a disposable weekly antibacterial pillowcase is prepared. The coating spontaneously generates hydroxyl negative ions under normal temperature and light-free conditions, which destroys bacterial cell membranes and decomposes odors. It is designed to be used for 7 days without washing.

Benefits of technology

It continuously generates highly active hydroxyl negative ions in a dark, enclosed environment, achieving antibacterial, mite-inhibiting, and deodorizing effects. It avoids the accumulation of pollution caused by long-term use, provides a clear standard for hygienic replacement, and keeps the pillowcase soft, skin-friendly, and breathable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108926A_ABST
    Figure CN123108926A_ABST
Patent Text Reader

Abstract

This invention discloses a micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase, belonging to the field of functional sanitary home textile technology. The antibacterial pillowcase includes a pillowcase base fabric and a functional negative ion coating loaded on the surface of the base fabric. The functional negative ion coating is prepared by mixing micro-nano activated hydroxyl negative ion composite powder, water-based flexible film-forming aid, nano-dispersant, wetting and penetrating agent, plant antibacterial stabilizer, and deionized water in a specific weight ratio. The micro-nano activated hydroxyl negative ion composite powder is modified by low-temperature calcination and ball milling, with a particle size of 200 to 500 nanometers, and can continuously generate hydroxyl negative ions by ionizing air water molecules under normal temperature and light-free conditions. This pillowcase adopts a disposable weekly disposable design, with a rated safe use period of 7 days. It can continuously achieve antibacterial, anti-mite, and odor decomposition without light or electricity. The coating is ultra-thin, soft, and does not shed powder. After the use period, it can be directly discarded and replaced without washing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional sanitary home textiles and antibacterial and purifying materials, specifically a micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase. Background Technology

[0002] Pillows are intimate home textile products that come into close contact with the body for extended periods during sleep. While sleeping at night, the head, face, and neck remain in contact with the pillowcase for several hours, causing sweat, sebum, and shed skin to accumulate on the surface. Traditional cotton or synthetic fiber pillowcases, with repeated use and washing, are highly susceptible to the growth of harmful microorganisms such as Staphylococcus aureus, Escherichia coli, mold, and dust mites. These microorganisms multiply rapidly, feeding on the accumulated sebum and shed skin, and their metabolic byproducts oxidize and ferment, producing a rancid odor. This not only affects the sleep experience but can also trigger problems such as facial acne, itchy skin, allergies, and respiratory discomfort, posing a continuous threat to sleep hygiene and skin health.

[0003] To address the aforementioned issues, various functional pillowcase products have emerged in the existing technology, primarily employing the following technical methods: The first type is silver ion antibacterial technology. Silver ions have strong bactericidal capabilities and are widely used in antibacterial finishing of home textile products. However, silver ions are prone to oxidation and discoloration during long-term use, causing the surface of pillowcases to turn yellow or black, affecting their appearance. At the same time, the antibacterial effect of silver ions decreases significantly with the number of washes and the duration of use, making it difficult to maintain a stable antibacterial level throughout the entire lifespan of the pillowcase. In addition, the residue of silver ions on the surface of pillowcases and their potential irritation to the skin are also of great concern.

[0004] The second category is natural antibacterial fibers such as bamboo fiber. Bamboo fiber is used in pillowcase manufacturing because it has certain natural antibacterial properties. However, the antibacterial components of bamboo fiber are gradually lost during fiber processing and repeated washing, resulting in insufficient antibacterial durability. In addition, bamboo fiber has a narrow antibacterial spectrum and limited inhibitory effect on mold and dust mites.

[0005] The third type is activated carbon adsorption technology. Activated carbon relies on its porous structure to adsorb odor molecules, which can reduce pillow odor to some extent. However, activated carbon only has physical adsorption capacity and cannot decompose and remove odor organic matter. When the adsorption sites are saturated, the adsorbed odor molecules may be released again under conditions of increased temperature or pressure, causing secondary pollution. At the same time, activated carbon particles are easy to fall off the fabric surface, affecting the feel and cleanliness.

[0006] The fourth category is conventional negative ion fabric technology. Existing negative ion fabrics typically add mineral powders such as tourmaline to the fibers or coatings, releasing negative ions through piezoelectric or pyroelectric effects. However, the activation of these negative ion materials requires external energy input such as light, temperature changes, or mechanical friction. In the dim light, constant temperature, and low friction environment during sleep at night, the amount of negative ions released is significantly reduced. More importantly, conventional negative ion fabrics mainly release negative oxygen ions, which have a low oxidation-reduction potential and lack strong oxidative decomposition capabilities. They cannot destroy bacterial cell membrane structures or degrade organic odor molecules, and can only improve the feeling of air freshness to a certain extent, failing to fundamentally solve the problems of microbial growth and odor residue on pillow surfaces.

[0007] In addition to the inherent limitations of the aforementioned antibacterial and purification technologies, existing pillowcase products also present a systemic hygiene management problem: Currently, all pillowcases on the market are designed for long-term reuse, with no clearly defined safe usage period or replacement standards. Ordinary households typically find it difficult to wash and disinfect pillowcases frequently, often using them continuously for weeks or even months without changing them, causing the pillow's microenvironment to deteriorate through repeated contamination. While hotels, guesthouses, hospitals, and other public accommodations do change and wash pillowcases, the washing process mainly removes visible stains, failing to thoroughly eliminate deeply ingrained bacteria and mites, and the risk of cross-contamination is even higher in public settings.

[0008] In summary, the existing technology lacks a functional pillowcase product that can continuously release hydroxyl negative ions with strong oxidative decomposition capabilities in dim light and normal temperature environments, kill microorganisms and decompose odors at the source, and has a clear hygiene replacement cycle and does not require washing. Summary of the Invention

[0009] To address the aforementioned problems in existing technologies, the main technical problem this invention aims to solve is that existing functional pillowcases rely on light stimulation or only possess physical adsorption capabilities for antibacterial purification. They cannot continuously generate hydroxyl negative ions with oxidative decomposition capabilities in the dimly lit, enclosed environment of sleep, resulting in unsustainable antibacterial, anti-mite, and odor-decomposing effects. The secondary technical problem this invention aims to solve is that existing pillowcases are designed for long-term reuse, lacking a clear hygiene replacement cycle, leading to the continuous accumulation of microorganisms and sebum contaminants on the pillow surface and cumbersome cleaning processes.

[0010] To address the aforementioned technical problems, this invention provides a micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase, comprising a pillowcase base fabric and a functional negative ion coating loaded on the surface of the pillowcase base fabric. The functional negative ion coating uses micro-nano activated hydroxyl negative ion composite powder as the core functional raw material, combined with a water-based flexible film-forming aid, a nano-dispersant, a wetting and penetrating agent, and a plant-based antibacterial stabilizer, and is prepared using deionized water as the dispersion medium according to a specific weight ratio. The micro-nano activated hydroxyl negative ion composite powder is made from natural mineral raw materials, and undergoes low-temperature calcination activation and high-speed ball milling modification treatment to control the powder particle size within the range of 200 to 500 nanometers. The activated and modified mineral powder surface forms abundant active sites, enabling it to spontaneously adsorb water molecules from the air under normal temperature, no light, and normal pressure conditions. Through the micro-electric field effect on the powder surface, the water molecules are ionized, continuously generating highly active hydroxyl negative ions. Hydroxyl anions have strong oxidizing properties, which can destroy the bacterial cell membrane structure, denature and inactivate microbial proteins, and oxidize and degrade the odor-causing organic molecules produced by sebum oxidation and sweat decomposition into odorless small molecules, thereby achieving multiple functions of antibacterial, mite-inhibiting and deodorizing in the pillow microenvironment.

[0011] In terms of coating system design, a water-based flexible film-forming agent forms an ultra-thin, transparent, flexible protective film on the surface of the pillowcase base fabric, firmly anchoring micro- and nano-powder particles to the fiber surface and preventing the powder from falling off due to friction during use, while maintaining the original softness and breathability of the pillowcase. A nano-dispersant prevents the nano-powder particles from agglomerating in the finishing solution through steric hindrance and electrostatic repulsion, ensuring a uniform coating without color spots. A wetting and penetrating agent reduces the surface tension of the finishing solution, promoting the penetration and uniform adhesion of functional components to the nonwoven fiber surface, improving the bonding strength between the coating and the base fabric. A plant-based antibacterial stabilizer, on the one hand, helps inhibit the growth of mold and bacteria, synergizing with the oxidative bactericidal effect of hydroxyl negative ions; on the other hand, it neutralizes the slight irritation that mineral powders may cause, improving the fabric's skin-friendly safety, while also stabilizing the negative ion release efficiency.

[0012] Regarding product usage, this invention designs the pillowcase as a disposable, weekly-use product with a rated safe usage period of 7 days. The product uses individual, sterile, sealed packaging. After opening, it can be placed on the pillow for use. It continuously provides antibacterial, anti-mite, deodorizing, and purifying effects within the 7-day period. After the period, it can be discarded and replaced with a new pillowcase without washing. This weekly-use design eliminates the problem of contaminant accumulation caused by long-term reuse and also avoids damage to the functional coating during washing.

[0013] In a preferred embodiment, the raw material weight ratio of the functional negative ion coating is as follows: 5.0 parts of micro / nano activated hydroxyl negative ion composite powder, 10.0 parts of water-based flexible film-forming aid, 0.4 parts of nano dispersant, 0.25 parts of wetting and penetrating agent, 1.8 parts of plant antibacterial stabilizer, and 82.55 parts of deionized water. This ratio achieves a balance between negative ion release efficiency, coating adhesion, and skin-friendly softness.

[0014] In a preferred embodiment, the pillowcase base fabric is a microfiber spunlace nonwoven fabric with a weight of 80 to 120 grams per square meter. Spunlace nonwoven fabrics within this weight range have fine, soft fibers and a smooth, uniform surface, providing a good substrate for functional coatings while also possessing suitable breathability and moisture absorption. Furthermore, the fiber gaps are small enough to prevent nanoparticles from penetrating and detaching from the fabric surface.

[0015] In a preferred embodiment, the activation modification temperature of the micro / nano activated hydroxyl anion composite powder is 350 to 420 degrees Celsius. Low-temperature calcination within this range effectively activates the surface active sites of the mineral powder without causing mineral lattice deactivation due to excessively high temperatures. After high-speed ball milling and classification, the powder particle size is controlled between 200 and 500 nanometers. This particle size range ensures the powder has a large specific surface area and high reactivity, while also facilitating uniform dispersion in aqueous systems. The activated powder can stably excite hydroxyl anions within a wide temperature range of -10 degrees Celsius to 65 degrees Celsius, without relying on ultraviolet irradiation or requiring an external power source.

[0016] In a preferred embodiment, the functional negative ion coating is prepared using a single-sided padding and low-temperature air-drying molding process, with the coating thickness controlled between 0.01 and 0.03 mm. Single-sided padding ensures that the functional coating is concentrated on the front of the pillowcase that comes into contact with the body, saving raw materials while preventing the coating from penetrating to the back and affecting its spreadability and fit. The ultra-thin coating is transparent, colorless, and has no particle-like feel, and will not change the softness or appearance of the pillowcase base fabric.

[0017] This invention also provides a method for preparing the above-mentioned antibacterial pillowcase, comprising the following steps: First, at room temperature, dissolve the nano-dispersant, wetting and penetrating agent, and plant antibacterial stabilizer in deionized water, and stir at low speed for 5 to 10 minutes to fully dissolve and disperse the additives, forming a uniform and stable base solution; then, slowly add micro-nano activated hydroxyl negative ion composite powder to the base solution, and homogenize by high-speed shearing for 20 to 30 minutes to break up the soft agglomerates of the powder using high shear force, so that the nanoparticles are uniformly suspended in the liquid phase; then, cool the system to 35 to 40 degrees Celsius, slowly add the water-based flexible film-forming aid, and stir at low speed for 10 to 15 minutes for compounding, avoiding the introduction of a large number of air bubbles by high-speed stirring, to obtain a functional negative ion finishing liquid; then, uniformly pass the ultrafine fiber spunlace nonwoven fabric through the finishing liquid for single-sided impregnation, controlling the roll-up rate, i.e., the liquid-carrying rate, between 45% and 55% to load the base fabric with an appropriate amount of functional components; finally, at 55 to 65 degrees Celsius... The fibers are dried and cured under low-temperature hot air conditions at 100 degrees Celsius, which allows the film-forming agent to form a continuous and uniform flexible film on the fiber surface. After natural cooling, the fibers are cut into pillowcase sizes and folded and then individually aseptically sealed.

[0018] This invention also provides a method for applying the above-mentioned antibacterial pillowcase: The individually sterile, sealed antibacterial pillowcase is opened and placed directly on the pillow surface. During the 7-day usage period, the functional negative ion coating continuously contacts air and water molecules, releasing hydroxyl negative ions, which inhibit and kill bacteria, mold, and mites on the pillow surface. Simultaneously, it continuously decomposes odor molecules produced by the oxidation of sweat and sebum from the head, keeping the pillow surface clean and fresh. After the 7-day period, the pillowcase is removed from the pillow and discarded, replaced with a new weekly disposable pillowcase. No washing is required during the entire usage process.

[0019] Compared with the prior art, the present invention has the following beneficial effects: First, addressing the problem that existing functional pillowcases rely on light stimulation and have insufficient purification capabilities in low-light environments, this invention uses micro-nano natural mineral composite powder that has been modified by low-temperature activation. Its surface active sites can spontaneously adsorb and ionize air water molecules under normal temperature and light-free conditions, continuously generating hydroxyl negative ions. It does not require ultraviolet irradiation or an external power source and can still work stably in a dark and enclosed environment during sleep all night, adapting to use in a wide temperature range.

[0020] Secondly, addressing the problem that existing technologies only have adsorption capacity but cannot decompose organic matter and whose antibacterial effects are easily weakened, the hydroxyl negative ions released by this invention have strong oxidizing properties, which can oxidize and destroy bacterial cell membranes, denature mite proteins, and degrade sebum oxidation products and sweat odor organic molecules into odorless small molecules, thus achieving antibacterial, mite-inhibiting, and odor-removing effects from the root; at the same time, plant antibacterial stabilizers provide auxiliary antibacterial effects, forming a dual synergistic purification mechanism with hydroxyl negative ions.

[0021] Third, addressing the issues of existing functional coatings being prone to powdering, hardening, and affecting the skin-friendly feel, this invention uses a water-based flexible film-forming agent to form an ultra-thin flexible protective film on the base fabric surface. Combined with nano-dispersants and wetting and penetrating agents, it ensures uniform dispersion and firm adhesion of the powder. The coating thickness is only 0.01 to 0.03 mm, transparent and colorless, without a grainy feel, does not harden, and does not shed powder, maintaining the soft, skin-friendly, breathable, and dry feel of the pillowcase.

[0022] Fourth, in response to the problems of existing pillowcases being reused for a long time, having poor hygiene, and being cumbersome to clean, this invention adopts a 7-day weekly disposable pillowcase model, coupled with independent aseptic sealed packaging. It can be used immediately after opening the bag, and can be discarded after the expiration date without washing. This establishes a clear hygiene replacement standard in terms of product form, avoiding the long-term accumulation of microorganisms and sebum contaminants on the pillow surface, and also eliminating the loss of functional ingredients caused by washing.

[0023] Fifth, the preparation process of this invention adopts an all-water system and a low-temperature curing process, which does not require organic solvents and high-temperature sintering. The process route is simple and suitable for large-scale mass production. The independent sealed packaging ensures that the functional components of the product are stable under room temperature storage conditions, and the product can be activated and used immediately after opening the bag. Attached Figure Description

[0024] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 is a partial cross-sectional structural diagram of the micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase provided in an embodiment of the present invention; Figure 2 is a magnified schematic diagram of the microstructure of the functional negative ion coating in Figure 1; Figure 3 is a flowchart of the preparation process of the micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase provided in the embodiment of the present invention; Figure 4 is a schematic diagram of the principle of hydroxyl negative ion release and antibacterial and deodorizing effects provided in the embodiment of the present invention; Figure 5 is a schematic diagram of the weekly disposable antibacterial pillowcase with micro-nano mineral hydroxyl negative ion provided in the embodiment of the present invention.

[0025] Labeling instructions: 1 - Pillowcase base fabric, 2 - Functional negative ion coating, 21 - Water-based flexible film-forming layer, 22 - Micro-nano activated hydroxyl negative ion composite powder particles, 23 - Nano dispersant, 3 - Water molecules, 4 - Release direction, 5 - Bacteria, 6 - Odor organic molecules, 7 - Human head, 8 - Individually sealed packaging bag, 9 - Antibacterial pillowcase, 10 - Disposable recycling container. Detailed Implementation

[0026] Embodiments of the present invention are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0027] It should be understood that the following embodiments are for illustrative purposes only and are not intended to limit the scope of protection.

[0028] As shown in Figure 1, the micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase provided by the present invention includes a pillowcase base fabric 1 and a functional negative ion coating 2 loaded on the surface of the pillowcase base fabric 1. The pillowcase base fabric 1 serves as a supporting structure, providing an adhesion substrate for the functional negative ion coating 2; the functional negative ion coating 2 uniformly covers the front side of the pillowcase base fabric 1 that comes into contact with the human body, and is the core structural layer for achieving antibacterial, mite-inhibiting, and odor-decomposing functions.

[0029] As shown in Figure 2, the functional negative ion coating 2 comprises, at the microscale, an aqueous flexible film-forming layer 21, micro / nano activated hydroxyl negative ion composite powder particles 22 dispersed in the aqueous flexible film-forming layer 21, and a nano dispersant 23. The aqueous flexible film-forming layer 21 is a continuous organic polymer film that encapsulates and anchors the micro / nano activated hydroxyl negative ion composite powder particles 22 onto the fiber surface of the pillowcase base fabric 1. The nano dispersant 23 adheres to the surface of the powder particles, preventing the particles from agglomerating. Part of the surface of the micro / nano activated hydroxyl negative ion composite powder particles 22 is exposed to the outside of the coating, allowing them to contact water molecules 3 in the air. Through the surface micro-electric field effect, the water molecules 3 are ionized, and the generated hydroxyl negative ions diffuse into the space above the pillow surface along the release direction 4.

[0030] In this invention, the pillowcase base fabric 1 is made of ultrafine fiber spunlace nonwoven fabric with a weight of 80 to 120 grams per square meter. The spunlace nonwoven fabric is made by using a high-pressure water jet piercing process to entangle the ultrafine fibers together. The fibers are fine, the fabric surface is uniform and flat, and the feel is soft and skin-friendly. It does not contain chemical adhesives. The base fabric in this weight range has suitable stiffness and drape, and it is not easy to slip when laid on the pillow. At the same time, the pores between the fibers are fine enough to prevent nano-sized powder particles from leaking out of the pores of the fabric, so as to achieve breathability without powder penetration.

[0031] In this invention, the micro-nano activated hydroxyl anion composite powder is made from natural mineral raw materials and then subjected to low-temperature calcination activation treatment within the temperature range of 350 to 420 degrees Celsius. Low-temperature calcination causes solid-phase reactions between mineral components, forming lattice defects and surface energy levels with catalytic ionization activity on the powder surface. The calcination temperature is controlled within the above range to ensure the activation effect while avoiding excessive temperature that would cause the mineral lattice to become dense and lose its activity. The calcined mineral clinker is then subjected to wet ball milling and air classification using a high-speed ball mill to control the powder particle size to 200 to 500 nanometers. Powders in this particle size range have a large specific surface area, high density of surface active sites, and a large contact area with air and water molecules, which is conducive to the continuous ionization and generation of hydroxyl anions. At the same time, powders in this particle size range are not prone to hard agglomeration in aqueous dispersion systems, making it easy to prepare a uniform and stable finishing liquid.

[0032] In this invention, the water-based flexible film-forming aid is selected from water-based polyurethane or water-based acrylate flexible film-forming substances. This type of film-forming aid can form a continuous, transparent, and flexible film on the fiber surface under low-temperature drying conditions. The film has a low glass transition temperature and is in a highly elastic state at room temperature, so it will not make the pillowcase feel stiff. The film has a high air permeability and will not block the contact between air water molecules and powder particles, ensuring the continuous release of hydroxyl negative ions.

[0033] In this invention, the nano-dispersant is a polyacrylate or polycarboxylate polymeric dispersant. One end of its molecular chain is anchored to the surface of the powder particles, while the other end extends into the aqueous phase to form steric hindrance. At the same time, it imparts the same charge to the particle surface, generating electrostatic repulsion. This dual effect effectively prevents the nanoparticles from agglomerating and settling in the liquid phase. The wetting and penetrating agent is a nonionic surfactant, such as fatty alcohol polyoxyethylene ether, used to reduce the surface tension of the finishing liquid, allowing the finishing liquid to spread rapidly on the surface of the nonwoven fabric fibers and penetrate into the fiber gaps, improving the uniformity and binding strength of the functional components on the fibers. The plant-based antibacterial stabilizer is a natural plant-derived antibacterial ingredient, such as tea tree oil, artemisia argyi extract, or chitosan. These ingredients have a certain inhibitory effect on Gram-positive bacteria, Gram-negative bacteria, and fungi, and are gentle and non-irritating to the skin. At the same time, the plant-based antibacterial stabilizer can adjust the ionic strength and pH of the finishing liquid, reduce the dissolution of trace metal ions in the mineral powder, and stabilize the negative ion release efficiency.

[0034] The present invention will be further described in detail below through Examples 1 to 5 and Comparative Examples 1 to 3. Examples 1 to 5 and Comparative Examples 1 to 2 all adopted the same preparation process route, differing only in the raw material ratio and process parameters; Comparative Example 3 was a commercially available silver ion antibacterial pillowcase control sample. The raw material ratios of each example and comparative example are shown in Table 1, and the preparation process parameters are shown in Table 2.

[0035] Table 1. Raw material ratios (parts by weight) for each embodiment and comparative example.

[0036] Table 2. Preparation process parameters for each embodiment and comparative example;

[0037] Example 1; Example 1 is the preferred embodiment of the present invention. As shown in Figure 3, the antibacterial pillowcase of this embodiment is prepared according to the following steps: Step S1: Prepare the base solution. Add 82.55 parts of deionized water to a mixing tank at room temperature. While stirring at low speed, add 0.4 parts of nano-dispersant, 0.25 parts of wetting and penetrating agent, and 1.8 parts of plant antibacterial stabilizer in sequence. Continue stirring at low speed for 8 minutes to ensure that the three additives are fully dissolved and evenly dispersed in the water, resulting in a clear and transparent base solution. The stirring speed should be such that a gentle vortex forms on the liquid surface without entraining a large number of air bubbles. The purpose of preparing the base solution first is to allow the dispersant and wetting agent to fully dissolve and spread in the water, providing a good dispersion environment for the subsequent addition of powder.

[0038] Step S2, homogenization and dispersion of powder. While maintaining stirring, 5.0 parts of micro-nano activated hydroxyl anion composite powder are slowly and uniformly added to the base solution to avoid the powder from being concentrated and forming clumps. After the powder is added, high-speed shear homogenization is switched and continued for 25 minutes. The strong turbulence and shear force generated by high-speed shearing can break up the soft agglomerates between powder particles, so that the nanoparticles are uniformly suspended in the liquid phase as single particles, forming a uniform and stable powder dispersion. During the shear homogenization process, the dispersion gradually changes from the initial flocculent suspension to a fine and uniform emulsion.

[0039] Step S3, Film-forming system compounding. The temperature of the powder dispersion slurry is lowered to 40 degrees Celsius. While stirring at low speed, 10.0 parts of an aqueous flexible film-forming aid are slowly added. Stirring at low speed continues for 12 minutes to ensure the film-forming aid is fully and evenly mixed with the powder dispersion slurry, resulting in a functional negative ion finishing liquid. Adding the film-forming aid after cooling is to prevent premature film formation or bubble generation in the mixing tank due to excessively high temperature. Low-speed stirring is to prevent excessive air bubbles from being drawn in during high-speed stirring, which would affect the uniformity of the subsequent pad-coating.

[0040] Step S4, fabric padding finishing. A roll of microfiber spunlace nonwoven fabric with a weight of 100 g / m² is guided through a padding tank containing a functional negative ion finishing solution at a constant speed, so that the front side of the base fabric is in contact with the finishing solution. The liquid content is controlled to be 50% by the squeezing of the rollers. Single-sided padding is achieved by adjusting the liquid level in the padding tank and the position of the guide rollers, so that the finishing solution only penetrates to a certain depth from the front side of the base fabric without penetrating to the back side.

[0041] Step S5, low-temperature curing and molding. The impregnated base fabric enters the hot air drying chamber and is dried and cured at a low temperature of 60 degrees Celsius. Low-temperature drying allows the moisture to evaporate slowly, and the water-based flexible film-forming agent forms a continuous and uniform flexible film on the fiber surface, firmly anchoring the powder particles. After drying, the base fabric is naturally cooled to room temperature, cut according to the pillowcase specifications, folded, and individually sterile sealed to obtain the finished micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase.

[0042] In this embodiment, the calcination activation temperature of the micro-nano activated hydroxyl negative ion composite powder is 380 degrees Celsius, and the particle size of the powder after ball milling is 200 to 500 nanometers; the water-based flexible film-forming aid is a water-based polyurethane film-forming substance; the nano dispersant is a polyacrylate dispersant; the wetting and penetrating agent is a fatty alcohol polyoxyethylene ether; the plant antibacterial stabilizer is a compound of tea tree oil and chitosan; the thickness of the obtained functional negative ion coating is 0.02 mm.

[0043] Example 2; The difference between Example 2 and Example 1 is as follows: the amount of micro / nano activated hydroxyl anion composite powder is 3.5 parts (the lower limit of the scope defined in the claims), the amount of nano dispersant is 0.3 parts, the amount of wetting and penetrating agent is 0.20 parts, the amount of plant antibacterial stabilizer is 1.5 parts, and the amount of deionized water is 84.50 parts; the pillowcase base fabric is made of ultrafine fiber spunlace nonwoven fabric with a basis weight of 80 g / m²; in the preparation process, the low-speed stirring time in step S1 is 5 minutes, the high-speed shearing homogenization time in step S2 is 20 minutes, the film-forming aid is added after cooling to 35 degrees Celsius in step S3 and low-speed stirring is carried out for 10 minutes, the liquid carryover rate is controlled at 45% in step S4, and the drying temperature in step S5 is 55 degrees Celsius; the calcination activation temperature of the micro / nano activated hydroxyl anion composite powder is 350 degrees Celsius. The temperature was set at 100 degrees Celsius; the water-based flexible film-forming agent was selected from water-based acrylic film-forming substances; the plant antibacterial stabilizer was selected from Artemisia argyi extract; and the thickness of the resulting functional negative ion coating was 0.01 mm.

[0044] Example 3; The difference between Example 3 and Example 1 is as follows: the amount of micro / nano activated hydroxyl negative ion composite powder is 6.5 parts (the upper limit of the scope defined in the claims), the amount of nano dispersant is 0.5 parts, the amount of wetting and penetrating agent is 0.30 parts, the amount of plant antibacterial stabilizer is 2.0 parts, and the amount of deionized water is 80.70 parts; the pillowcase base fabric is a superfine fiber spunlace nonwoven fabric with a basis weight of 120 g / m²; in the preparation process, the low-speed stirring time in step S1 is 10 minutes, the high-speed shearing homogenization time in step S2 is 30 minutes, the low-speed stirring time in step S3 is 15 minutes, the liquid content in step S4 is controlled at 55%, and the drying temperature in step S5 is 65 degrees Celsius; the calcination activation temperature of the micro / nano activated hydroxyl negative ion composite powder is 420 degrees Celsius; the plant antibacterial stabilizer is chitosan; and the thickness of the obtained functional negative ion coating is 0.03 mm.

[0045] Example 4; The difference between Example 4 and Example 1 is that the amount of water-based flexible film-forming aid is 8.0 parts (the lower limit of the scope defined by the claims), and the amount of deionized water is 84.55 parts; the amounts of other raw materials, the basis weight, and the preparation process parameters are the same as in Example 1; the thickness of the obtained functional negative ion coating is 0.015 mm.

[0046] Example 5; The difference between Example 5 and Example 1 is that the amount of water-based flexible film-forming aid is 12.0 parts (the upper limit of the scope defined by the claims), and the amount of deionized water is 80.55 parts; the amount of other raw materials, the basis weight, and the preparation process parameters are the same as in Example 1; the thickness of the obtained functional negative ion coating is 0.025 mm.

[0047] Comparative Example 1; The difference between Comparative Example 1 and Example 1 is that no micro / nano activated hydroxyl anion composite powder was added (i.e., the amount of composite powder was 0), and the amount of deionized water was adjusted accordingly to 87.55 parts; the remaining raw material amounts, base fabric weight, and preparation process parameters were the same as in Example 1. This comparative example was used to examine the basic properties of the pillowcase without functional powder.

[0048] Comparative Example 2; The difference between Comparative Example 2 and Example 1 is as follows: the amount of micro / nano activated hydroxyl anion composite powder is 8.0 parts (exceeding the upper limit of the scope defined in the claims), the amount of nano dispersant is 0.6 parts, the amount of wetting and penetrating agent is 0.40 parts, the amount of plant antibacterial stabilizer is 2.5 parts, and the amount of deionized water is 78.50 parts; in the preparation process, the low-speed stirring time in step S1 is 10 minutes, the high-speed shearing homogenization time in step S2 is 30 minutes, the low-speed stirring time in step S3 is 15 minutes, the liquid carryover rate in step S4 is controlled at 55%, and the drying temperature in step S5 is 65 degrees Celsius. This comparative example is used to investigate the effect of excessive powder on the coating performance.

[0049] Comparative Example 3; Comparative Example 3 is a commercially available silver ion antibacterial pillowcase as a control sample. This pillowcase uses a cotton base fabric and is treated with a silver ion antibacterial finishing agent. It is labeled as having antibacterial function and is a long-term reusable product that requires regular washing during use. This comparative example is used to compare its performance with the weekly disposable hydroxyl negative ion antibacterial pillowcase of the present invention.

[0050] Performance testing and comparison; The pillowcase samples obtained from Examples 1 to 5 and Comparative Examples 1 to 3 were tested for antibacterial performance according to GB / T21866-2008 "Determination of Antibacterial Properties and Antibacterial Effects of Antibacterial Coatings (Films)". The tested bacteria included Escherichia coli, Staphylococcus aureus, and Candida albicans. A dust mite repellency test was conducted according to the method in Appendix of GB / T 21866-2008. The release concentration of hydroxyl negative ions and the removal rate of odor gases were tested according to JC / T 1074-2008 "Purification Performance of Indoor Air Purification Functional Coating Materials". Simultaneously, the physical properties of the coating, such as coating thickness, powder shedding, feel, and breathability, were evaluated. The results of the antibacterial and anti-mite performance tests are shown in Table 3, the results of the hydroxyl negative ion release concentration tests are shown in Table 4, the results of the odor decomposition performance tests are shown in Table 5, and the results of the coating physical performance evaluation are shown in Table 6.

[0051] Table 3 Comparison of antibacterial and anti-mite properties;

[0052] Table 4 Comparison of hydroxyl anion release concentrations (ions / cm³) 3 );

[0053] Table 5 Comparison of odor gas removal rates (after 24 hours of action, %)

[0054] Table 6. Comparison of physical properties of coatings;

[0055] The test results in Tables 3 to 6 show that: Example 1 uses the optimal formulation, which shows a balanced performance in antibacterial and anti-mite properties, negative ion release, odor decomposition, and coating physical properties. It achieves a high level of antibacterial rate against Escherichia coli and Staphylococcus aureus, and also has a good inhibitory effect on Candida albicans and dust mites. The hydroxyl negative ion retention rate is high after 7 days. The coating does not shed powder, has a soft and skin-friendly feel, and its appearance does not change within a 7-day use period. It has the best overall performance.

[0056] In Example 2, the amount of composite powder used is at the lower limit of the range, and the antibacterial rate and negative ion concentration are reduced accordingly, but still remain at an effective level. The coating is thinner and softer with excellent breathability, making it suitable for application scenarios that require a light and thin feel.

[0057] In Example 3, the amount of composite powder used was at the upper limit of the range, resulting in the highest antibacterial rate and negative ion concentration. However, the coating was slightly thicker, the feel was stiffer, and there was a slight powdery feel, indicating that the dispersion and anchoring difficulty increased when the amount of powder was close to the upper limit.

[0058] In Example 4, the amount of film-forming aid was at the lower limit of the range, and the antibacterial and odor decomposition performance was good. However, due to the thin film, slight powdering occurred after friction, and the coating durability decreased.

[0059] In Example 5, the amount of film-forming aid used was at the upper limit of the range. The coating was firmly anchored and there was no powder shedding. The negative ion retention rate was the highest after 7 days. However, due to the relatively thick coating, the feel was slightly stiff and the breathability was average.

[0060] Comparative Example 1: No functional powder was added. All antibacterial and purification indicators were at extremely low levels. Only the plant antibacterial stabilizer provided a weak antibacterial effect, proving that the micro-nano activated hydroxyl negative ion composite powder is a necessary component to realize the core function of this invention.

[0061] In Comparative Example 2, the amount of powder used exceeded the upper limit. Although the initial antibacterial rate and negative ion concentration were the highest, the poor powder dispersion led to obvious powder shedding, a hard and rough feel, and obvious powder marks and yellowing of the coating after 7 days of use. The negative ion retention rate decreased significantly after 7 days, indicating that excessive powder actually damaged the overall performance and durability of the coating.

[0062] Comparative Example 3: The commercially available silver ion pillowcases showed some initial antibacterial effect against Escherichia coli and Staphylococcus aureus, but had a weak inhibitory effect on Candida albicans and dust mites, and did not have the ability to release negative ions or decompose odors. After several washes, the silver ions were lost, the antibacterial effect was significantly reduced, and the surface of the pillowcase turned yellow and black, failing to maintain stable efficacy throughout the entire use cycle.

[0063] The above comparison results show that the raw material ratio range and process parameter range defined by the present invention are the key to achieving a comprehensive balance of antibacterial and anti-mite properties, odor decomposition, coating durability, and skin-friendly feel; if the amount of powder is too low, the effect will be insufficient, and if the amount is too high, the powder will fall off and the coating will become hard; if the amount of film-forming aid is too low, the anchoring will be weak, and if the amount is too high, the coating will become hard and the breathability will decrease; the ratio in Example 1 achieves the optimal balance among various properties.

[0064] As shown in Figure 4, when the antibacterial pillowcase of the present invention is used, the antibacterial pillowcase 9 laid on the surface of the pillow comes into contact with the human head 7; the micro-nano activated hydroxyl negative ion composite powder particles 22 in the functional negative ion coating 2 continuously come into contact with water molecules 3 in the air. Under the action of the micro electric field on the powder surface, the water molecules are ionized, and the generated hydroxyl negative ions diffuse upwards along the release direction 4; when the hydroxyl negative ions come into contact with bacteria 5 on the pillow surface, their strong oxidizing properties can destroy the cell membrane structure of the bacteria, causing the contents of the bacteria to leak out and die; when they come into contact with odorous organic molecules 6, the hydroxyl negative ions can break the chemical bonds in the organic molecules, oxidizing and degrading them into odorless small molecule compounds; for dust mites, the hydroxyl negative ions can oxidize the proteins on the surface of the mite and the respiratory system, thus inhibiting their survival environment; the effective ingredients in the plant antibacterial stabilizer continuously inhibit the germination and growth of mold spores, forming a synergistic effect with the hydroxyl negative ions; the above process is spontaneously and continuously carried out under normal temperature, no light, and normal pressure conditions, without the need for light excitation or external power supply.

[0065] As shown in Figure 5, the antibacterial pillowcase of this invention adopts a weekly disposable usage mode. The product is packaged in an individually sealed bag 8 at the factory. The sealed packaging isolates it from external pollution and moisture, ensuring the stability of the functional components during storage. When using, open the bag 8, take out the antibacterial pillowcase 9, and place it on the pillow. Opening the bag activates the contact between the powder and water molecules in the air, releasing hydroxyl negative ions. During the 7-day usage period, the pillowcase continues to exert its antibacterial, anti-mite, and deodorizing effects. After the 7-day period, remove the pillowcase and place it in the disposal and recycling container 10, replacing it with a new individually packaged pillowcase. The entire usage process requires no washing, avoiding damage to the functional coating from washing and the labor costs associated with the washing process.

[0066] In other embodiments, the calcination activation temperature of the micro-nano activated hydroxyl negative ion composite powder can be adjusted within the range of 350 to 420 degrees Celsius according to the specific mineral composition. The particle size of the ball-milled powder, ranging from 200 to 500 nanometers, can achieve the function of releasing hydroxyl negative ions at room temperature without light. The basis weight of the pillowcase base fabric, ranging from 80 to 120 grams per square meter, can be selected according to hand feel preference and cost requirements. A lower basis weight results in a lighter and softer pillowcase, while a higher basis weight results in a thicker and firmer pillowcase. The thickness of the functional negative ion coating ranges from 0.01 to 0.03 mm. The powder loading and air permeability can be guaranteed within millimeters; the process parameters such as stirring time, shearing time, and drying temperature during the preparation process can be appropriately adjusted according to equipment conditions and production speed within the range defined in the claims; the plant antibacterial stabilizer can be one or more combinations of natural plant-derived antibacterial components such as tea tree oil, artemisia argyi extract, and chitosan; the water-based flexible film-forming aid can be one or a combination of two water-based polyurethane or water-based acrylate film-forming substances; all the above alternative embodiments can achieve the purpose of the present invention.

[0067] The micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase of this invention is suitable for daily sleep use at home, as well as for disposable hygiene in public accommodation places such as hotels, homestays, and hospitals. It is also suitable for travel and is suitable for mothers and infants as well as people with sensitive skin.

[0068] Although embodiments of the invention have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the claims and their equivalents.

Claims

1. A micro / nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase, characterized in that, Includes a pillowcase base fabric and a functional negative ion coating loaded on the surface of the pillowcase base fabric; The functional negative ion coating is prepared from the following raw materials in parts by weight: 3.5-6.5 parts of micro-nano activated hydroxyl negative ion composite powder, 8.0-12.0 parts of water-based flexible film-forming aid, 0.2-0.6 parts of nano dispersant, 0.1-0.4 parts of wetting and penetrating agent, 1.0-2.5 parts of plant antibacterial stabilizer, and deionized water to make up to 100 parts; The micro-nano activated hydroxyl negative ion composite powder is a natural mineral composite powder modified by low-temperature calcination and ball milling. The particle size of the micro-nano activated hydroxyl negative ion composite powder is 200-500 nm. The micro-nano activated hydroxyl negative ion composite powder can adsorb water molecules in the air and ionize to generate hydroxyl negative ions under normal temperature and light-free conditions. The pillowcase base fabric and the functional negative ion coating constitute a disposable weekly pillowcase, and the rated safe use period of the disposable weekly pillowcase is 7 days.

2. The micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 1, characterized in that, The raw material weight ratio of the functional negative ion coating is as follows: 5.0 parts of micro-nano activated hydroxyl negative ion composite powder, 10.0 parts of water-based flexible film-forming aid, 0.4 parts of nano dispersant, 0.25 parts of wetting and penetrating agent, 1.8 parts of plant antibacterial stabilizer, and 82.55 parts of deionized water.

3. The micro / nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 1, characterized in that, The pillowcase base fabric is a microfiber spunlace nonwoven fabric with a weight of 80-120 g / m².

4. The micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 1, characterized in that, The micro-nano activated hydroxyl anion composite powder is subjected to low-temperature activation modification at 350-420℃ and high-speed ball milling classification. The micro-nano activated hydroxyl anion composite powder can activate hydroxyl anions under ambient temperature conditions of -10℃ to 65℃, and does not rely on ultraviolet light or require electricity.

5. The micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 1, characterized in that, The functional negative ion coating is prepared by single-sided dip-coating and low-temperature air-drying molding process, and the thickness of the functional negative ion coating is 0.01-0.03 mm.

6. A method for preparing a micro / nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Preparation of base solution: Under normal temperature conditions, add nano-dispersant, wetting and penetrating agent and plant antibacterial stabilizer into deionized water and stir at low speed for 5-10 minutes to obtain base solution; S2. Homogeneous dispersion of powder: Micro-nano activated hydroxyl anion composite powder is added to the substrate solution and homogenized by high-speed shearing for 20-30 minutes to make the powder uniformly dispersed. S3. Film-forming system compounding: Cool the solution treated in step S2 to 35-40℃, add water-based flexible film-forming aid, stir at low speed for 10-15 minutes to obtain functional negative ion finishing solution; S4. Fabric padding treatment: The pillowcase base fabric is immersed in the functional negative ion finishing solution for single-sided padding treatment, and the liquid retention rate is controlled at 45% to 55%. S5. Low-temperature curing and molding: The pillowcase base fabric treated in step S4 is dried and cured with low-temperature hot air at 55-65℃. After natural cooling, it is cut, folded and individually aseptically sealed and packaged to obtain micro-nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase.

7. The preparation method of the micro / nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 6, characterized in that, In step S1, the low-speed stirring time is 8 minutes.

8. The preparation method of the micro / nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 6, characterized in that, In step S2, the high-speed shearing homogenization time is 25 min; in step S3, after cooling to 40℃, the water-based flexible film-forming aid is added, and the low-speed stirring time is 12 min.

9. The preparation method of the micro / nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 6, characterized in that, In step S4, the liquid content is 50%; in step S5, the temperature for low-temperature hot air drying and curing is 60°C.

10. A method for applying the micro / nano mineral hydroxyl negative ion weekly disposable antibacterial pillowcase according to claim 1, characterized in that, After opening the individually sterile sealed antibacterial pillowcase, place it on the pillow. During the 7-day usage period, the functional negative ion coating continuously releases hydroxyl negative ions to inhibit bacteria, mold, and mites on the pillow surface and decompose odors from head sweat and oxidized oils. After the usage period, discard and replace the antibacterial pillowcase; no washing is required.